The present invention relates to the rolled electrochemical components such as cells, double-layered capacitors and like, more specifically, to the improvement of the end section of the collector which is connected to the collecting plate.
The rolled electrochemical components are widely used in batteries, double-charge-layered capacitors and like. Generally, this component has a set of electrode plates which is revolved into a roll and provided with a stripe-shaped separator disposed between a positive electrode plate which is coated with active material on its stripe-shaped collector and a negative electrode plate which is coated with active material on its stripe-shaped collector. The set of electrode plates together with electrolyte is accommodated in a metal casing and protrudes from the collector of the electrode plate of the positive or negative electrode on both upper and lower end faces or one end face of said set of electrode plates. A collecting plate is typically welded on the top end of the collector.
In the past, a structure was presented, in which a collecting section had a thin metal plate welded and in which the thickness is increased. On an end section of the collector, splits (in the description, “split” means that a collector is only cut resulting in a split which has essentially no width or separation; the “notch” means that a collector is partly cut off and a notch is formed which has a broad width) are formed on the collecting section, and a collecting plate is welded on the collecting section with the notches. Therefore, compared with the cell in which the collector is directly welded to the collecting plate without the thin metal plate welded on its end section, the collecting section will not be damaged and not be bent to such an extent that the separator would be punched or pricked through (i.e., having a hole formed therein) even though the collecting section is strongly pressed through the collecting plate, so that the possibility of an inner short-circuit can be reduced, and the electrical connection between the collecting section and the collecting plate can be stabilized (see, Japanese Patent Published No. 2000-77054).
For the foregoing collection structure of the prior art, however, a thin metal plate is welded on an end section of a collector to form a collecting section with splits formed in an equally-spaced manner, so that there is a problem that the collecting section positioned in the innermost periphery of the set of electrode plate with the smallest radius of curvature which are revolved into a roll can not have a smooth arc-shape but a sharp crimping or crippling, so that the separator may be punched through, thereby the inner short-circuit may occur.
The present invention is directed to solve the foregoing technical problem in prior art. The object of the invention is to provide a set of electrode plates for rolled electrochemical components and cells comprising such components, in which there is reliable and stable electrical connection between the collecting section and the collecting plate in the cell and the inner short-circuit may be avoided in the set.
Hence, with the rolled electrochemical component of the present invention, a high quality component having reliable and stable electrical connection between the collecting section and the collecting plate thereof is provided, which prevents an inner short-circuit in the set of roll-shaped electrode plates.
The object of the invention is to provide a set of electrode plates for rolled electrochemical component and a cell comprising such components, in which there is reliable and stable electrical connection between the collecting section and the collecting plate in the cell so that an inner short-circuit may be avoided in the set of electrode plates.
In order to realize above object, a set of electrode plates for rolled electrochemical component of the invention, comprises a stripe-shaped first electrode plate, a stripe-shaped second electrode plate and a stripe-shaped separator, said separator being positioned between the first electrode plate and the second electrode plate, and these three being revolved into a roll in the length direction, wherein said first electrode plate comprises a stripe-shaped first collector and the active material coated on the surface of said first collector and said second electrode plate comprises a stripe-shaped second collector and the active material coated on the surface of said second collector, a first exposed portion with a predetermined width on which the active material is not coated being formed on at least one of two terminals in a width direction of the first electrode plate to constitute a first collecting section, a second exposed portion with a predetermined width on which the active material is not coated being formed on at least one of two terminals in a width direction of the second electrode plate to constitute a second collecting section, characterized in that a structure for preventing sharp crimping is formed on at least one of said first collecting section and said second collecting section in at least the innermost periphery of the set of electrode plates.
According to the invention, because the structure for preventing sharp crimping is formed on at least one of said first collecting section and said second collecting section in at least the innermost periphery of the set of electrode plates, the resistance on the initial revolved section is small when revolving is started, the revolving can be executed easily around a revolving core rod and the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
In the inventive set or cell, said structure for preventing sharp crimping is formed by cutting off the collecting section which are positioned in at least the innermost periphery.
