Abstract
The invention relates to a catalyst composition comprising anionic clay, lanthanum (hydr)oxide carbonate, and cerium oxide. This composition can suitably be used in FCC for the reduction of NOx and/or SOx emissions, the reduction of the S and/or N-content in fuels, and as a metal trap. The composition can be prepared by forming a precipitate from a solution comprising a divalent metal salt, a trivalent metal salt, a lanthanum salt, and a cerium salt, calcining the precipitate at 200-800° C., and rehydrating the calcined precipitate in the presence of a carbonate source to form a composition comprising anionic clay, lanthanum (hydr)oxide carbonate, and cerium oxide.
Description

FIGURES


FIG. 1 presents a Powder X-ray Diffraction Pattern (using Cu K-alpha radiation) of a composition comprising a Mg—Al anionic clay and a lanthanum (hydr)oxide carbonate.



FIG. 2 presents a Powder X-ray Diffraction Pattem (using Cu K-alpha radiation) of a composition comprising a Mg—Al anionic clay, lanthanum (hydr)oxide carbonate, and cerium oxide.





EXAMPLES
Comparative Example 1

An aqueous solution comprising Mg(NO3)2, Al(NO3)3, and La(N03)3 with an Mg/Al molar ratio of 3 and a La-content of 30 wt % (calculated as La2O3 and based on the total weight of the resulting catalyst composition calculated as oxides) was prepared. The pH of the solution was adjusted to 10 using NaOH, thereby forming a precipitate.


The precipitate was filtered, washed, and dried, and subsequently calcined at 350° C. for four hours. The calcined product was then rehydrated in an aqueous solution containing 1 M Na2CO3 at 85° C. overnight.


The resulting product was isolated. Its Powder X-Ray Diffraction (PXRD) pattern is shown in FIG. 1. The reflections at 11.4 and 22.9° 2-theta (d=7.76 and 3.88 Å) indicate the presence of anionic clay; the reflections at 15.7, 20.4, 23.8, and 30.2° 2-theta (d=5.65, 4.35, 3.73, and 2.96) indicate the presence of lanthanum hydroxide carbonate.


Example 2

Comparative Example 1 was repeated, except that instead of 30 wt % La, the solution contained 15 wt % La and 15 wt % Ce (calculated as La2O3 and CeO2, respectively, and based on the total weight of the resulting catalyst composition calculated as oxides).


The PXRD pattern of the resulting composition is shown in FIG. 2. The reflections at about 11.4 and 23° 2-theta indicate the presence of anionic clay; the small reflections at about 16, 20.3, 23.8, and 30.2° 2-theta indicate the presence of lanthanum hydroxide carbonate; the broad reflection at about 29° 2-theta indicates the presence of CeO2.


Example 3

The products of Comparative Example 1 and Examples 2 were tested for their de-SOx ability in FCC processes using the thermographimetric test described in Ind. Eng. Chem. Res. Vol. 27 (1988) pp. 1356-1360. A standard commercial de-SOx additive was used as a reference.


Either 17.3 or 27.3 mg (see Table below) of the samples were heated under nitrogen at 700° C. for 30 minutes. Next, the nitrogen was replaced by a gas containing 0.32% SO2, 2.0% O2, and balance N2 with a flow rate of 200 ml/min. After 30 minutes the S02-containing gas was replaced by nitrogen and the temperature was reduced to 650° C. After 15 minutes, nitrogen was replaced by pure H2 and this condition was maintained for 20 minutes. This cycle was repeated 3 times. The sample's SOx uptake and its release during hydrogen treatment were measured as the sample's weight change (in %).


The SOx uptake and release during the third cycle are shown in Table I. This Table also displays the effectiveness ratio, which is defined as the ratio of SOx release over SOx uptake. The ideal effectiveness ratio is 1, which means that all the SOx that was taken up has been released again, leading to a longer catalyst life.













TABLE I






sample

SOx release




weight
SOx uptake
(% wt
Effectiveness


Sample
(mg)
(% wt increase)
decrease)
ratio



















Comparative
27.3
14
1.3
0.09


Example 1


Example 2
17.3
35
27
0.77


Commercial
17.3
28
2
0.07


additive


Commercial
27.3
17
1.3
0.08


additive









This table shows that the SOx release and, hence, the effectiveness ratio of the composition according to the invention is higher than that of a standard commercial de-SOx additive and of a composition comprising only anionic clay and lanthanum hydroxide carbonate.

Claims
  • 1. Catalyst composition comprising anionic clay, lanthanum (hydr)oxide carbonate, and cerium oxide.
  • 2. Composition according to claim 1 comprising 10-50 wt % lanthanum (hydr)oxide carbonate, 5-20 wt % cerium oxide, and balance anionic clay, all calculated as oxides and based on the total weight of the composition.
  • 3. Composition according to claim 2 wherein the anionic clay is an Mg—Al, Zn—Al, Cu—Al, Mg—Co, and/or Mg—Fe anionic clay
  • 4. Process for the preparation of a catalyst composition according to claim 1, comprising the steps of: forming a precipitate from a solution comprising a divalent metal salt, a trivalent metal salt, a lanthanum salt, and a cerium salt,a. calcining the precipitate at 200-800° C., andb. rehydrating the calcined precipitate in the presence of a carbonate source to form a composition comprising anionic clay, lanthanum (hydr)oxide carbonate, and cerium oxide.
  • 5. Use of the catalyst composition according to claim 1 in an FCC process.
  • 6. Use according to claim 5 for the reduction of NOx and/or SOx emissions.
  • 7. Use according to claim 5 for the reduction of the S and/or N-content in fuels.
  • 8. Use according to claim 5 for the passivation of Ni and V.
Priority Claims (1)
Number Date Country Kind
04075064.8 Jan 2004 EP regional
PCT Information
Filing Document Filing Date Country Kind 371c Date
PCT/EP04/13914 12/6/2004 WO 00 7/5/2007
Provisional Applications (1)
Number Date Country
60527758 Dec 2003 US