Metal-insulator-metal tunnel junctions (MIMTJs) are fundamental building blocks for microelectronics including magnetic tunnel junctions (MTJs) for spintronics and fast access nonvolatile magnetic memory, and Josephson tunnel junctions (JJs) for particle detectors, magnetic field sensors, and qubits for quantum computation. The performance of MIMTJs depends critically on the quality of the insulating tunnel barrier. (L. A. Abelson et al., Proceedings of the IEEE, vol. 92, pp. 1517-1533, 2004.) Considering native oxides can naturally form on the surface of most metals, producing an atomically-thin, uniform, and pinhole-free tunnel barrier represents a major challenge in the research of MIMTJs. In Nb/Al/AlOx/Nb JJs, for example, an ultrathin tunnel barrier is the key to preserve phase coherence across the superconducting Nb electrodes, since the critical current (Ic) through the JJ exponentially decays with the barrier thickness. (A. W. Kleinsasser et al., Applied Superconductivity, IEEE Transactions on, vol. 5, pp. 26-30, 1995.) Thermal oxidation has been the industry standard to produce AlOx tunnel barriers for JJs through in situ oxygen diffusion into an Al wetting layer, however this diffusion mediated process has difficulty achieving a uniform tunnel barrier with a well-defined thickness. (B. Seeber, Handbook of applied superconductivity vol. 2: CRC press, 1998.) Despite successful commercial applications of these JJs in devices such as superconducting quantum interference devices (SQUIDs) and voltage standards, two-level defects (TLDs) in the AlOx tunnel barrier are one of the major sources of decoherence in superconducting qubits. (R. McDermott, Applied Superconductivity, IEEE Transactions on, vol. 19, pp. 2-13, 2009.)
Provided are methods for forming tunnel barrier layers as well as multilayer structures comprising the tunnel barrier layers.
In one aspect, methods for forming tunnel barrier layers are provided, including a method comprising exposing a surface of a material, the surface free of oxygen, to an initial water pulse for a pulse time and at a pulse temperature, the pulse time and pulse temperature selected to maximize hydroxylation of the surface; and exposing the hydroxylated surface to alternating, separated pulses of precursors under conditions to induce reactions between the hydroxylated surface and the precursors to form a tunnel barrier layer on the surface of the material via atomic layer deposition (ALD), the tunnel barrier layer having an average thickness of no more than 1 nm and being formed without an intervening interfacial layer between the tunnel barrier layer and the surface of the material.
In another aspect, multilayer structures are provided, including a multilayer structure comprising a tunnel barrier layer formed directly on a surface of a material without an intervening interfacial layer between the tunnel barrier layer and the surface of the material, the tunnel barrier layer composed of an amorphous metal oxide, wherein the tunnel barrier layer has an average thickness of no more than 1 nm.
Other principal features and advantages of the disclosure will become apparent to those skilled in the art upon review of the following drawings, the detailed description, and the appended claims.
Illustrative embodiments of the invention will hereafter be described with reference to the accompanying drawings, wherein like numerals denote like elements.
Provided are methods for forming tunnel barrier layers as well as multilayer structures comprising the tunnel barrier layers. The methods are based, at least in part, on the inventors' findings regarding how to achieve hydroxylation of a material surface followed by tunnel barrier layer deposition via atomic layer deposition (ALD) while minimizing or preventing formation of an interfacial layer between the tunnel barrier layer and the material surface. The phrase “interfacial layer” refers to the incorporation of oxygen (O) into the material from the surface of that material (i.e., surface-to-bulk incorporation of oxygen). The resulting oxygen-containing surface region of the material is referred to as an interfacial layer (IL). An interfacial layer on aluminum may be referred to herein as an AlOx interfacial layer and an interfacial layer on iron may be referred to herein as an FeOx interfacial layer. Neither the thickness nor the stoichiometry of an interfacial layer is well defined. (See
The methods may be carried out on an apparatus based on that described in U.S. Pat. Pub. No. 20160040288, which is hereby incorporated by reference in its entirety. Such an apparatus includes a chamber for ultrahigh vacuum physical vapor deposition (UHV PVD) or high/ultrahigh vacuum chemical vapor phase deposition (HV/UHV CVD) at a base pressure of 10−8 Torr or lower (e.g., 10−8 to 10−10 Torr) and a HV chamber for in situ ALD at a base pressure of 5×10−6 Torr or lower (e.g., 5×10−6 to 5×10−7 Torr). Such an apparatus includes an additional chamber for in situ sample transfer between the two deposition chambers at a base pressure of 10−4-10−6 Torr or lower (e.g., 10−6 to 10−7 Torr). The in situ transfer process may be fast, e.g., less than about 2 minutes, less than about 1.5 minutes, or in the range of from about 30 seconds to 1.5 minutes. The ALD chamber in the apparatus may be blackbody heated to a desired temperature (i.e., the chamber walls are heated such that the chamber walls themselves emit sufficient energy to heat the interior of the chamber, and thus, components within the interior, including a substrate upon which the tunnel barrier layer is formed). Blackbody heating may be accomplished via resistive heat tape wrapped around the outer surface of the ALD chamber.
Methods for forming the tunnel barrier layers are provided. In embodiments, the method comprises activating a surface of a material onto which the tunnel barrier layer is to be formed by functionalizing the surface with hydroxyl groups. The material (and its surface) are initially characterized as being free of oxygen (i.e., prior to activation). The oxygen may originate from O2 or other compounds such as H2O. By “free” it is meant that there is no oxygen or the amount of oxygen is so small so as to not to materially affect the properties of the tunnel barrier layer formed on the surface of the material. Prior to activation, scanning tunneling spectroscopy (STS) may be used (in situ) to confirm that the surface of the material is bare, i.e., is free of oxygen (e.g., from dI/dV spectra). (See
Next, the method comprises exposing the activated surface (i.e., hydroxylated surface) to alternating, separated pulses of precursors (e.g., an organometallic precursor pulse followed by a water precursor pulse) under conditions sufficient to induce reactions between the hydroxylated surface and precursors, thereby providing the tunnel barrier layer via ALD on the surface of the material. The activation and the tunnel barrier layer deposition steps may be carried out in the ALD chamber of the apparatus described above.
