This invention pertains generally to utilizing a micro tool probe to characterize micro surface areas of an object. More particularly, the invention pertains to a probe Nano-indenter, Scanning Probe Microscopy (SPM), Atomic Force Microscopy (AFM), Scanning Electron Microscopy (SEM), Transmission Electron Microscopy (TEM), combinations thereof, or other similar tools having a probe tip. The method in accordance with the present invention creates a rendering (an image or transform) derived from an association of signals (acoustic or ultrasonic) to surface contact of the probe tip. Further, in accordance with the invention a user may classify the renderings dependent upon prior load-unload (LUL) curve mapping and other a-priori knowledge, all while machine/deep learning is employed in an unsupervised mode for sorting out characteristic joint time frequency domain signatures derived from the signal. Prior unknown or unclassified renderings can be added by the operator to the quantified data base dependent upon statistical significance and newly generated knowledge.
Prior micro tools have determined certain characteristics of a material, however the prior known tools include limitations that are overcome by the present invention. For example, quantitative nano scale characterization devices such as nanoindenters and use of Atomic Force Microscopes (AFM) are very effective at rendering general material properties of a sample, such as elasticity modulus or sample hardness, or derive elastic contact properties of a sample, however these tools are limited to quasi-static or low frequency dynamic response. Subtle nanoscale volumetric changes occur during a materials' phase transformation, the plasticity induced yield stress onset, twining, thin film fracture modes that are not affectively characterized by current nano scale characterization devices. Also probe contact of these areas typically generates high frequency elastic and surface acoustic waves generally called by Acoustic Emissions (AE). In addition, monitoring the dynamics of multi-cycling loads at nanoscale provide a user with the knowledge of the critical fatigue cycles which is a very important parameter in describing reliability of thin film interfaces. The faster test can be achieved by a higher multi-cycle loading frequency. Thus, hundreds of kHz or even a MHz multi-cycling shorten nano fatigue tests to minutes and seconds instead of hours. It would be desirably to provide a micro tool capable of identifying micro locations on the sample where these changes (including nano fatigue induced changes) occur and provide reliable material characterizations at the identified locations.
Passive acoustic wave monitoring in polycrystalline metallic materials has been utilized as a non-destructive defect detection tool. From the instrumentation/metrology perspective, the idea behind simultaneous acoustic emission monitoring and quasi-static nanomechanical testing is to perform complementing measurements at two or more well-spaced frequency ranges simultaneously. In contrast to dynamic nanoindentation applications, instrument structural modes and acoustic emission monitoring ranges are separated by several orders of magnitude which allow simultaneous quasi-static and acoustic monitoring without any modal interference. Modal interferences may occur at conditions when the nanomechanical test instrument is being operated at frequencies above the rigid body mode frequency, where higher modes are being excited. This phenomenon complicates the interpretation of results requiring complex identification in order to separate the instrument's and materials' responses. Typical rigid body modes for nanoindenters are between 10 and 300 Hz. Recent commercially available MEMS based nanoindenters extend that range to several kHz. On the other hand, a typical acoustic emission monitoring range is 50 kHz-2 MHz.
Simultaneous nanoindentation and AE monitoring systems have been used in an attempt to correlate quantitative acoustic wave properties with local contact materials phenomena such as the plasticity yield point initiation for W (100). Although attempts were made to identify correlations between load-unload curves and integrated AE waveforms, the nanoindentation load-unload curves did not reveal any artifacts or excursions even though AE events were observed from phase transformation. The complexity of the contact phenomena renders difficulty to use a single number or waveform integrated energy characterizing event to correlate or “fingerprint” the contact phenomena. Several attempts have been made to look at the characteristic acoustical signatures via signal decomposition techniques: such as, Short Time Fourier Transforms (STFT), wavelets or CWT coefficients. However, the prior acoustic signature recognition concepts lacked a systematic framework capable of classifying and predicting the outcome. The present invention is able to utilize AE events to “fingerprint” the contact phenomena. Similar to the passively acquired Acoustic Emission, the present invention is also able to utilize reflected ultrasonic signals taken during nano fatigue monitoring to provide a fingerprint and classify the contact phenomena with the inventions robust deep learning methodology.