According to this structure, there is no collecting section on at least the innermost periphery of the set of electrode plates, and hence the involving-resistance from the collecting section cut off and the sharp crimping formed in the collecting section does not appear, resulting in the revolving being easy and the inner-short-circuit being prevented.
In the inventive set or cell, at least 4 splits starting from a side edge of the collecting section in its width direction are formed on the collecting section which is positioned at least in the innermost periphery.
According to this structure, when being revolved, the sharp crimping does not occur on the innermost periphery, so the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
In the inventive set or cell, said structure for preventing sharp crimping is formed by forming at least one notch and at least one strip-shaped collecting section at least in the innermost periphery.
According to this structure, when being revolved, the sharp crimping does not occur on the innermost periphery, so the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
In the inventive set or cell, said structure for preventing sharp crimping is formed by forming at least one notch or at least four splits in at least one of the layers constituting the collecting section at least in the innermost periphery.
According to this structure, when being revolved, the sharp crimping does not occur on the innermost periphery, so the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
A cell of the present invention, comprises: a set of electrode plates, said set of electrode plates comprising a stripe-shaped positive electrode plate, a stripe-shaped negative electrode plate and a stripe-shaped separator, said separator being positioned between the positive electrode plate and the negative electrode plate, and these three being revolved into a roll in the length direction, wherein said positive electrode plate comprises a stripe-shaped positive collector and the active material coated on the surface of said positive collector and said negative electrode plate comprises a stripe-shaped negative collector and the active material coated on the surface of negative second collector, two exposed portions with a predetermined width on which the active material is not coated being formed on at least one of two terminals in a width direction respectively of the positive and negative electrode plates to respectively constitute a positive collecting section and a negative collecting section; a negative collecting plate connected electrically to said negative collecting section; and a positive collecting plate connected electrically to said positive collecting section; characterized in that a structure for preventing sharp crimping is formed on at least one of the positive collecting section and the negative collecting section in at least the innermost periphery of the set of electrode plates.
According to the invention, because the structure for preventing sharp crimping is formed on at least one of said first collecting section and said second collecting section in at least the innermost periphery of the set of electrode plates, the resistance on the initial revolved section is small when revolving is started, the revolving can be executed easily around a revolving core rod and the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
As an embodiment of the invention,
In
Positive electrode plate 1 and negative electrode plate 2 have the structure as described specifically below. Positive electrode plate 1 is formed by coating both sides of collector 1a made of aluminum foil with positive active-substance 1b, while one end section of positive collector 1a (upper section in
Both end sections of separator 3 protrude upward and downward beyond both end edges of the sections of positive electrode plate 1 or negative electrode plate 2 which is coated with the active material.
Moreover, positive collecting plate 10 is welded to positive collector 1a, negative collecting plate 11 is welded to negative collector 2a, and positive collecting plate 10 and negative collecting plate 11 are welded to the inner surface of cell cap 7 and the inner bottom of cell housing 6 respectively. Connecting piece 10a is provided on positive collecting plate 10 as a wiring piece for connecting collecting plate 10 to the inner surface of cell cap 7. Connecting piece 11a is provided in the center section of collecting plate for connecting negative collecting plate 11 to the inner bottom of cell housing 6.
The liquid electrolyte is the solution which is formed, for example, by dissolving LiPF6 as solute in concentration of 1 mol/dm3 in the mixed solvent of ethylene carbonate (EC) and (DEC) diethyl carbonate in volume ratio of 1:1.