In embodiments, the material which is to be hydroxylated and on which the tunnel barrier layer is to be formed is a wetting layer. Various materials may be used for the wetting layer, depending upon the application. In embodiments, the wetting layer is composed of a metal (or a metal alloy), e.g., aluminum (Al), magnesium (Mg), hafnium (Hf), iron (Fe). The wetting layer may be characterized by its thickness, i.e., an average value measured at a representative number of locations across the surface. In embodiments, the average thickness is at least 5 nm, at least 6 nm, or at least 7 nm. In embodiments, the average thickness is in a range of from 0.5 nm to 7 nm. Because embodiments of the present methods are actually able to minimize or prevent the formation of interfacial layers, thicker wetting layers may be used as compared to some conventional approaches in which the thickness of the wetting layer had been minimized (although not eliminated) in order to reduce the effect of an interfacial layer. The wetting layer may be formed in the UV PVD or UV CVD chamber in the apparatus described above. The wetting layer may be formed on a variety of other material layers, depending upon the application and desired multilayered structure (e.g., desired metal-insulator-metal structure). Other material layers include other metals and their alloys, e.g., niobium (Nb), iridium (Ir), cobalt (Co). A specific illustrative alloy is FeCo. Semiconductors, e.g., Si, may also be used.
In embodiments, no wetting layer is used and the material which is to be hydroxylated and on which the tunnel barrier layer is to be formed is determined by the desired multilayer structure (e.g., to form a metal insulator metal tunnel junction (MIMTJ), a magnetic tunnel junction (MTJ), etc.). By way of illustration, if the desired multilayer structure is a MTJ, the material may be a ferromagnetic material, e.g., iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. These embodiments are related to the unexpected finding that the present methods can achieve extremely thin tunnel barrier layers having high Eb even without the use of a wetting layer (see Example 3).
In the present methods, activation of the surface of the material (e.g., wetting layer or ferromagnetic material) is activated using a water pulse to functionalize the surface with hydroxyl groups. It has been found that certain conditions under which the surface of the material is exposed to the water pulse affect the extent of, and uniformity, of the hydroxylation on the surface. That is, it is not enough to simply make use of an initial water pulse. Instead, the water pulse conditions are desirably selected to provide an optimal amount (e.g., surface density) of adsorbed water on the surface in order to achieve optimal hydroxylation, e.g., to maximize the number of hydroxyl groups to completely cover the surface, including with a monolayer of the hydroxyl groups. Complete coverage is useful to achieve a pinhole free, atomically thin tunnel barrier. The amount of adsorbed water is desirably sufficiently high to achieve proton transfer between pairs of adsorbed water molecules in order to dissociate the water into OH− and H+ groups. However, the amount of adsorbed water is desirably not so high (e.g., greater than a monolayer of water) to lead to the formation of water clusters. The water pulse conditions include the pulse time (the length of time the surface is exposed to the water pulse). In embodiments, the pulse time is less than 3 seconds, in the range of 1 to 3 seconds, or about 2 seconds.
The water pulse conditions also include the pulse temperature (the temperature of the surface during exposure to the water pulse), which is also selected to achieve optimal hydroxylation, e.g., to maximize the number of hydroxyl groups on the surface. The temperature is desirably sufficiently high to facilitate water dissociation, but not so high as to lead to the dissociation of OH− groups to O− and H+ groups. Hydroxyl group dissociation can result in diffusion of oxygen into the material, effectively creating an interfacial layer which degrades the properties of the tunnel barrier layer. In embodiments, the pulse temperature is in the range of from about 150° C. to about 190° C. In embodiments, the pulse temperature is in the range of from about 125° C. to about 215° C., from about 120° C. to about 210° C. or from about 130° C. to about 220° C.
Confirmation of optimal water pulse conditions which achieve the desired result may be carried out using STS as described in the Examples below, including by achieving a maximum Eb for the tunnel barrier layer. More specifically, optimal water pulse conditions may be those which provide a desired ALD coverage defined as the percent of STS spectra showing a tunnel barrier layer having a Eb>1 eV (barrier heights <1 eV are associated with thermal AlOx, which generally has a Eb of about 0.6 eV to 1 eV). The percent of STS spectra refers to the percentage of a total number of collected STS spectra (e.g., 100) taken from random locations across the surface of the tunnel barrier layer. (See Examples, below.) In embodiments, the optimal water pulse conditions are those which provide an ALD coverage of at least 85%, at least 90%, at least 92%, or at least 94%. (See
As noted above, in the second, tunnel barrier layer deposition step, the activated (hydroxylated) surface is exposed to alternating, separated pulses of precursors to induce reactions between the hydroxylated surface and the precursors, thereby forming the tunnel barrier layer via atomic layer deposition (ALD) on the activated surface. The choice of precursors determines the composition of the tunnel barrier layer. However, the tunnel barrier layer is composed of a dielectric material. Suitable dielectric materials include metal oxides such as Al2O3, MgO, and HfO2. In this step, precursors (e.g., H2O and trimethylaluminum for Al2O3 deposition) and conditions (pulse time, pulse temperature, use of purge pulses, etc.) may be adjusted as known in the art. The number of pulse pairs, or ALD cycles, may be adjusted to provide a desired thickness for the tunnel barrier layer. In embodiments, the average thickness of the tunnel barrier layer is no more than 1.5 nm, no more than 1.3 nm, no more than 1.2 nm, no more than 0.7 nm, no more than 0.4 nm, or no more than 0.2 nm. The term “average” here as the same meaning as described above with respect to the thickness of the wetting layer. This includes embodiments in which the average thickness of the tunnel barrier layer is in the range of from 0.1 nm to 1.5 nm or from 0.2 nm to 1.2 nm. The thickness of the tunnel barrier layer may be reported as the thickness provided by the selected number of ALD cycles, e.g., 1 ALD cycle, 5 ALD cycles, etc.
It has been further found that other certain conditions of the method further enable the formation of high quality tunnel barrier layers on the surface of the material without leading to the formation of an intervening interfacial layer. One such condition involves the use of a preheated ALD chamber. In particular, the ALD chamber used to carry out the activation and tunnel barrier layer deposition steps may be preheated prior to introducing the material into the ALD chamber. The preheated temperature depends upon the dielectric material to be used to form the tunnel barrier layer. The preheated temperature is generally greater than the selected pulse temperature (described above). In embodiments the preheated temperature is at least about 250° C., at least about 260° C., or at least about 265° C.
Another such condition involves the use of dynamic heating of the material surface prior to activation and tunnel barrier layer deposition. By “dynamic heating” it is meant that the temperature of the material surface is changing (i.e., increasing) rather than constant during the step in which dynamic heating is used. In particular, after introducing the material to the preheated ALD chamber, the material may be heated at a selected heating rate for a selected time to the selected pulse temperature (described above) prior to initiating activation and tunnel barrier layer deposition. As described above, the selected pulse temperature may be in the range of from about 150° C. to about 190° C. The selected time is generally quite fast, in order to minimize or prevent incorporation of oxygen into the material. In embodiments, the selected time is about 30 minutes or less, about 20 minutes or less, about 15 minutes or less, or in the range of from about 10 to about 30 minutes. The selected heating rate depends upon the initial temperature of the material as well as the selected chamber vacuum, the selected pulse temperature and the selected time. Confirmation of optimal dynamic heating conditions may be achieved as described above with respect to the optimal water pulse conditions. (See
After dynamic heating to the selected pulse temperature, activation and tunnel barrier layer deposition are carried out as described above. Dynamic heating may be used during activation and tunnel barrier layer deposition as well. However, although the heating rate is generally quite fast, hydroxylation and the rate of formation of the tunnel barrier layer via ALD are much faster, e.g., 10 times as fast.