Embodiments according to aspects of the invention include a method and device to characterize nanoindentation/scratch induced acoustic signal events or ultrasonic wave propagation induced signals (ultrasonic signals) using an ultrasonic nanoindentation tip running in the passive mode associated with acoustic events and running in an active mode associated with nanofatigue test. The acoustic events are detected in combination with an Acoustic Emission sensor. The ultrasonic tip acquires signals associated with the nanoindentation/scratch and ultrasonically induced nanofatigue tests. The method consists of JTF domain signal transform, signal entropy filtering, and Machine/Deep learning implemented into control software/hardware that is synchronized with signal data acquisition and nanoindentation hardware. The hardware is comprised of an ultrasonic tip/Acoustic Emission sensor, fast DAC/ADC board, signal conditioner, and nanomechanical test instrument. During nanofatigue testing the nanoindentation tip actively oscillates at a chosen resonant frequency and is capable of acquiring signals within 20 kHz-4 MHz bandwidth. The synergy of Machine/Deep Learning together with JTF domain signal processing and monitoring hardware renders possible a correlation and characterization of the micro areas on a surface.
In accordance with aspects of the invention, deep learning is utilized for the characterization of acoustic and nanofatigue events. The overall objective is to utilize deep learning neural network classification for typical nanoindentation induced small data sets of several hundred events (either acoustic emission (AE) events or nanofatigue events). The combination of Continuous Wavelet Transforms (CWT) based signal decomposition and entropy minimization based filtering creates topographic scattergram of the events. The image recognition neural network trains on those scattergrams according to specified classifications. This creates signature maps that can be associated with nanoindentation induced specific materials phenomena which are then used in the classification/characterization of unidentified events.
A combination micro tool probe tip and ultrasonic transducer capable of transmitting longitudinal resonant high frequency ultrasonic waves is utilized to obtain signals associated with acoustic emission events correlated with probe tip contacts of a multilayered sample. Alternatively, the probe tip is utilized to obtain ultrasonic signals corresponding with nanofatigue events. A preferred resolution may be obtained by changing different longitudinal vibrations and torsional oscillation modes of the multi-mode ultrasonic transducer in contact with the sample. The obtained acoustic output signal represents acoustic impedance of the sample which is a function of the material properties.
Also described herein is an ultrasonic tip system for metrology and 2D topology type tools. The ultrasonic tip system includes a probe tip, a comparator, a wave guide, and an energy source. The probe tip includes an ultrasonic transducer/receiver that may direct ultrasonic waves towards a sample and an elongated wave guide coupled to the ultrasonic transducer, wherein the wave guide may vibrate longitudinally and oscillates rotationally dependent upon a frequency of the ultrasonic waves from the ultrasonic transducer. This type of ultrasonic tip system attached to a nanoindenter shaft is illustrated in
Embodiments according to aspects of the invention also include a method of characterizing micro regions of a surface of an object. The method may include calibrating a metrology or topology micro tool probe. When calibrating, the control of the ultrasonic probe tip is adjusted so that waves propagate through the elongated column at a resonant frequency with a range of frequencies between 100 kHz to 2 MHz. During calibration the boundary conditions for the resonant frequency may be determined. Once calibrated, the micro tool is controlled to contact a micro region of a surface of an object utilizing the micro tool probe. Acoustic emission event signals or ultrasonic signals are acquired that are associated with contact between the probe tip and the surface of the object. The micro tool system correlates acoustic emission event signals or ultrasonic signals with data points on a load unload curve. Images or renderings are created that represent correlated acoustic emission event signals or ultrasonic event signals respectively with LUL events. These images or renderings are compared with images or rederings having known material characteristics to thereafter characterize the associated micro region of the surface of the object.
