CORROSION INHIBITING POLYMER COMPOSITIONS, MIXTURES, AND METHODS OF USING THE SAME

Information

  • Patent Application
  • 20180030345
  • Publication Number
    20180030345
  • Date Filed
    January 26, 2017
    7 years ago
  • Date Published
    February 01, 2018
    6 years ago
Abstract
Disclosed herein are polymer compositions useful for inhibiting corrosion of metal surfaces in industrial process water recirculating systems. The polymer compositions include interpolymers of about 90 mol % to about 97 mol % of a first monomer, about 0.01 mol % to about 5 mol % of a second monomer that is chemically different from the first monomer, and about 0.01 mol % to about 5 mol % of a third monomer that is chemically different from the first and second monomers; and optionally a fourth monomer that is chemically different from the first, second, and third monomers. About 0.05 ppm to about 200 ppm by weight of the polymer composition is dispersed in an industrial process water source, optionally in the presence of a divalent or higher valency metal ion. The dispersed polymer compositions significantly reduce the corrosion rate of metal surfaces of industrial equipment, even after one or more cycles of concentration.
Description
TECHNICAL FIELD

The present invention relates to polymer compositions and aqueous mixtures of the same for use as corrosion inhibitors. The polymer compositions herein inhibit corrosion in water containing systems in relatively low concentrations.


BACKGROUND

Cooling systems, desalination, or other water containing systems can become less efficient or malfunction over time due to corrosion caused at least in part by impurities or “corrodents” in the water circulating through the system. Corrodents, such as salts and/or other dissolved solids, liquids, or gasses cause, accelerate, or promote corrosion of metal containments such as metal pipelines used to transport the water sources toward, into, out of, or away from a subterranean formation; metal tanks used to hold the water sources for a period of time; surfaces of water containing equipment such as heat exchangers, dishwashers, or laundry machines; and/or other metal equipment that contacts the water sources before, during, or after injection or production. Non-limiting examples of such corrodents are hydrogen sulfide, carbon dioxide, oxygen, sodium chloride, calcium chloride, and/or sulfur dioxide. Corrosion can pit, crack, erode, or otherwise degrade the surfaces of the system that contact the water. In some applications, aqueous liquids are injected into the earth and/or recovered from the earth during subterranean hydrocarbon recovery processes such as hydraulic fracturing (fracking) and tertiary oil recovery. In all these systems, asset integrity due to corrosion can be compromised which results in increased repair and maintenance costs and even premature failure of the equipment. In one or more such processes, an aqueous liquid called an “injectate” is injected into a subterranean formation. Injectates include water and entrained solids and/or solvents therein. In one or more such processes a water source called “produced water” is recovered, i.e. flows back from the subterranean formation and is collected. Produced water includes one or more of injectate, connate (native water present in the subterranean formation along with the hydrocarbon), sea water, and minor (<5 wt. %) amounts of hydrocarbon products, which are hydrocarbon liquids or solids entrained (dispersed, emulsified, or dissolved) in the produced water. In embodiments, one or more of the injectate and the produced water includes corrodents. As a result, operators of water circulating systems, and almost all operators in the oil and gas industry, employ corrosion inhibitors to reduce internal corrosion in metal containments which are contacted by aqueous liquids containing corrodents.


Corrosion may be caused by a relatively high amount of corrodents or corrosive conditions (e.g., high temperature or a pH below 4 or above 10). For example, sea water has a high amount of scale causing calcium ions and carbonate ions compared to freshwater in addition to total dissolved solids such as chlorides. Water containing systems utilizing sea water often undergo heavy corrosion as the sea water is thermally shocked or concentrated, and must be protected against such corrosion to last and efficiently function. Typically, at higher temperatures such as above 50 or 80 degrees Celsius and/or at higher concentrations cause by evaporation, corrosion may progress more readily. Thus, systems operating at high temperatures may undergo faster or more extensive corrosion than systems operating at ambient temperatures. Similarly, scales can deposit out of the water source onto the surfaces of the system at temperatures and higher concentration of scale forming components in the water source, which can lead to under deposit corrosion.


Typically, corrosion inhibiting agents include phosphorous containing components, such as phosphates or phosphonates. Such phosphorous containing components may not be desirable if the water is going to be discharged from the system, because phosphorous containing components can foul water sources and surfaces that come in contact with the same, often causing unwanted or harmful blooms of algae or other plant life. The algae can be responsible for microbial induced corrosion or under deposit corrosion.


Coastal or isolated areas may not have a ready supply of water having low total dissolved solids (e.g., less than about 4000 ppm) for circulation through some water containing systems. Even freshwater may be recirculated through a water containing system only a limited number of times before the TDS content therein concentrates to a point where this environment can cause significant challenge to corrosion. However, replacement freshwater may not be a readily available resource. As long as water having low amounts of total dissolved solids is in relatively short supply, users of systems requiring water, such as desalination, cooling, pulp processing, ware-washing, laundry, etc., will continue to search for means of efficiently using the water sources on hand, such as high TDS (e.g., over 4,000 ppm) water sources. Even soft water may also provide a highly corrosive environment the soft water may not have enough buffer capacity and/or low alkalinity, which may cause large pH swings.