After tunnel barrier layer deposition, the method may include additional steps, e.g., formation of another material layer on the tunnel barrier layer, depending upon the application. For example, a layer of metal may be formed to provide a metal-insulator-metal multilayer structure or a layer of semiconductor (e.g., Si) may be formed to provide a semiconductor-insulation-semiconductor multilayer structure.
The resulting tunnel barrier layer may be characterized by certain properties, including any of the properties described in the Examples below. By way of illustration, the tunnel barrier layer may be characterized by its tunnel barrier height, Eb. The tunnel barrier height may be measured using STS and determined from dI/dV spectra as described in the Examples below. In embodiments, the tunnel barrier layer is an Al2O3 tunnel barrier layer having an Eb of at least 1.2 eV, a least 1.3 eV, at least 1.4 eV, at least 1.5 eV, or at least 1.6 eV. This Eb may be an average Eb as determined from a representative number of locations across the tunnel barrier layer. (See
The tunnel barrier layer may be characterized by its band gap, which may be measured using STS as described in the Example below. In embodiments, the tunnel barrier layer has a band gap which is the same as the bulk band gap. By “bulk band gap” is meant the band gap value for the material of the tunnel barrier layer in its bulk, single-crystalline form. By “same,” it is meant that the values are within ±15%, ±10%, ±5%, ±1%, or less, of each other. In embodiments, the tunnel barrier layer is an Al2O3 tunnel barrier layer having a band gap of about 2.5 eV.
The tunnel barrier layer may be characterized by its lack of crystalline structure, i.e., by being amorphous. This is by contrast to epitaxial layers, having a well-defined crystal structure and crystal orientation relative to the surface on which it is grown.
Devices comprising the tunnel barrier layer and the multilayer structures are also provided. An illustrative device is a Josephson Junction device. (See, e.g.,
Introduction
This Example uses Atomic Layer Deposition (ALD) for the synthesis of atomically-thin tunnel barriers for high performance MIMTJs. ALD is a chemical vapor process that utilizes self-limited surface reactions to grow films one atomic layer at a time [6, 7]. The ALD Al2O3 process is illustrated in
Precise ALD growth and nucleation on metals is challenging, e.g., due to the issue of native oxide growth. For example, ALD nucleation on inert metal surfaces, such as Pt and Au, can be completely frustrated for the first 30-50 cycles of alternating precursor pulses whereas for reactive metals, such as Al, even in situ deposited films can acquire an interfacial layer (IL) of AlOx up to ˜2 nm thick [9-11]. In a previous work, Lu et al fabricated Nb/Al/Al2O3/Nb JJs using in situ ALD of Al2O3. It has been determined that the presence of an IL>0.5 nm in thickness could be at least partially attributed to the vacuum pressure (˜500 mTorr) during sample transfer and pre-ALD heating [11-13]. This IL prevented the realization of truly atomically-thin tunnel barriers and led to poor quality JJs. By contrast, in this Example, these challenges are addressed in part by performing the transfer and pre-ALD heating under high-vacuum (HV). This Example reports the successful fabrication of atomically-thin ALD Al2O3 tunnel barriers. In situ scanning tunneling spectroscopy (STS) was employed to probe the growth mechanisms and physical properties of the ALD Al2O3 tunnel barriers and JJs were fabricated to illustrate the viability of ALD Al2O3 tunnel barriers for MIMTJs.
For samples which underwent in situ STS characterization, a bilayer of Nb (20 nm)/Al (7 nm) was magnetron sputtered onto a Si/Au (50 nm) substrate which was mechanically clamped to a sample stage to serve as the ground contact for the Scanning Tunneling Microscope (RHK). The Au was thermally evaporated onto an updoped Si wafer with a native oxide. An ex situ Atomic force microscope measured its surface roughness to be ˜1.2 nm. Immediately following the Al sputtering, an aluminum oxide tunnel barrier was formed by either thermal oxidation or ALD. For the thermal oxidation samples, UHP O2 (99.993%) was introduced to the sputtering chamber for an oxygen exposure of 1150, 1020, and 42 torr-seconds, respectively. The samples with ALD tunnel barriers were transferred to a preheated ALD chamber and then heated for 15 min or 75 min to a temperature of 200° C.-220° C. Following sample heating, reagents H2O and trimethylaluminium (TMA) were pulsed into the ALD chamber for 1-3 s with a purge step (35 s of N2) between pulses to deposit the ALD Al2O3 tunnel barriers.
After tunnel barrier fabrication, the samples were transferred under high vacuum (HV), in situ, to the STM chamber which had a pressure of ˜2×10−10 Torr. A single mechanically-cleaved Pt—Ir STM tip was used for all STM studies. Constant height IV and dI/dV spectroscopy were taken simultaneously using the lock-in amplifier method with a voltage modulation of 100 mV at 1 kHz. The tunnel barrier height was determined by the intersection of two bisquare-method linear fits to ln(dI/dV). (See M. M. Ugeda, et al., Giant bandgap renormalization and excitonic effects in a monolayer transition metal dichalcogenide semiconductor, Nat. Mater. 13, 1091 (2014).) The endpoints for this linear fit were determined by eye. One line fit the band gap regime, and the other the conduction band. This ln(dI/dV) linear-fit method is chosen over I-V or (dI/dV)/(IN) fit methods for its insensitivity to high noise in STS spectra. (See R. M. Feenstra, et al., Low-temperature tunneling spectroscopy of Ge (111)c (2×8) surfaces, Phys. Rev. B 71, 125316 (2005) and L. Dorneles, et al., The use of Simmons' equation to quantify the insulating barrier parameters in Al=AlOx=Al tunnel junctions, Appl. Phys. 500 Lett. 82, 2832 (2003).) Approximately 40-80 dI/dV spectra are taken on each sample >100 nm apart from one another in order to get reasonable statistics on the sample's surface.