The method in accordance with aspects of the invention may further comprise decomposing the acquired acoustic emission event signal or ultrasonic signal and representing the signal in a joint time-frequency domain. The joint time frequency domain includes at least one of continuous wavelet transforms, matching pursuit, Wigner-Ville, curvelets, ridgelets, and shearlets. Also, the joint time frequency domain may consist of deterministic, stochastic and harmonic components. Further, characterizing the micro region of the surface of the object may include the use of convolutive neural networks (CNN) or long-short term memory (LSTM) networks.
The micro tool probe of the present invention is particularly well suited for use with a micro tool probe tip of a metrology or topology tool that includes a casing having an enclosed bottom and top, a probe tip holder having an end extending out of the bottom of the casing, a probe tip coupled to the probe tip holder, a support ring engaged with the probe tip holder to support the probe tip holder above the bottom of the casing, a micro actuator engaged to the support ring, an acoustic sensor contained by the casing and engaged to the support ring, a signal conditioner and JTF domain transforms, and an image generator. The micro actuator includes a first planar spring, a second planar spring, and a spacer sandwiched between the first planar spring and the second planar spring. The micro tool probe may include an acoustic sensor that is capable of acquiring acoustic emission event signals within a 20 kHz-4 MHz bandwidth.
Embodiments according to aspects of the invention may further include a signal conditioner coupled to the acoustic sensor. Also, the first and second planar springs are constructed of a shape memory alloy. The first and second planar springs may include a thin film piezo layer deposited on planar surfaces of the first and second planar springs. Actuation of the first and second planar springs is accomplished by applying an electrical voltage potential to the first and second planar springs. In accordance with aspects of the invention, the probe tip may include the acoustic sensor oriented above, below, or integrated with the probe tip. Also, the micro actuator may provide quasi-static load on contact between the probe tip and an object.
The accompanying drawings, which are incorporated in and constitute a portion of this specification, illustrate embodiments of the invention and, together with the detailed description, serve to further explain the invention. The embodiments illustrated herein are presently preferred; however, it should be understood, that the invention is not limited to the precise arrangements and instrumentalities shown. For a fuller understanding of the nature and advantages of the invention, reference should be made to the detailed description in conjunction with the accompanying drawings.
In the various figures, which are not necessarily drawn to scale, like numerals throughout the figures identify substantially similar components.
The following description provides detail of various embodiments of the invention, one or more examples of which are set forth below. Each of these embodiments are provided by way of explanation of the invention, and not intended to be a limitation of the invention. Further, those skilled in the art will appreciate that various modifications and variations may be made in the present invention without departing from the scope or spirit of the invention. By way of example, those skilled in the art will recognize that features illustrated or described as part of one embodiment, may be used in another embodiment to yield a still further embodiment. Thus, it is intended that the present invention also cover such modifications and variations that come within the scope of the appended claims and their equivalents.
The methodology related to nanoindentation induced AE signal characterization includes advanced signal processing such as wavelets, entropy minimization, and machine/deep learning deployment. Due to the complex structure consisting of multiple deterministic and stochastic components, passively monitored acoustic signals have to be analyzed/decomposed using techniques that have stochastic and deterministic base functions. Discrete Wavelet Transformation (DWT) and Continuous Wavelet Transformations (CWT) are utilized in describing very complex acoustic and biological systems signals. Even though DWT are computationally efficient, the CWT are preferred to provide “smooth” boundary transitions that are critical for converting Joint Time-Frequency (JTF) scattergram into a Deep Learning CNN acceptable graphic format. A Gabor's wavelet, used in generating AE signal scattergram, is constructed with a two-dimensional Gaussian window g(x,y) multiplied by sinusoidal waves propagating along K orientations {ak} 1≤k≤K as follows:
ϕK (x, y)=g(x, y) exp[−iη (x cos(αk)+y sin (αk))]
The Gabor's wavelet is complex. Other transforms that can be utilized in building JTF domain scattergrams are Wigner-Ville, matching pursuit, curvelets, ridgelets, or shearlets. CWT coefficient filtering can be accomplished by Shannon's entropy minimization; in the case of Gabor's wavelet, it can be expressed in the form:
min(E(ϕ)=ΣKϕk ln (ϕk))
The entropy minimization for CWT coefficient sorting/filtering is implemented in sequential steps. The resulting scattergram is converted into a specified size jpeg image (e.g., 224×224×3). A simple neural network can be expressed by a multi-layer perceptron. The multi-layer perceptron λ makes predictions {tilde over (y)}n of the target yn via a function {tilde over (y)}n (xn,W) where the vector W represents all parameters of the network. Given a data set {(xn,yn)}, the overall goal is to learn the parameters W to minimize the objective:
The regularization term ψ(W) can represent L1 or L2 norm penalties or tree regularization. A large network of multi-layered perceptrons set to achieve specialized classification tasks in unsupervised learning environment constitutes a deep learning neural network. Image recognition deep learning neural networks such as GoogLeNet, AlexNet, Caffe may be utilized for the deep learning system.