An exemplary method for manufacturing the electrode plates is now described more specifically below. For positive electrode plate 10, the procedure is: mixing electrolyzed MnO2 and Li2CO3 in mixing ratio 1:2, calcining the mixture under temperature of 800□ in the air for 20 hours to produce LiMn2O4, mixing LiMn2O4, acetylene black as a conductor and polyfluorovinylidene as adhesive in weight ratio 92:3:5 to be a mixture as positive active material 1b, above mixing ratio referring to the ratio between the solid compositions, moreover, dissolving polyfluorovinylidene as adhesive in dissolvent of NMP to make positive active-substance 1b be in a pasty state, coating both sides of positive collector 1a with 15 μm thickness made of aluminum foil with the paste of positive active-substance 1b to form layers of positive active-substance 1b in the manner that a lateral edge section with approximately 5 mm width remains without being coated, the layer-thickness on both sides being substantially the same and whole thickness of two layers being approximately 280 μm after coating and drying, and then pressing and shaping the resulting positive electrode plate 1 to make it have thickness of approximately 200 μm.
For negative electrode plate 2, mixing artificial graphite and sutylen butadiene rubber (SBR) as a binder in weight ratio 97:3 to be a mixture as negative active-substance 2b, above mixing ratio referring to the ratio between the solid-state compositions, moreover, dissolving SBR as adhesive in dissolvent of water-solvable resolvent to make negative active-substance 2b be in a pasty state, coating both sides of negative collector 2a with 14 μm thickness made of copper foil with the paste of negative active-substance 2b to form layers of negative active material 2b in the manner that a lateral edge section with 5 mm width remains without being coated, and then pressing and shaping resulting negative electrode plate 2 to make it have thickness of 170 μm.
When manufacturing a Lithium ion secondary battery, positive electrode plate 1 and negative electrode plate 2 obtained as described above are placed opposite to each other with separator 3 being sandwiched therebetween and revolved into a roll to form set 4 of electrode plates in the state that positive collecting section 9 and negative collecting section 15 protrude. The lengths of the sections both positive collecting section 9 and negative collecting section 15 protruding respectively from the end section of separator 3 to both sides are approximately 0.5 mm.
Then positive collecting plate 10 is placed on the positive side of set 4 of electrode plates, making it pressed against positive collecting section 9. Positive collecting plate 10 is ultrasonic-welded with positive collecting section 9 in the state that they are pressed against each other. Then connecting piece 10a having approximately 5 mm in width, 0.15 mm in thickness and 70 mm in length is ultrasonic-welded onto positive collecting plate 10. Moreover, negative collecting plate 11 is provided on the negative side of set 4 of electrode plates, making it pressed against collecting section 15 of positive electrode. Negative collecting plate 11 is resistance-welded with negative collecting section 15 in the state that they are pressed against each other.
Set 4 of electrode plates incorporated with positive collecting plate 10 and negative collecting plate 11 is accommodated in cell housing 6, collecting plate 11 being resistance-welded with the bottom of cell housing 6. Moreover, connecting piece 10a is pressed against cell cap 7 and laser-welded in the state of contacting, then the liquid electrolyte is poured into cell housing 6 with set 4 of electrode plates being therein to soak in vacuum, and cell housing 6 is sealed with cell cap 7.
Positive electrode plate 1 and negative electrode plate 2 will be described in detail below. Two electrode plates can have a same structure, but can have different structures as well. For easy understanding, the thickness of the electrode plate is showed in magnifying manner.
First, as shown in
Then the exposed portion of the collector having a predetermined width protruding from boundary 12 is flexed along a straight line 13 parallel to the boundary, as shown in
In addition,
In the description, “innermost periphery” means the periphery of a circle positioned at the innermost portion of the winded set of electrode plates, and “collecting section” means a general term for first collecting section, second collecting section or both, or positive collecting section, negative collecting section or both, except a special designation.
Positive electrode plate 1 is formed to have the size of approximately 55 mm in width and 570 mm in length. Collector 1a of positive electrode plate 1 is folded once in above-mentioned method to form positive collecting section 9 of approximately 2.5 mm in width.