The ab initio molecular dynamics simulations for the initial water activation pulse used a 2×2 supercell of FCC Al (111) surface under constant equilibrium volume and temperature and adopted Bohn-Oppenheimer molecular dynamics as implemented in VASP [14-16]. The canonical ensemble simulations employed the London dispersion correction using the van der Waals density functional of Langreth and Lundqvist [17] with a high plane wave energy cut-off of 450 eV to ensure high precision. The electronic and ionic convergence criteria used were 10−4 eV and 10−3 eV respectively. Energy barrier and reaction pathways are investigated using the climbing-image-nudge elastic-band method (D. Sheppard, et al., Optimization methods for finding minimum energy paths, J. Chem. Phys. 128, 134106 (2008)) as implemented in the QUANTUM ESPRESSO code (G. Paolo, et al., QUANTUM ESPRESSO: A modular and open-source software project for quantum simulations of materials, J. Phys. Condens. Matter 21, 395502 (2009)).
Nb—Al/ALD-Al2O3/Nb trilayers were fabricated in a homemade deposition system, which integrated UHV sputtering and ALD in situ [12, 18]. For comparison, traditional thermally oxidized Nb—Al/AlOx/Nb trilayers were also fabricated. The Nb films were sputtered at 1.7 nm/s to minimize the formation of NbOx from trace oxygen. The sputtering chamber had a base pressure of ˜10−7 Torr or better and the sample stage was chilled-water cooled to approximately 10° C. The bottom Nb was 150 nm, and the top Nb was 50 nm. Samples with ALD tunnel barriers were transferred in situ to the preheated ALD chamber and heated for 75 min under HV. The wafer design used to investigate the quality of tunnel barriers contains 12 square junctions of four different sizes ranging from 4 μm×4 μm to 10 μm×10 μm and was fabricated using the self-aligned niobium trilayer process described in W. Chen, et al., Fabrication of high-quality Josephson junctions for quantum computation using a self-aligned process, Microelectron. Eng. 73, 767 (2004). The JJ dc current-voltage characteristics (IVC) were measured at 4.2K in a liquid helium storage dewar.
Results and Discussion
In Situ Scanning Tunneling Spectroscopy and Molecular Dynamics Simulations
ALD is a low-vacuum process that is incompatible with UHV required for both physical vapor deposition of functional electrodes and in situ characterization using STM. To address this issue, an integrated Sputtering-ALD-STM system was used to allow for UHV deposition of metals, UHV STM characterization of surfaces and interfaces, and HV (10−6-10−7 Torr) in situ sample transportation between the chambers [18]. This HV transport reduces the metal electrode's exposure to trace gases and hence IL formation. This Example further avoids IL formation by addressing the temperature difference between sputtering at 10-14° C. and ALD at 200° C.-220° C. In particular, the samples were inserted into a preheated ALD chamber for different times and dynamically heated to 200° C.-220° C. under HV. Two dynamic heating times of 75 min and 15 min are described here to illustrate the importance of controlling this procedure in order to achieve a clean interface between the Al and ALD Al2O3 tunnel barrier.
In
To initiate the ALD Al2O3, the Al wetting layer was exposed to a H2O pulse to hydroxylate its surface. In order to understand the kinetics of this hydroxylation process, the behavior of H2O on the Al surface was investigated using Ab-initio molecular dynamics (AIMD) and Climbing-Image-Nudge Elastic Band (CI-NEB) simulations. When only one H2O molecule (i.e. without H2O molecules in proximity) is present on the Al surface, H2O dissociation into OH− is thermodynamically unfavorable. In contrast, when multiple H2O molecules are present on the Al (111) surface, dissociation occurs after just a few ps. A proton transfer between nearby H2O molecules creates OH− and H3O+, followed by H3O+ dissociation into H2Oad and H+ad. The reaction pathway of this dehydrogenation process has an overall net exothermic reaction with a ˜0.5 eV energy barrier. The remaining transition states were verified with additional NEB simulations to have very small or negligible energy barriers. This shows that the H2O areal density from the H2O pulse can be used to ensure an efficient hydroxylation reaction and a uniform monolayer of OH− on the Al surface. The stability of these OH− groups is also a consideration as dissociation into 0 and Wads could lead to oxygen diffusion into the Al wetting layer and IL formation. However, it was determined that these OH− groups do not readily dissociate at a temperature of ˜200° C. Nevertheless, this dissociation may become a concern at significantly higher temperatures.
In order to experimentally probe this hydroxylation process, one cycle of ALD Al2O3 was performed on an Al wetting layer with an initial H2O pulse of variable duration.
In addition to its paramount role in nucleation, the hydroxylation of the Al wetting layer prevents oxygen from diffusing into the Al to form an IL during the ALD process. This argument is supported by the dI/dV characteristics and Eb observed for the thermal AlOx and the ALD Al2O3 tunnel barriers. The dI/dV spectra for a thermal AlOx tunnel barrier of ˜1.3 nm, in estimated thickness [13], is shown alongside a ten-cycle ALD Al2O3 tunnel barrier with a comparable thickness of 1.2 nm in
It is particularly interesting that the ALD Al2O3 Eb value was maintained as the number of ALD cycles, N, varied from 1 to 10 (
Josephson Junction Characterization
To demonstrate how this ALD Al2O3 tunnel barrier performs in a demanding MIMTJ application, JJs were fabricated and their dc current-voltage characteristics (IVCs) measured at 4.2 K. The IVC of a 5-cycle junction with a designed area of 100 μm2 is shown in
Recently, by measuring the dependence of JJ's critical current density on oxygen exposure, a proxy for tunnel barrier thickness d, Kang et al determined the thermal AlOx tunnel barrier Eb to be ˜0.64 eV [13]. (There was a factor of 2 error in the exponential of Eq (1). Once corrected, their reported thermal AlOx Eb was 0.64 eV.) Notice that it is very difficult to calibrate the relationship between d and oxygen exposure. In contrast, due to the self-limited, layer-by-layer growth nature of ALD, the growth rate of the ALD Al2O3 tunnel barrier has been precisely calibrated as dALD=0.115±0.005 nm/cycle [11]. To determine the ALD JJ Eb, the measured critical current density, Gn=(RnA)−1∂Jc, was plotted against dALD in
where me is the electron mass, ℏ is the Planck constant, and Go is the specific conductance for dALD=0. The tunnel barrier height determined from the best fit was Eb=1.10±0.06 eV. This Eb value agrees well with the STS measurements.
Ideal tunnel junctions require a uniform tunnel barrier with no microscopic pinholes. Pinholes lead to subgap leakage current and a distorted magnetic field dependence on critical current, Ic. The magnetic field dependence of the critical current, Ic(H), for a 5-cycle junction is shown in
A denser tunnel barrier should have fewer atomic-scale two-level defects (TLDs). TLDs have been identified as one of the major sources of decoherence for superconducting qubits, which are considered one of the strongest candidates for the implementation of scalable quantum computing [29]. It has been observed that TLDs embedded inside the oxide tunnel barrier and/or at the superconductor/oxide interface can couple strongly to Josephson qubits. These TLDs lead to splitting in the transition energy spectrum of the qubit, large fluctuations in Ic, and distortions in junctions' switching current distribution Psw(I) [30-32]. Therefore, Psw(I) can be used as a diagnostic tool for the detection of TLDs in tunnel barriers which couple strongly to the junction.