By way of example, and without limitation intended, a GoogLeNet deep learning convolutive neural network (CNN) may be utilized having 144 layers that are optimized for generic image classification/recognition and operates on 224×224×3 sized jpeg images. This deep learning network provides performance/availability criteria and may be deployed for classification of nanoindentation induced acoustic events. Mathematical formula and spreadsheet manipulation software installed on a personal computer having an operating system that executes GPUs may be used to assist the learning process. The neural network settings may include the Stochastic Gradient Descent with Momentum optimizer, the learning rate of 0.0003 per epoch, and a mini batch of 10 observations per each iteration. The GoogLeNet may be trained on predefined classifiers and then deployed on the unidentified acoustic signal data sets. Training and test data may be split at a ratio of 70/30 and then randomized for each separate run.
The next step 50 converts JTF scattergrams into acceptable graphical format images to prepare data for the dedicated ML/Deep Learning characterization step. The ML/Deep learning creation/selection step 54 performs image recognition of recorded AE signatures and classifies them according to the classifications established by the operator. Here, unknown signatures undergo the operator's review on whether to be added into a new category.
The setting of the ML/DL parameters step 60 involves choosing a number of images to train, set the learning rate, set the number of epochs and iterations, and to choose the optimization algorithm for training. The typical dynamics of the Deep Learning process conducted on several hundred passive acoustic image is shown in
The nanomechanical test instrument 100 with in-situ AE monitoring capability is depicted schematically in
The passive acoustic monitoring system consists of the ultrasonic nanoindentation tip 110, signal conditioner 160 and fast ADC/DAC 172 which is synchronized with the nanoindenter controller 162. The ultrasonic nanoindentation tip 110 registers AE events during nanoindentation. During testing, it is operated in the passive pickup mode while an active mode is used for initial calibration. The signal conditioner amplifies the AE signal by ˜80 dB and has 100 kHz to 2 MHz bandpass filter. Data is acquired by the fast ADC/DAC 172 which has an 8 MHz sampling rate and 16-bit resolution.
Typical nanoindentation load-unload curves on W (100) with correlated AE events is shown in
The “W100” and “W100 ch” events located below the yield point were likely due to dislocation nucleation and/or oxide fracture. Also, “W100” and “W100 ch” events found at the end of unloading segment were potentially due to the tip pull-off. There is no explanation on the nature of “W100” and “W100 ch” AE events found on the unload segment between loads of 750 μN and 45 μN. In addition, 150 nm thick GaAr coated Si wafer samples were used to generate AE signatures on a different than W (100) material for comparison purposes and were labeled by “GalAr”. A total of 245 AE signals were obtained during 50 AE monitored nanoindentation tests. A diamond 40 nm radius cube corner tip was used. All four types of typical AE signals are plotted in
Turning attention now to
The probe holder 200 includes shaft 228 with an integrated voice coil that is mounted on two sets of flat springs ensuring low stiffness of ˜100 N/m. The upper spring 226 is secured with the ring 224. A center capacitance plate 234 is mounted on the shaft 228 and secured with rings 232 and 238. The lower spring 222 is mounted on the shaft 228 and is secured by the ring 214 and spacers 248, 220. The ultrasonic tip 210 is mounted onto the end of the shaft 228. The voice coil with shaft 228 is driven by the permanent magnet assembly 230 where outer diameter of the top flat spring 226 rests on. The spring 226 is secured by the spacer 224. The outer top capacitive electrode 240 is resting on the spacer 224 and is supported by the spacer 242. The bottom capacitive electrode 244 is resting on the spacer 242 and is supported by the spacer 248. The bottom flat spring 222 is resting on the spacer 248 and is secured by the spacer 220. The assembly is mounted inside of the cylindrical frame 218 and secured by the bottom plate 216. It is all secured from the top by the dedicated cover plate 236. The spacer 242 ensures the spacing/gap needed by the center 234, top 240, and the bottom 244 capacitance plates to perform differential measurement. The differential capacitance measurement can be formalized by the following expression:
Here, the output current lout is measured on the differential capacitance channels of C1 and C2. A is a capacitive electrode area, x—is the moving distance of the shaft, and d is the fixed distance between plates.