Thus, there is a substantial need in the industry for polymer compositions that are free of phosphorous and that are suitable for use as corrosion inhibitors in water containing systems.


SUMMARY

In an embodiment, a corrosion inhibiting polymer mixture is disclosed. The corrosion inhibiting polymer mixture comprising a water source and about 0.05 ppm to about 200 ppm of a polymer composition. The polymer composition comprises about 50 mol % to about 99 mol % of a first monomer comprising a carboxylic acid residue. The polymer composition further comprises about 0.01 mol % to about 45 mol % of a second monomer comprising one of a sulfonated acid residue or a second carboxylic acid residue, wherein the first monomer is chemically different from the second monomer.


In an embodiment, a polymer composition is disclosed. The polymer composition comprsing a plurality of monomers, the plurality of monomers including three, four, or five monomers. The plurality monomers comprises about 90 mol % to about 97 mol % of a first monomer comprising a residue of one of acrylic acid, a salt thereof, or a conjugate base thereof; maleic acid, a salt thereof, or a conjugate base thereof; or methacrylic acid, a salt thereof, or a conjugate base thereof. The plurality monomers comprises about 0.01 mol % to about 5 mol % of a second monomer comprising a residue of one of 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof maleic acid, a salt thereof, or a conjugate base thereof; methacrylic acid, a salt thereof, or a conjugate base thereof; or sulfostyrene, wherein the first monomer is chemically different from the second monomer. The plurality monomers comprises about 0.01 mol % to about 5 mol % of a third monomer, the third monomer comprising a residue of one of 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof; itaconic acid, a salt thereof, or a conjugate base thereof crotonic acid, a salt thereof, or a conjugate base thereof tert-butylacrylamide, a salt thereof, or a conjugate base thereof or dimethylacrylamide, a salt thereof, or a conjugate base thereof and wherein the third monomer is chemically different from the first monomer and the second monomer.


In an embodiment, a method of inhibiting corrosion in water containing systems is disclosed. The method comprises adding about 0.05 ppm to 1000 ppm of a corrosion inhibiting polymer composition to a water source to form a corrosion inhibiting polymer mixture. The corrosion inhibiting polymer composition comprises about 55 mol % to about 99 mol % of a first monomer and the first monomer comprises a residue of one of a carboxylic acid or a conjugate base thereof. The corrosion inhibiting polymer composition comprises about 0.01 mol % to about 45 mol % of a second monomer comprising a residue of one of a sulfonated acid or a conjugate base thereof, or a second carboxylic acid or a conjugate base thereof, wherein the first monomer is chemically different from the second monomer. The method includes applying the corrosion inhibiting polymer mixture to a water containing system.


In an embodiment, a water containing system is disclosed. The water containing system includes the corrosion inhibiting polymer mixture of disclosed above therein, in a concentration of less than about 200 ppm.


Additional advantages and novel features of the invention will be set forth in part in the description that follows, and in part will become apparent to those skilled in the art upon examination of the following, or may be learned through routine experimentation upon practice of the invention.





BRIEF DESCRIPTION OF THE DRAWINGS


FIG. 1 is graph of corrosion rate versus time for various working examples.



FIG. 2 is a graph of corrosion rate versus time for a composition of the invention recirculated in a pilot cooling tower for 14 days.





DETAILED DESCRIPTION

Although the present disclosure provides references to preferred embodiments, persons skilled in the art will recognize that changes may be made in form and detail without departing from the spirit and scope of the invention. Various embodiments will be described in detail with reference to the drawings, wherein like reference numerals represent like parts and assemblies throughout the several views. Reference to various embodiments does not limit the scope of the claims attached hereto. Additionally, any examples set forth in this specification are not intended to be limiting and merely set forth some of the many possible embodiments for the appended claims.


Definitions

Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. In case of conflict, the present document, including definitions, will control. Preferred methods and materials are described below, although methods and materials similar or equivalent to those described herein can be used in practice or testing of the present invention. All publications, patent applications, patents and other references mentioned herein are incorporated by reference in their entirety. The materials, methods, and examples disclosed herein are illustrative only and not intended to be limiting.


As used herein, the term “polymer composition” means a water soluble, emulsible, or dispersible polymer of two or more interpolymerized monomeric units. Unless otherwise specified or provided by context, “polymer composition” refers to the polymer as synthesized, that is, prior to mixture in a water source as a corrosion inhibitor or another use. As used herein, the term “monomer” is used in context to mean an unsaturated radically polymerizable compound, a conjugate base thereof, a salt thereof (e.g., carboxylate salt), or the polymerized residue thereof. Monomers may include an anionic monomer or cationic monomer. As used herein, the term “anionic monomer” means an unsaturated compound or polymerized residue thereof bearing an acidic group having a pKa of about 5 or less, the conjugate base thereof bearing a negative charge, or a salt thereof. As used herein, the term “cationic monomer” means an unsaturated compound or polymerized residue thereof bearing a positive charge, or a salt thereof.