In summary, an in situ STS study has been carried out to understand the nucleation mechanisms of ALD Al2O3 on an Al wetting layer. It has been found that a well-controlled hydroxylation of the Al wetting layer, through a carefully controlled first H2O pulse, enables the creation of an atomically-thin ALD Al2O3 tunnel barrier which is of significantly higher quality than the industrial standard thermal AlOx tunnel barrier. Specifically, the ALD Al2O3 tunnel barrier has a high Eb of 1.42 eV which is maintained as the barrier thickness is varied in the range of 0.12-1.2 nm. Furthermore, this ALD Al2O3 tunnel barrier has a band gap of 2.5 eV and exhibits hard electrical breakdowns similar to high-quality epitaxial Al2O3 thin films. In contrast, the thermal AlOx tunnel barrier has a low Eb of −0.67 eV only in the barrier thickness range exceeding 0.6 nm. At smaller thicknesses, enhanced soft electrical breakdown occurs and the Eb decreases. Finally, it was found that minimizing the pre-ALD exposure of the Al surface in the ALD chamber, even in high vacuum, prevented AlOx IL formation which otherwise leads to a reduced Eb, especially at smaller barrier thicknesses. This result demonstrates for the first time the viability of the ALD process to create an atomically-thin Al2O3 tunnel barrier which has a significantly denser, less defective internal structure than thermal AlOx—as demanded for the next generation of high performance MIMTJs.
Introduction
As described above, the present industry standard tunnel barrier for MIMTJ devices is thermal AlOx which is created through a controlled oxygen diffusion into an Al wetting layer [5] shown schematically in
In particular, Example 2 makes use of ALD of Al2O3. As described above, ALD is a chemical vapor process (CVD) which grows Al2O3 one atomic layer each time through a series of H2O and Trimethylaluminium (TMA) reactant pulses. Purge steps between pulses prevent CVD reactions to enable self-limited, conformal growth on the sample surface. This serial process enables atomic-scale control of the Al2O3 thickness as each ALD reaction cycle deposits a single layer of Al2O3 0.11-0.12 nm thick [10, 11]. Ideal 1-cycle and 5-cycle ALD Al2O3 tunnel barriers are depicted schematically in
However, achieving such an ideal ALD Al2O3 tunnel barrier is by no means trivial since ALD Al2O3 growth cannot begin unless a hydroxylated surface is available [12, 13]. Unfortunately, such a surface is not readily available on metals. While hydroxylation of a metal surface is possible through a so-called in situ incubation process by sacrificing the first tens of ALD cycles [13], the treated metal surface typically contains a defective interfacial layer (IL) that is several nm in thickness. Such a thick IL is unacceptable for MIMTJs. Even with a thin IL, depicted schematically in
In Example 2, molecular dynamics simulations and in situ Scanning Tunneling Spectroscopy (STS) were employed to investigate the possible mechanisms of IL formation and its influence on the growth and dielectric properties of atomically-thin and ultrathin ALD Al2O3 tunnel barriers. It is speculated that thermal oxidation of the Al wetting layer occurs during a prolonged pre-ALD heating time from exposure to trace O2 or H2O. This IL reduced the Al2O3 barrier height, especially in the atomically-thin regime. Minimizing the Al wetting layer's pre-ALD exposure led to an increased barrier height which was constant with thickness. A transition from predominantly soft dielectric breakdown in the presence of an IL to hard breakdown when the IL becomes negligible was also observed. Considering the soft breakdown is characteristic to the thermal AlOx tunnel barriers while the hard breakdown resembles that of crystalline Al2O3, eliminating IL indeed is shown to be critical for high-quality ALD Al2O3 tunnel barriers for MIMTJs.
Computational Simulations on the IL growth mechanisms and its effect on ALD growth were carried out using Density Functional Theory (DFT) calculations using the Nudged-elastic band (NEB) method [17] and ab-initio molecular dynamics (AIMD) simulations under constant temperature and volume (NVT) with 1 fs for each trajectory step as implemented in VASP[18] and Quantum Espresso [19] codes. Detailed procedures to model the Al surface reactions have been provided elsewhere [20-22].
To create the metal-insulator structure for in situ Scanning Tunneling Spectroscopy (STS), a bilayer of Nb (20 nm)/Al (7 nm) was DC magnetron sputtered onto a Si/Au (50 nm) substrate. The Nb and Al layers were sputtered at 1.7 nm/s and 0.5 nm/s respectively and the Au was evaporated onto an undoped Si wafer with a native oxide to serve as a ground contact for the SPM system (RHK). In order to reduce oxidation following magnetron sputtering, the samples were transferred to the ALD chamber in a unique, home-built vacuum chamber which is capable of in situ sample transport under HV between the sputtering, ALD, and SPM chambers. [23] To reach a suitable temperature for ALD, the samples had to bridge the temperature difference of ˜12° C., for sputtering, to 100-350° C. for ALD [24]. After the in situ transport to the preheated ALD chamber, the samples were dynamically heated under HV in preparation for ALD. Following heating, 1-5 cycles of ALD Al2O3 were deposited with a 5 sccm N2 carrier gas to create the dielectric tunnel barrier. The first reactant pulse was H2O in order to hydroxylate the Al surface to allow for ALD nucleation in the first ALD cycle. This first H2O pulse has been described in detail in Example 1. To compare the characteristics of ALD Al2O3 tunnel barriers to traditional thermal AlOx tunnel barriers, a ˜0.3 nm and ˜0.6 nm thermal AlOx tunnel barriers were also fabricated using a 3.81 Torr-sec and a 42 Torr-sec UHP O2 exposure in the sputtering chamber [6].
To examine the Al2O3 tunnel barriers in situ, the samples were transferred, under HV, to the SPM chamber for measurement immediately following tunnel barrier fabrication. The SPM chamber had a pressure of ˜2×10−10 Torr. A single mechanically-cleaved Pt—Ir Scanning Tunneling Microscopy (STM) tip was used for all SPM studies. Constant height IV and dI/dV spectroscopy were taken simultaneously using the lock-in amplifier method with a voltage modulation of 100 mV at 1 kHz or 30 mV at 5 kHz. The STM tip was held fixed at each scanned location and the bias was sequentially ramped up and down 20 times to examine the dielectric breakdown of the Al2O3 tunnel barrier.