When cutting off the part of collecting section 9 which is in the innermost periphery of set 4 of electrode plates, the cutting process begins at the end edge of positive collecting section 9 which is positioned in the innermost periphery, continues along boundary 12 between the section which is coated with positive active-substance 1b and the positive collector 1a, and ends at the point approximately 100 mm away from the end edge, the section therebetween of positive collecting section 9 being cut off.
Stripe-shaped negative electrode plate 2 can be formed in the same manner as stripe-shaped positive electrode plate 1.
Negative electrode plate 2 is formed to have the size of approximately 61 mm in width and 600 mm in length. Collector 2a of negative electrode plate 2 is folded once in the method shown in
The process of cutting off the part of negative collecting section 15 which is positioned in the innermost periphery of set 4 of electrode plates is the same as positive electrode plate 1.
For the Lithium ion secondary battery formed from the electrode plates of the embodiment, because the collecting section is formed by folding once on the end section of the collector, the collecting section will not be damaged and will not be bent to such an extent that the separator would be punched through even though the collecting plate is pressed when being welded, so that the inner short-circuit can be reduced. Moreover, because the collecting section is not flexed greatly, the connection between the collecting sections and the collecting plates are reliable and stable.
Moreover, because the collecting section is not provided for the innermost periphery of the set of electrode plates with small radius of curvature when it is revolved into a roll, the resistance on the initial revolved section is small when revolving is started, so that this section can be revolved into a roll around a revolving core rod quickly, thereby the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
In this embodiment, a plurality of splits 14 from an end edge of positive collecting section 9 towards a direction parallel to a shorter side (wideness) of stripe-shaped positive electrode plate 1 are formed on positive collecting section 9 of positive electrode plate 1, and disposed in the manner that a periphery portion of a circle on inner periphery of the revolved set of electrode plates comprises at least 4 splits and the spaces of splits 14 positioned in the inner periphery of winded set 4 of electrode plates are smaller than those of splits 14 positioned elsewhere. The inner periphery comprises the innermost periphery and the periphery of some circles abutting on the innermost periphery on which the sharp crimping may be caused. More specifically, the positive collecting section 9 is cut with a cutter from the end edge of positive collecting section 9 towards a direction parallel to a shorter side of stripe-shaped positive electrode plate 1, that is, to boundary 12 between the section which is coated with positive active-substance 1b and positive collector 1a. The spaces of splits 14 are approximately 5 mm in positive collecting section 9 which is positioned in the inner periphery of set 4 of electrode plates, 15 mm in positive collecting section 9 which is positioned in other periphery of set 4 of electrode plates.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner as stripe-shaped positive electrode plate 1.
For the Lithium ion secondary battery constituted of the electrode plates of the embodiment, because the collecting section is formed by folding once on the end section of the collector, the collecting section will not be damaged and not be bent to such an extent that the separator would be punched through even though the collecting plate is pressed when being welded, so that the probability of an inner short-circuit can be reduced. Moreover, because the collecting section is not flexed greatly, the connection between the collecting section and the collecting plates is reliable and stable.
Moreover, in the inner periphery of the set of electrode plates where the spaces of the splits in the collecting section are smaller than those in other section, the resistance on the initial revolved section is small when revolving is started, so that this section can be revolved into a roll around a revolving core rod easily, thereby the inner short-circuit due to the sharp crimping (namely, a sharp angle portion) formed in the collecting section can be prevented.
In this embodiment, collecting section 9 is not provided for the part of collecting section 9 which is positioned in the innermost periphery of set 4 of electrode plates in revolving state. More specifically, this can be realized in the manner that the part of positive collecting section 9 which is positioned in the innermost periphery is cut off after positive collecting section 9 is formed, alternatively, the part of positive collector la which is positioned in the innermost periphery is cut off in advance. And a plurality of splits 14 in the direction from the end edge of positive collecting section 9 to the shorter side of stripe-shaped positive electrode plate 1 are formed.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner.
