Claims
- 1. A method of depositing a tapered electrode on a support tube comprising the steps:
- (1) providing a ceramic support tube, having a porous wall and two ends;
- (2) masking at least one circumferential band inside of the tube, where at least the inside of one end of the tube is masked, leaving at least one unmasked band inside of the tube;
- (3) evacuating air from inside of the tube, to provide a permeability gradation in the tube wall between masked and unmasked circumferential bands;
- (4) applying a liquid dispersion of solid electrode material particles to the outside surface of the evacuated tube, wherein liquid flows through the support tube wall, the particles coat a uniform deposit thickness on the outside surface over the unmasked inner bands of the tube where there is unrestricted liquid flow, and coat a tapered deposit thickness on the outside surface over at least part of the masked inner bands of the tube where there is restricted liquid flow, with the thinnest part of the taper near the ends of the support tube; and
- (5) sintering the applied deposit on the support tube.
- 2. The method of claim 1, where the support tube comprises stabilized zirconia, the electrode particles comprise doped LaMnO.sub.3 having a particle size of from 0.2 micrometer to 75 micrometers, and the dispersion is applied in step (4) by immersing the tube in the dispersion.
- 3. The method of claim 1, where the support tube has one closed end, is from 20% porous to 40% porous with an average pore size of from 1 micrometer to 3 micrometers, the electrode particles are ball milled with water and then added to water to form the dispersion, and where the inside masking in step (2) is near the closed end.
- 4. The method of claim 1, where the dispersion has a pH of from 7 to 8.5, and comprises from 1 wt. % to 20 wt. % electrode particle solids.
- 5. The method of claim 1, where the masking in step (2) is by applying to the circumferential band to be masked, a film of organic material which will burn off at temperatures below 900.degree. C.
- 6. The method of claim 1, where the masking in step (2) is by sealingly engaging an inflated bladder to the circumferential band to be masked.
- 7. The method of claim 1, where the electrode particles are dispersed in water, and in step (4), liquid entering the evacuated support tube over the circumferential masking band will have restricted passage and travel substantially parallel to the support wall surface in order to flow through the porous support wall and will deposit less particles than liquid entering over the unmasked band which allows unrestricted flow.
- 8. The method of claim 1, including as final steps, application of a solid oxide electrolyte over most of the electrode deposit and then applying an outer cermet electrode over the electrolyte.
- 9. A support tube having a tapered electrode applied by the method of claim 1.
- 10. A method of depositing a tapered electrode on a support tube comprising the steps:
- (1) providing a stabilized zirconia support tube, having a 20% porous to 40% porous wall, an open end and a closed end;
- (2) masking at least one circumferential band inside of the tube, where at least the inside of the closed end is masked, by sealingly engaging an inflated bladder to the circumferential band to be masked, leaving at least one unmasked band inside of the tube;
- (3) evacuating air from inside of the tube, to provide a permeability gradation in the tube wall between masked and unmasked circumferential bands;
- (4) applying an aqueous dispersion of solid, doped LaMnO.sub.3 particles to the outside surface of the evacuated tube by immersing the tube in the dispersion, wherein water flows through the support tube wall, the particles coat a uniform deposit thickness on the outside surface over the unmasked inner bands of the tube where there is unrestricted liquid flow, and coat a tapered deposit thickness on the outside surface over at least part of the masked inner bands of the tube where there is restricted liquid flow, with the thinnest part of the taper near the ends of the support tube; and
- (5) sintering the applied deposit on the support tube.
- 11. The method of claim 10, where the support tube has an average pore size of from 1 micrometer to 3 micrometers, the doped LaMnO.sub.3 particles have a particle size from 0.2 micrometer to 75 micrometers, the dispersion has a pH of from 7 to 8.5, and the dispersion comprises from 1 wt. % to 20 wt. % solids
- 12. The method of claim 10, where in step (4), water entering the evacuated support tube over the circumferential masking band will have restricted passage and travel substantially parallel to the support wall surface in order to flow through the porous support wall and will deposit less particles than water entering over the unmasked band which allows unrestricted flow.
- 13. The method of claim 10, including as final steps, application of a solid oxide electrolyte over most of the electrode deposit and then applying an outer cermet electrode over the electrolyte.
Government Interests
The Government of the United States of America has rights in this invention pursuant to Contract No. DE-AC21-80ET-17089, awarded by the United States Department of Energy.
US Referenced Citations (5)