Numerical Simulations on the Effect of IL Formation
Should an IL form at the Al—Al2O3 interface, it most likely forms during the pre-ALD sample heating step of the tunnel barrier fabrication. To reach a suitable temperature for ALD, the samples had to bridge the temperature difference of ˜12° C., for sputtering, to 100-350° C. for ALD [24]. Trace O2 or H2O originating from the ALD reactor during this heating step may form an IL via the thermal oxidation process. To shed light on the microscopic mechanisms of this IL formation, a number of ab-initio molecular dynamics (AIMD) simulations were run.
Aside from oxygen, a thermal AlOx IL may form indirectly upon exposure to H2O. The H2O source may originate from either the initial hydroxylating H2O pulse or from exposure to trace H2O from the ALD reactor which has a vacuum pressure on the order of 10−4 to 10−5 Torr during pre-ALD sample heating. The second simulation shown in
To understand how the presence of an IL may impact the ALD Al2O3 film growth, the ideal case of ALD growth on hydroxylated Aluminum surface without an IL is evaluated (
Throughout the AIMD simulations, intermolecular hydrogen bonds present amongst the adsorbed OH− molecules were observed, as evidenced by the frequent alignments of the hydrogen atoms. The OH− intermolecular bond length laterally is quite short, in the range of 1.4 Å to 2.0 Å. A hydrogen bond results and horizontally-aligns the OH− adsorbates. This horizontal alignment can only be achieved by a high OH− surface packing density on the Al (111) substrate. As a consequence of this horizontal alignment, the O ion in the OH− is exposed towards the Al cation from the TMA. A vertical OH− produces significant steric hindrance for the TMA adsorption on the OH−. The horizontal OH− alignment, which forms from a high OH− surface density on the Al(111), enables an efficient TMA adsorption on the hydroxylated Aluminum wetting layer.
While it has been well-established that the ALD reactions, particularly with respect to TMA are self-terminating, that is not the case for the hydroxylation of the Al(111) surface. Rougher Al surface topology, created by the ingress of oxygen from a thermal AlOx IL, may lead to a reduced OH− surface density. The additional steric hindrance from now vertically aligned OH− will likely lead to a reduced TMA density in the first ALD cycle; as shown schematically in
Further AIMD simulations were conducted to evaluate the energy barrier for the release of CH4 from the TMA molecule on the hydroxylated Al surface following the reaction in equation (1).
∥—OH+∥—O—Al—(CH3)3(II-O)2—Al(CH3)2+CH4(g) (1)
AIMD snapshots for the simulation of the reaction are shown in
In Situ Scanning Tunneling Spectroscopy
From the simulations in
To achieve this, a short-term dynamic pre-ALD heating strategy was developed and both the effect of sample temperature and sample heating time in the ALD chamber were probed.
T(t)=Ti+(Tf−Ti)(1−e−t/τ) (2)
Ti is the sample temperature prior to heating, Tf is the steady-state temperature, and τ is the time constant of the fit. As expected, increasing the blackbody heater wattage led to a significantly reduced time constant and an increase of the maximum sample temperature. This dynamic heating strategy has the advantage of bringing the sample's temperature to ALD-suitable temperatures very quickly at the expense of a non-constant temperature during ALD. Depending on the heater wattage and time position on
To experimentally examine the temperature dependence of the hydroxylating H2O pulse, in situ Scanning Tunneling Spectroscopy (STS) was utilized to probe the Local Density of States of the 1 cycle ALD Al2O3 samples with different temperatures during the 1st H2O pulse. The bias voltage in STS dI/dV spectra corresponds to the electron energy, in eV, above the Fermi level. On the Log dI/dV scale, the band gap regime should be flat, and the conduction band should be roughly linear [29]. The barrier height, (Eb), defined as the onset of the conduction band, is reflective of the quality and density of Al2O3 within the tunnel barrier [9, 30]. Representative dI/dV and IV STS spectra are shown in
The possibility still remains that an IL may form from exposure to trace oxygen and H2O in the ALD chamber during the time it takes to heat the sample to this temperature window of 150° C. to 190° C.
When these tunnel barriers are grown thicker, the contribution of the interface to tunneling reduces. Therefore at 5 cycles ALD (˜0.6 nm) in thickness, the STS dI/dV spectra are primarily probing the Al2O3 density rather than the disorder at the Al interface. As can be seen in
However, aside from Eb there are additional requirements that a tunneling barrier must fulfill to serve as a useful insulating layer for MIMTJs. That is, that the insulator the ALD Al2O3 film must be spatially uniform across the junction area and must be pinhole-free through the barrier thickness. The conformal nature of ALD gives ALD Al2O3 tunnel barriers a unique advantage in special uniformity over PVD-deposited or thermally oxidized tunnel barrier such as AlOx. However, the pinhole-free nature of ALD Al2O3 is still in question. Also of interest is the spatial uniformity of the quality of the tunneling barrier, namely Eb. To examine these properties in the ALD Al2O3 tunnel barriers, the STM was scanned over a small area of just 32 nm in
The behavior of these insulating films under intense dielectric stress (>10 MV/cm) can provide additional clues on the nature and significance of the Al—Al2O3 interface. Many of the thermal and ALD spectra broke down under the local STM-induced electric field as the STM bias was ramped up and down many times. Thermal AlOx is known to breakdown (BD) in a gradual, soft manner as disorder increases within the tunnel barrier through defect migration. Eventually the STS spectrum becomes linear/metallic. [9, 30, 32, 34-36] Interestingly, this soft BD effect was observed in all of the films, but at varying severity.
In contrast, ALD films without an IL displayed a very different form of BD.
A simple statistical study was done to shed light into how often these BD events occur in the three types of different atomically-thin tunnel barriers. Numerous STS dI/dV spectra were taken over random positions on the sample surface separated by at least 100 nm and the frequency of the BD events for each type of tunnel barrier is shown in
Conclusions
In conclusion, exposure of the Al surface to trace oxygen or H2O led to a distorted Al surface and IL formation. By reducing the time the sample spent pre-heating for ALD at elevated temperatures, the extent of IL formation was reduced. This IL reduced the Al2O3 density during the first ALD cycle, or atomic-layer. This reduced Al2O3 density led to a lower tunnel barrier height and increased the disorder within the atomically-thin film. This defective interface also led to a slight reduction in the tunnel barrier quality as the film thickness was increased into the ultrathin thickness regime of 0.5-2 nm. Remarkably, ALD sample “without an IL” had consistent STS spectra and Eb even as the thickness was pushed down to the atomically-thin limit of 1 ALD cycle. This Eb consistency with thickness confirms that no significant IL is present and shows that an MIMTJ with a high-quality, atomically thin ALD Al2O3 tunnel barrier is possible. However, some disorder may remain at the Al—Al2O3 interface or within the ALD Al2O3 tunnel barrier. This disorder is evident by the number and severity of soft breakdown events observed in the 1 cycle ALD Al2O3 films “without an IL”. This disorder may have been caused by either H2O dissociation into 0 and H during the first ALD H2O pulse or may be disorder within the ALD Al2O3 film itself. In either case, this disorder was very minor and did not measurably impair the tunneling properties such as Eb.