For the Lithium ion secondary battery formed from the electrode plates of the embodiment, because the collecting section is formed by folding once on the end section of the collector, the collecting section will not be damaged and not be bent to such an extent that the separator would be punched through even though the collecting plate is pressed when being welded, so that the inner short-circuit can be reduced. Moreover, because the collecting section is not flexed greatly, the connection between the collecting section and the collecting plates can be reliable and stable.
Moreover, because the collecting section is not provided for the innermost periphery of the set of electrode plates with small radius of curvature when it is revolved into a roll, and a plurality of splits are provided in the collecting section, the resistance on the initial revolved section is small when revolving is started, so that this section can be revolved into a roll around the revolving core rod quickly, thereby the effect of preventing the inner short-circuit due to the sharp crimping formed in the collecting section can be improved.
In this embodiment, the spaces of splits 14 positioned in the inner periphery of set 4 of electrode plates are smaller than those of splits 14 positioned elsewhere. Meanwhile, collecting section 9 is not provided for the part of collecting section 9 which is positioned in the innermost periphery of set 4 of electrode plates in revolving state. More specifically, this can be realized in the manner that the part of positive collecting section 9 which is positioned in the innermost periphery is cut off after positive collecting section 9 is formed, alternatively, the part of collector 1a of positive electrode which is positioned in the innermost periphery is cut off in advance.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner.
For the Lithium ion secondary battery constituted of the electrode plates of the embodiment, because the collecting section is not provided for the innermost periphery of the set of electrode plates with the smallest radius of curvature when it is revolved into a roll, and in the inner periphery of the set of electrode plates where the spaces of the splits provided in the collecting section in the revolving state are smaller than those in other section, resistance on the initial revolved section is decreased to a minimum when revolving is started, so that this section can be revolved into a roll easily, thereby the inner short-circuit due to the sharp crimping formed in the collecting section can be prevented.
In this embodiment, a corrugation perpendicular to the direction of its length is formed on positive collecting section 9 plate 1. More specifically, the corrugation can be formed by clamping and pressing positive collecting section 9 using corrugation-shaped mould.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner.
For the Lithium ion secondary battery constituted of the electrode plates of the embodiment, the mechanical strength of the collecting section can be further increased with the aid of the corrugation, and the effect of preventing the inner short-circuit due to the flex of the collecting section is improved.
In this embodiment, positive collecting section 9 is not provided for the part of positive collecting section 9 which is positioned in the outermost periphery of set 4 of electrode plates in revolving state as shown in
When cutting off the part of collecting section 9 which is in the outermost periphery of set 4 of electrode plates, the cutting process begins at the end edge of positive collecting section 9 which is positioned in the outermost periphery, continues along boundary 12 between the section which is coated with positive active-substance 1b and positive collector 1a, and ends at the point 70 mm away from the end edge, the section therebetween of positive collecting section 9 being cut off.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner.
For the Lithium ion secondary battery constituted of the electrode plates of the embodiment, when a set of electrode plates revolved into a roll being inserted in a casing, the collecting section in the outmost periphery of the set of electrode plates will be not hanged on the opening of the casing, so that the set of electrode plates can be inserted in the casing easily because the collecting section is not provided for the outmost periphery of the set of electrode plates, the efficiency of production and the quality being able to be increased.
In this embodiment, a plurality of splits 14 from an end edge of positive collecting section 9 towards a direction parallel to a shorter side (wideness) of stripe-shaped positive electrode plate 1 are formed on positive collecting section 9 of positive electrode plate 1, and disposed in the manner that a space of two splits 14 abutting each other on positive collecting section 9 is logarithmically increased from inner periphery to outer periphery of winded set 4 of electrode plates.