The nanomechanical test instrument 600 with active nanofatigue monitoring capability is depicted schematically in
The active ultrasonic waveform monitoring system consists of the ultrasonic nanoindentation tip 610 and fast ADC/DAC 672 which is synchronized with the nanoindenter controller 662. The oscillating ultrasonic nanoindentation tip 610 generates ultrasonic waves and registers returning ultrasonic pulses during the nanoindentation/scratch test. The data is acquired by a fast ADC/DAC which has 4-8 MHz sampling rate and at least 16-bit resolution and 100 kHz to 2 MHz bandpass filter.
The ultrasonic monitoring system consists of the ultrasonic nanoindentation tip 610, and fast ADC/DAC of 672 which is synchronized with the nanoindenter controller 662. The ultrasonic nanoindentation tip 610 generates a few nanometers displacement and registers returning ultrasonic wave signals during nanoindentation. During testing, it is operated in the passive pickup mode while an active mode is used for initial calibration and ultrasonic wave generation.
The differential capacitance measurement can be formalized by the following expression:
Here, the output current Iout is measured on the differential capacitance channels of C1 and C2. A is a capacitive electrode area, x—is the moving distance of the shaft, and d is the fixed distance between plates.
The ultrasonic nanoindentation tip 610 is used in the synchronized active ultrasonic monitoring. In the active ultrasonic mode piezoelectric elements operate on a combination of direct and inverse piezo effect where one of the elements is driven by the resonance frequency voltage input 662. The other element acts as an ultrasonic wave signal pickup 664 collecting ultrasonic wave energy transmitted via shaft and diamond tip. Having both piezoactive and passive elements available, the ultrasonic nanoindentation tip can be calibrated.
Two well-accepted theoretical models can be considered in deriving relationship between a number of nanofatigue cycles and mechanical characteristics such as film toughness KIC, elastic modulus E and contact geometry [1, 2, 3, 9, 10]. The reversed-cycling approach is applicable for a rather low number of fatigue cycles NR and can be expressed as:
Where α1˜1 is an arbitrary constant. The εf is a monotonic true effective fracture strain which can be expressed in terms of spherical contact fracture mechanics as follows:
Here, σYS is the yield stress and r is the distance from the natural plastic flaw where the fracture strain is exceeded. At the fracture strain of ε=εf, the stress intensity is equivalent to the film fracture toughness KI=KIC, and E is modulus dominated by the substrate. Following the concept of geometrically necessary dislocations the plastic strain for a spherical contact εaP can be expressed as:
Here, a, R and δ are the contact geometry parameters, i.e., spherical contact radius, radius of the tip and displacement into the surface, respectively. Thus, Eq. 2 for the reversed-cycling failure cycles can be rewritten as:
In this case the only unknown is r. Considering this to be a fraction Y of the slip band IS piled-up at the film which produces a light wear process induced by the increase in friction. Therefore, KIC is achieved at r˜γ IS by the following number of fatigue cycles:
Ratcheting or Manson-Coffin fatigue applied to the single contact would take fewer cycles to produce failure where number of failure cycles NMC can be expressed as:
Where α2˜1 is an arbitrary constant. In the case of a single point
contact it leads to the light wear under ratcheting boundaries where failure cycles can be expressed as follows:
The above equations are used to relate nanoscale spherical contact geometry, material properties, fracture toughness and anticipated nanofatigue cycles.