Introduction
Magnetic Tunnel Junction (MTJs) are the building blocks for non-volatile magnetoresistive random access memory (MRAM) and are created by sandwiching an ultrathin insulator between two ferromagnetic layers1-4. MRAM has significant performance and power consumption advantages over standard dynamic random access memory or flash memory with fast read, write times and a memory state which is retained without power draw2, 4, 5. MTJs operate with a differing spin-polarized electron tunneling resistance for parallel and antiparallel magnetization of the ferromagnetic layers. This Tunneling Magneto Resistance (TMR) is critical to MTJ device performance and is particularly sensitive to the quality and thickness of the insulating layer. High TMR values are desirable for greater signal to noise ratio, lower power consumption, higher speed, and large design margin for device fabrication6. Current state of the art MTJs have TMR values of 10-70% for AlOx tunnel barriers7, 8 and at least a factor of three higher for crystalline MgO tunnel barriers5, 9, 10.
The recent progress in MTJs fabrication using ALD insulators uses ex situ deposition of 2-5 nm thick ALD tunnel barriers in order to reduce the leakage current which indeed decrease the spin tunneling11-14. The transport measurements for epitaxial MgO show barrier heights in the range of 0.4-0.9 eV5, 15, 16 due to the presence of oxygen vacancy defects in MgO. This reported barrier height for epitaxial MgO is much lower compared to ultrathin ALD Al2O3 tunnel barrier height ˜1.5 eV17, 18. The low barrier height on MgO and larger tunnel barrier thickness, indicates a poor quality tunnel barrier with a high density of defects.
While MTJs with MgO tunnel barriers have excellent TMR values, they require a complex sample fabrication process which is incompatible with many industry thermal budgets and results in poor uniformity across the wafer20-24. The AlOx tunnel barriers fabricated using thermal or plasma assisted aluminum oxidation are significantly more compatible with industry applications, however defects within tunnel barrier and poor interface between metal-insulator results in an asymmetric structure. The electronic states tunneling through amorphous AlOx cannot preserve their symmetry due to coupling with the evanescent states in the tunnel barrier resulting in incoherent tunneling which significantly reduces the spin tunneling current1. As a figure of merit for MTJs, high TMR exceeding 100% is desirable for many practical applications of spintronic devices. The quality of the tunnel barrier may also be characterized using scanning tunneling spectroscopy (STS) and dI/dV curves to find the barrier height, which for thermal AlOx tunnel barriers is 0.82-1.20 eV at room temperature25. From these tunneling spectroscopy studies, it has been concluded that low-energy extended electron states in the very thin and disordered oxide layer causes a reduction in TMR26.
In this Example, the in situ ALD Al2O3 process described in Examples 1 and 2 is adapted for MTJ devices by fabricating Fe/Al—Al2O3 bilayer structures with varying Al and Al2O3 thicknesses. In situ STS was used to examine the electron tunneling through the Al2O3 to quantify its quality as the Al layer was systematically reduced to determine if a defective interfacial layer (IL) formed. In tandem, ab initio Molecular Dynamics (AIMD) simulations were run to examine adapting the pre-ALD H2O pulse to produce OH groups directly on the Fe polycrystalline surface.
Methods
To create the metal-insulator structure for in situ STS, a trilayer of Nb (50 nm)/Fe (20 nm)/Al (x nm) was DC magnetron sputtered onto a Si/Au (50 nm) substrate at a deposition rate of 1.0 nm/s, 1.7 nm/s, and 0.5 nm/s. The Al thickness was varied in the range of 0-7 nm. After sputtering, the samples were transferred in situ to the ALD chamber under high vacuum where a pre-ALD H2O pulse hydroxylated the surface and a layer of Al2O3 was grown using the optimized ALD conditions discussed in Example 2, above. After ALD, the samples were in situ transferred under high vacuum to the STS chamber which had a pressure of about 1×10−9 Torr. dI/dV spectra were taken over 100-200 random locations on the sample's surface using a mechanically-cleaved Pt—Ir tip with a voltage modulation of 30 mV at 5 kHz and a set point of 2 V, 200 pA. The tunnel barrier height was estimated by the intersection of two bisquare-method linear fits to ln(dI/dV) and the ALD coverage was defined as the percentage of locations which had dI/dV spectra consistent with ALD Al2O3 using the methods described in Examples 1 and 2, above. AIMD simulations for H2O molecules on the Fe (100), Fe (110), and Fe (111) surface were run under a constant volume and temperature ensemble as implemented in VASP code30. The Fe slabs were constructed using experimentally determined lattice parameters31 and were adjusted in size to accommodate thermal expansion. A “water pool” was added to the top site of each Fe surface to simulate the pre-ALD H2O pulse. Additional details for the simulation procedure can be found in Examples 1 and 2, above.
Results and Discussion
Spin-polarized electron scattering in the ALD Al2O3 MTJ will be strongly dependent on the aluminum thickness. Therefore, the first step towards adapting this in situ ALD Al2O3 process for MTJ devices is to reduce the thickness of the Al layer on Fe and to examine the resulting ALD Al2O3 quality. As shown in
To eliminate the possibility that this Eb reduction is due to the development of an FeOx IL, the ALD cycle number was varied with the Al thickness held constant at 1 nm. The resulting Eb and ALD coverage is shown in
This rough surface may be due to the formation of an Al—Fe intermetallic layer. AIMD simulations have shown that the thickness of the Al—Fe intermetallic layer depends strongly on the Fe orientation; Fe(111) being the most severe with an intermetallic layer thickness of around 0.5 nm32. However, these simulations were run at room temperature for simulated e-beam evaporation. Aluminum deposited by magnetron sputtering will have additional kinetic energy which may extend this intermetallic layer thickness into the 1 nm range. This Al—Fe intermetallic may significantly increase the surface roughness. Overall though, while some ALD Al2O3 quality was lost going from 7 nm to 1 nm Al on Fe, the resulting ALD Al2O3 tunnel barrier is still of excellent quality and is quite promising for MTJ devices.
What is particularly interesting about the results of
To examine what degree IL formation occurs when in situ ALD Al2O3 is grown on Fe, ALD Al2O3 films were grown on Fe with varying cycle numbers. As shown in
Up to this point, the previously optimized ALD growth conditions (H2O pulse length and heating time (which affects pulse temperature)) for growing ALD on Fe have been used. Therefore, heating times were adjusted to determine the effect on ALD growth on Fe. Using the heating curve found empirically in Example 2, above, and the initial temperature (of the sample prior to heating) and heating power used for previous samples, three samples were fabricated and analyzed with different heating times.