More specifically, positive collecting section 9 is cut with a cutter from the end edge of positive collecting section 9 towards a direction parallel to a shorter side of stripe-shaped positive electrode plate 1, that is, towards boundary 12 between the section which is coated with positive active-substance 1b and positive collector 1a, to form a plurality of splits 14. The positive collecting section 9 is cut in the inner periphery of set 4 of electrode plates, in which the portions of spaces being respectively 5 mm, 7 mm and 10 mm between two splits 14 abutting each other are cut respectively 10 times, and last, the positive collecting section 9 is cut 8 times in the outer periphery of set 4 of electrode plates, in which a space between two splits abutting each other is 25 mm.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner as stripe-shaped positive electrode plate 1.
Since in forming of splits 14, a space of two splits 14 abutting each other on positive collecting section 9 is logarithmically increased from inner periphery to outer periphery of winded set 4 of electrode plates, the resistance on the initial revolved section is small when revolving is started, so that this section can be revolved into a roll around a revolving core rod quickly, thereby the effect of preventing the inner short-circuit resulting from the sharp crimping formed in the collecting section can be further enhanced.
In this embodiment, a notch 16 from an end edge of positive collecting section 9 towards a direction parallel to a shorter side (wideness) of stripe-shaped positive electrode plate 1 is formed from a location of approximately 5 mm apart from the inner side at the wideness direction of positive collecting section 9 at the innermost periphery, having a space of 15 mm. The inner periphery of approximately 5 mm forms a strip-shaped collecting section 17.
Specifically, positive collecting section 9 is cut and cut off a part with a cutter from the end edge at the length direction of positive collecting section 9 towards a direction parallel to a shorter side of stripe-shaped positive electrode plate 1, that is, towards boundary 12 between the section which is coated with positive active-substance 1b and positive collector 1a, to form notch 16.
In embodiment 8, one notch 16 is provided on the innermost periphery, however a plurality of notches 16 may be provided on the innermost periphery. The notches provided on the other periphery except the innermost periphery may be splits, or splits and notches.
Moreover, stripe-shaped negative electrode plate 2 can be formed in the same manner as stripe-shaped positive electrode plate 1.
In the cells constituted as the above description, 100 cells were prepared for each of the above embodiments.
In the Lithium ion secondary battery used in comparing example 1, thin metal plates are welded on the ends of the collectors in the whole set of electrode plates from its innermost periphery to its outermost periphery to form positive collecting section 9 and negative collecting section 15 which have the increased thickness, and splits 14 with same spaces are formed on both collecting sections. With such a positive electrode plate 1 and a negative electrode plate 2, the collecting section 9 and negative collecting section 15 are welded onto positive collecting plate 10 and negative collecting plate 11 respectively. The subsequent manufacturing procedures are the same as that of the embodiments. 100 cells like this are prepared.
In the Lithium ion secondary battery used in the comparing example 2, positive collecting section 9 and negative collecting section 15 are formed in the whole set of electrode plates from its innermost periphery to its outermost periphery without splits 14 formed in positive electrode plate 1 and negative electrode plate 2. Positive collecting section 9 and negative collecting section 15 are welded onto positive collecting plate 10 and negative collecting plate 11 respectively. The subsequent manufacturing procedures are the same as that of the embodiments. 100 cells like this are prepared.
Evaluation of the Cells
Fall-impact tests were performed for each 100 cells of the embodiment and comparing examples 1, 2 respectively. The falling height is 75 cm, and falling down of a cell thrice each for a state of the cell that is in an upright, an upside down and a horizontal direction respectively is one cycle.
For each cycle, the open-circuit voltages of a cell are measured to judge whether the inner short-circuit between the opposite electrode plates occurs, which results from pricking the seperator through due to the sharp crimping formed in the positive collecting section 9 or the collecting section of negative electrode. The inner short-circuit occurs when the open-circuit voltage of a cell drops, and the number of the cycles in which the open-circuit voltage of a cell drops can be compared and evaluated. Moreover, for a cell having open-circuit voltage dropped, the position where the inner short-circuit occurs can be confirmed by disassembling and analyzing the cell, and only the cells in which the inner short-circuits between the opposite electrode plates occur, which result from pricking the separators through due to the sharp crimping formed in the collecting sections of positive electrodes or the collecting sections of negative electrodes, can be counted.