With reference to
Operation of nanoindentation/scratch induced ultrasonic monitoring system with Machine/Deep Learning classification capability 500 is shown in
Once the system is setup, the tool may be controlled 530 so that the probe tip of the tool approaches the surface of an object. The surface approach step 30 involves finding the distance between the diamond stylus tip and the surface, then shifting the position laterally by a small amount. The ultrasonic nanoindentation tip frequency response is tested at this point.
The next step 534 is an actual nanoindent/scratch test that starts at the fresh surface location while monitoring ultrasonic signals. The objective of this step is finding the appropriate quasistatic load and ultrasonic excitation amplitude for reliable nanofatigue experiment on a given thin film.
Once all quasistatic and ultrasonic parameters are established the independent data collection begins 540.
The next step 542 associates the recorded ultrasonic signals with locations on the LUL time-domain curve. This is a necessary step performed by the operator to classify events. In the case of nanoindentation and depending on the sample, ultrasonically induced film interface failure, contact adhesion, different modes of fracture/failure and resulting film delamination behavior can be classified. A typical nanoindentation LUL time-domain curve obtained by ultrasonically excited indentation into a thin film is shown in
According to previously conducted studies, an ultrasonic signal recorded as a large excursion may be identified as a nanofatigue phenomenon. Therefore, a number of fatigue failure cycles NU derived from the ultrasonically excited nanoindentation experiments can be obtained from the LUL time-domain curve 710 at the breakthrough location time tB in this form:
NU=tBƒU
Here, tB provided in seconds and ƒU is an ultrasonic cycling frequency superimposed on the quasistatic nanoindentation load. A few nanometer in amplitude ultrasonic oscillations generate resulting ultrasonic signals that are being picked up by the ultrasonic nanoindentation tip.
Stick-slick behavior, brittle, ductile fracture, and thin film breakthrough characteristics can be identified from nanoscratch tests. In addition, a full characterization can involve other methods such as in-situ SPM imaging, FIB SEM cross-section images, and chemical analysis. This step is an operator driven step to establish initial classification of ultrasonic signals.
The JTF domain transform step 546 converts time domain ultrasonic signals into JTF domain spectrograms, see example JTF domain spectrograms at
The ML/Deep learning creation/selection step 54 performs image recognition of recorded AE signatures and classifies them according to the classifications established by the operator. Here, unknown signatures undergo the operator's review on whether to be added into a new category. The setting of the ML/DL parameters step 60 involves choosing a number of images to train, set the learning rate, set the number of epochs and iterations, and to choose the optimization algorithm for training.
The next step 550 converts JTF spectrograms into acceptable graphical format images or representations for Deep Learning, classifies them 554 and prepare data for the dedicated ML/Deep Learning characterization step 564. The ML/Deep learning and characterization steps 564 and 570 start with the parameter settings 560 such as number of iterations, learning rate and optimizing algorithm. The characterization step 570 finalizes as the learning process metrics. Step 570 performs actual image recognition of recorded ultrasonic signal signatures and classifies them according to the classifications established by the operator. Here, unknown signatures undergo the operator's review on whether to be added into a new category.
The training step 564 is completed when accuracy of 100% is reached consistently for several iterations.
In use, the nanomechanical instrument 100 is placed on a high stiffness Z-stage. A sample is positioned laterally by the XY-stage. The ultrasonic nanoindentation tip is used in the synchronized passive acoustic monitoring. In the active mode piezoelectric elements operate on a combination of direct and inverse piezo effect where one of the elements is driven by the resonance frequency input. The other element acts as a signal pickup. In the passive mode, a piezo electric element works as a signal receiver collecting acoustics wave energy transmitted via shaft and diamond tip. Having both active and passive modes available, the ultrasonic nanoindentation tip can be calibrated. In some embodiments the AE sensor may only have a receiver. The nanoindentor tip is particularly useful for nanoindentation induced AE signal characterization or nanofatigue characterization.