Each sample was fabricated with the same makeup as the previous samples (i.e. Nb/Fe/1 cycle of ALD); the three heating times chosen were 13, 15, and 17 minutes with pulse temperatures of 175, 189, and 200° C. respectively. As shown in
Finally, TMR measurements on the Fe/ALD-Al2O3/Fe MJTs are shown in
Conclusions
In conclusion, this Example reports the first success in growth of atomically thin (0.12-0.6 nm in thickness), low-defect Al2O3 tunnel barriers through atomic layer deposition directly on ferromagnetic Fe electrode. In situ STS studies reveal high tunnel barrier height up to 1.25 eV can be obtained on 0.12 nm thick ALD Al2O3 tunnel barriers directly on ferromagnetic Fe electrodes. This value is more than twice of that of the thermal AlOx tunnel barriers. This indicates a significantly lower defect concentration can be obtained in the ALD grown tunnel barriers, in addition to an order of magnitude reduction in the tunnel barrier thickness. Although an Al wetting layer may provide a slightly better nucleation surface for the ALD Al2O3 tunnel barriers as reflected in up to ˜15% improvement in the tunnel barrier height, it has been found that the wetting layer is not necessary. This observation is supported by the density function simulation of the hydroxylation of Fe with a H2O pulse before ALD Al2O3 tunnel barrier growth proceeds. Therefore, this work removes a fundamental roadblock towards achieving MTJs with atomically thin, defect-free dielectric tunnel barriers.
This Example shows that high quality Al2O3 tunnel barriers may be formed using the present methods even on rough surfaces, such as surfaces which exhibit a roughness similar to that of pre-processed circuits.
To create structures on the substrate and simulate surface non-uniformity/roughness, e.g., from additional layers of devices stacked on one another, Nb (˜150 nm) was DC magnetron sputtered onto a Si wafer and then etched into a pattern using reactive ion etching (RIE). Afterwards an insulating spacer layer of SiO2 (˜200 nm) was deposited followed by a layer of Au (˜50 nm), both via electron beam. This Au layer serves as an electrical contact for mounting the sample on the STM stage so that the sample can be held at various bias voltages. To monitor how the RMS roughness (i.e. the standard deviation of the surface height) changed as more layers were added on, the samples were analyzed using a Witech Alpha300 atomic force microscope (AFM) system. These AFM scans were done under contact mode over a 5×5 μm2 area on top of the Nb structure.
Once this substrate was prepared, it was placed in the in situ ALD deposition and sputtering system using in the Examples, above. First, Nb (˜50 nm) was deposited, followed by a deposition of Fe (˜20 nm) to simulate the bottom half of an MTJ. Wetting layers of Al, having thicknesses from 0 nm to 7 nm were used. Then the sample was transferred in situ to the ALD chamber, where it was heated via blackbody radiation from the chamber walls (which were heated via thermal wraps external to the chamber) for ˜15 minutes. Once the sample had reached ˜190° C. a pulse of deionized water was let into the chamber, followed by a vacuum purge cycle, then a pulse of trimethylaluminum (TMA) entered the chamber, again followed by a vacuum purge.
As discussed above, pulsing a small amount of deionized water onto the surface at these temperatures saturates the sample surface with OH groups needed for the TMA to bond to the surface. As the TMA interacts with the surface, it consumes nearly all the adsorbed OH forming amorphous Al2O3. When this process occurs one time it is referred to as one ALD cycle and produces ˜1.1-1.2 Å/cycle. This ALD process is self-limiting since once the adsorbed OH has been exhausted no further Al2O3 is able to form.
Lastly, the sample was transferred from the ALD chamber to the sputtering chamber where it was allowed to cool before it was transferred into the UHV STM chamber for analysis. Using a RHK UHV350 system and a camera to assure that the tip approached the area on the substrate where the Nb structures were located; STM dI/dV spectroscopy was carried out on the structured areas of the sample. dI/dV spectrum data was analyzed as described above. Through collecting multiple spectra (˜100 at different locations on the Nb structure) the average barrier height and the ALD coverage were calculated.
Results
To get a sense of what condition the surface was in before fabricating the MI layer, the roughness was measured before and after the deposition of the spacer layer (data not shown). Roughness measurements for the Nb structure produced an RMS roughness of (˜1.6 nm while the same measurement after depositing the spacer SiO2/Au layer resulted in a roughness of ˜2.3 nm, meaning that some small amount of roughness is introduced during deposition of this spacer layer. In an industry setting, this added roughness could be reduced through mechanical polishing or similar techniques. Lastly, the photoresist used to define the Nb structures could not be removed from one of the samples due to a processing error. This sample was used as a worst-case scenario for surface roughness, providing an extreme value of ˜15.1 nm. By fabricating an MI layer on this surface, ALD-growth on an extremely rough surface could be investigated.
dI/dV spectra were taken over a region having many winding pieces so as to more accurately represent an integrated circuit having a high density of features. As a baseline of comparison, previous STM data measured from a sample made up of Nb/Fe/Al (7 nm)/Al2O3 (1 cycle) was used which had been fabricated on a flat Si substrate. This control sample represents the optimal conditions of tunnel barrier layer fabrication. A representative spectrum of the control sample is shown in the top panel of
Although the tunnel barrier quality does decrease for rougher surfaces (most likely due to the introduction of defects caused by the roughened surface which affects OH nucleation and therefore Al2O3 nucleation), it is remarkable that even on rough surfaces, high quality Al2O3 barriers may be formed using the present methods.
The word “illustrative” is used herein to mean serving as an example, instance, or illustration. Any aspect or design described herein as “illustrative” is not necessarily to be construed as preferred or advantageous over other aspects or designs. Further, for the purposes of this disclosure and unless otherwise specified, “a” or “an” means “one or more”.
The foregoing description of illustrative embodiments of the invention has been presented for purposes of illustration and of description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed, and modifications and variations are possible in light of the above teachings or may be acquired from practice of the invention. The embodiments were chosen and described in order to explain the principles of the invention and as practical applications of the invention to enable one skilled in the art to utilize the invention in various embodiments and with various modifications as suited to the particular use contemplated. It is intended that the scope of the invention be defined by the claims appended hereto and their equivalents.
The present application claims priority to U.S. Provisional Patent Application No. 62/530,555 that was filed Jul. 10, 2017, the entire contents of which are hereby incorporated by reference.
This invention was made with government support under DMR1337737 and DMR1508494 awarded by the National Science Foundation and under W911NF-16-1-0029 awarded by the Army Research Office. The government has certain rights in the invention.
Number | Date | Country | |
---|---|---|---|
62530555 | Jul 2017 | US |