Result is Shown in Table 1
As shown in the table, the open-circuit voltages of the cells of embodiments 1-8 which obtain the same results begin to drop after 70 cycles. As a contrast, the open-circuit voltages of the cells of comparing examples 1 begin to drop after 40 cycles, and the open-circuit voltages of the cells of comparing examples 2 begin to drop after 30 cycles. It can be considered that the cells of the embodiment have better structure than that of the comparing ones, so that the inner short-circuits between the positive collecting section 9 and the collecting section of negative electrode are suppressed.
Moreover, comparing the result of disassembling and analyzing the cells having open-circuit voltages dropped, it is found that there is no cell of embodiments 1-8 in which the inner short-circuit between the collecting sections positioned in the innermost periphery of the set of electrode plates occurs, while the positions where the inner short-circuits occur in the comparing examples are all in the collecting sections positioned in the innermost peripheries of the sets of electrode plates.
Therefore, it can be considered that for the cells of the comparing examples, the collecting sections positioned in the innermost peripheries with the smallest radii of curvature of the sets of electrode plates which are revolved into rolls have sharp crimping, so that the separators may be punched through by the crimping, thereby the inner short-circuits may occur. On the other hand, for the cells of the embodiment, the collecting sections are not provided for the innermost peripheries of the sets of electrode plates with the smallest radii of curvature when they are revolved into rolls, so that the inner short-circuits can be suppressed.
While what described above is the collecting section which is formed by folding once an end section of a collector, the times of folding the end section of the collector can be more than one so long as the final thickness of the collecting section is smaller than that of the electrode plates. Although said folding times can be determined according to the thickness of the collector itself, it is preferred that the folding times are 1˜5. Hence, the same effect can be obtained using the collecting section formed by folding the end section of the collector several times. For the case of the embodiments, it is preferred that the positive collector made of aluminum foil is folded 3 times, and the negative collector made of copper foil is folded 2 times.
Moreover, in some electrochemical components, if a collector is made by a material having a higher mechanical strength, a collecting section may be formed directly by the collector not being folded.
The way of “split”, “notch” or “cutoff” is executed on all the layers constituting the collecting section in each of the above embodiments. However, if the way is executed on at least one layer therein, the effect of preventing the sharp crimping from being formed on the collecting section when being revolved may be also obtained, thereby the inner short-circuit being restrained.
Moreover, while what described above is the case that both the positive collecting plate and the negative collecting plate as described above are used in the collecting sections, the same effect can be obtained by using either one of two.
Moreover, while what described above is the case that the liquid electrolyte is used, the same effect can be obtained by using polymer electrolyte as the electrolyte other than liquid.
Moreover, while what described above is a cylinder-shaped Lithium ion secondary battery having the cylindrical size 18650 (18 in diameter and 650 in height), the same effect can be obtained when the shape and the size of cell are not limited.
Moreover, while what described above is a Lithium ion cell, the same effect can be obtained for the electrical components such as cells other than Lithium ion cells, double-layered capacitors and like.
As described above, they can be used to the rolled electrochemical components such as cells, double-charge-layered capacitors and like in which the positive electrode plate and the negative electrode plate are revolved into a roll with a separator being sandwiched therebetween, and the collectors are incorporated with the collecting plates. Furthermore the end sections of the collectors connected with the collecting plates are improved, so that the rolled electrochemical components with high quality can be provided.
Number | Date | Country | Kind |
---|---|---|---|
2003-426864 | Dec 2003 | JP | national |
Number | Name | Date | Kind |
---|---|---|---|
4313741 | Masuda et al. | Feb 1982 | A |
6187473 | Tamezane et al. | Feb 2001 | B1 |
Number | Date | Country |
---|---|---|
2000-077054 | Mar 2000 | JP |
Number | Date | Country | |
---|---|---|---|
20050142436 A1 | Jun 2005 | US |