These and various other aspects and features of the invention are described with the intent to be illustrative, and not restrictive. This invention has been described herein with detail in order to comply with the patent statutes and to provide those skilled in the art with information needed to apply the novel principles and to construct and use such specialized components as are required. It is to be understood, however, that the invention can be carried out by specifically different constructions, and that various modifications, both as to the construction and operating procedures, can be accomplished without departing from the scope of the invention. Further, in the appended claims, the transitional terms comprising and including are used in the open ended sense in that elements in addition to those enumerated may also be present. Other examples will be apparent to those of skill in the art upon reviewing this document.
This application claims the filing benefit and priority of U.S. Non-Provisional patent application Ser. No. 17/393,462 filed Aug. 4, 2021 the contents of which are incorporated herein by reference in their entireties.
| Number | Name | Date | Kind |
|---|---|---|---|
| 5965896 | Marton | Oct 1999 | A |
| 6945097 | Jardret et al. | Sep 2005 | B2 |
| 7107694 | Yang et al. | Sep 2006 | B2 |
| 7289202 | Groess et al. | Oct 2007 | B2 |
| 7492451 | Vaez-Iravani et al. | Feb 2009 | B2 |
| 7543519 | Chudoba et al. | Jun 2009 | B2 |
| 7624640 | Maris et al. | Dec 2009 | B2 |
| 7649624 | Xin et al. | Jan 2010 | B1 |
| 7814565 | Kim et al. | Oct 2010 | B2 |
| 7845214 | Hsu et al. | Dec 2010 | B2 |
| 7973547 | Nitsch et al. | Jul 2011 | B2 |
| 8003939 | Jindai et al. | Aug 2011 | B2 |
| 8087282 | Sawa et al. | Jan 2012 | B2 |
| 8186210 | Hangen | May 2012 | B2 |
| 8212995 | Koehler et al. | Jul 2012 | B2 |
| 8234912 | Suarez-Rivera et al. | Aug 2012 | B2 |
| 8245318 | Jin et al. | Aug 2012 | B2 |
| 8281648 | Leroux | Oct 2012 | B2 |
| 8294406 | Gajjar | Oct 2012 | B2 |
| 8302480 | Maris et al. | Nov 2012 | B2 |
| 8310128 | Ferreira et al. | Nov 2012 | B2 |
| 8322220 | Prater et al. | Dec 2012 | B2 |
| 8353060 | Watanabe et al. | Jan 2013 | B2 |
| 8370960 | Proksch et al. | Feb 2013 | B2 |
| 8387161 | Finlan et al. | Feb 2013 | B2 |
| 8448261 | Paissan et al. | May 2013 | B2 |
| 8453498 | Warren et al. | Jun 2013 | B2 |
| 8479310 | Humphris | Jul 2013 | B2 |
| 9753016 | Daugela | Sep 2017 | B1 |
| 9885691 | Daugela | Feb 2018 | B1 |
| 11346857 | Daugela | May 2022 | B1 |
| 20090272191 | Maris et al. | Nov 2009 | A1 |
| 20110174036 | Mauvoisin | Jul 2011 | A1 |
| 20110231966 | Passian et al. | Sep 2011 | A1 |
| 20120281207 | Yoshimizu et al. | Nov 2012 | A1 |
| Number | Date | Country |
|---|---|---|
| 9115747 | Oct 1991 | WO |
| 2013019717 | Feb 2013 | WO |
| Entry |
|---|
| Antanas Daugela and Jurgis Daugela, “Opto-nanomechanical test instrument in mechanical characterization of DLC coated MEMS devices”, Microsystem technologies, https://doi.org/10.1007/s00542-020-04800-1. |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 17393462 | Aug 2021 | US |
| Child | 17827759 | US |