As used herein, the term “chemically different” refers to chemical species having a different number of carbon atoms and/or different functionalities (e.g., moieties) from another species; different isomers; or two or more such differences. For the purposes of this disclosure an acid, an ion, a conjugate base, or a salt of a chemical species is not considered chemically different from the species.


As used herein, the term “polymer mixture” means a polymer composition, as disclosed herein, as mixed in water, a water source, an aqueous solution, or combinations of any of the foregoing. Polymer mixtures may include a polymer dispersion, a polymer emulsion, a dissolved polymer solution, or combinations of any of the foregoing in water and/or a water source. As context dictates, the term “mixing” may include emulsifying, dispersing, dissolving, or otherwise adding the polymer composition to water and/or the water source. As context dictates, the term “mixed” may refer to an emulsified, dispersed, dissolved, or other combination of the polymer composition and water and/or the water source, or to the act of mixing as described above.


As used herein, the term “polymer dispersion” means a solid polymer composition substantially suspended or dissolved in water or a water based solution. The polymer dispersion is a dispersion as formed, or in the case of some applications the dispersion before circulation, during circulation, after circulation, before injection, during injection, or after injection as determined by context. Water based solutions may include one or more dissolved salts, buffers, acids, bases, surfactants, or other dissolved, dispersed, or emulsified compounds, materials, components, or combinations thereof


As used herein, the term “polymer emulsion” means a liquid polymer composition substantially suspended in water and/or a water source. Emulsified polymer compositions (latices) include a continuous phase and a discontinuous phase dispersed in the continuous phase. In some embodiments, an emulsion is a microemulsion. Microemulsions are characterized as emulsions that are substantially transparent and thermodynamically stable. The polymer emulsion is an emulsion as formed, or in the case of some applications the emulsion before circulation, during circulation, after circulation, before injection, during injection, or after injection as determined by context. A polymer emulsion may include one or more dissolved salts, buffers, acids, bases, surfactants, or other dissolved, dispersed, or emulsified compounds, materials, components, or combinations thereof.


As used herein, the term “tagging agent” means a monomer capable of fluorescing or a derivative thereof. As used herein, the term “tagged polymer” means a polymer composition, as described herein, that has a tagging agent polymerized therein.


As used herein, “corrodents” are materials which cause, initiate, catalyze, accelerate, induce, decrease the onset time of, and/or otherwise promote the corrosion of metal in systems where the metal is contacted by a water source including the corrodent. Non-exhaustive examples of corrodents include oxygen gas, inorganic acids and bases, elemental alkali metals, manganese-based compounds, organic acids, halides, hydrogen sulfide, etc. In some embodiments, corrosive activity of corrodents are further affected by the presence of other compounds in a water source; thus, for example, low concentrations of calcium salts associated with water “hardness” are associated with greater corrosion by existing corrodents in a water source. In such embodiments, for example, a “corrodent” may be defined as a lack of calcium salts, or a low concentration of calcium salts in a water source.


As used herein, the term “corrosion inhibitor” is a material (e.g., polymer mixture) which inhibits corrosion of one or more metals in an industrial process water source when the corrosion inhibitor and/or a composition comprising the corrosion inhibitor is added to the water source and/or is applied to a metal before, during, and/or after exposure of the metal to an industrial process water source.


As used herein, the term “water source” or “industrial process water source” means a source of water having one or more corrodents. An industrial process water source is any water source disposed within or for disposal within industrial process equipment, where contact of the water source with the equipment can cause corrosion. In embodiments, a water source includes a total dissolved solids (“TDS”) content of about 200 ppm to 350,000 ppm (e.g., about 550 ppm or more, about1300 ppm or more, about 2400 ppm or more, or less than about 4000 ppm) such as about 4000 ppm to 350,000 ppm; or one or more of a dissolved calcium content of about 50 ppm to 15,000 ppm (e.g., about 100 ppm, about 400 ppm, or about 550 ppm) such as about 300 ppm to 15,000 ppm, a dissolved magnesium content of about 25 ppm to 30,000 ppm (e.g., about 50 ppm, about 165 ppm or about 380 ppm) such as about 1000 ppm to 30,000 ppm, a dissolved potassium content of about 10 ppm to 15,000 ppm (e.g., about 50 ppm) such as about 300 ppm to 15,000 ppm, a dissolved sodium content of about 100 ppm to 15,000 ppm (e.g., about 200 ppm) such as about 5,000 ppm to about 100,000 ppm, a dissolved silica content of about 5 ppm to 1000 ppm such as about 10 ppm to about 1000 ppm, dissolved chloride content of about 100 ppm to about 15,000 ppm (e.g., about 200 ppm, or about 600 ppm) such as about 200 ppm to about 10,000 ppm, carbonate alkalinity content of about 50 ppm to 5000 ppm (e.g., about 100 ppm, about 200 ppm, or about 250 ppm) such as about 150 ppm to about 3000 ppm, a dissolved iron content of about 0.01 ppm to about 10 ppm, a dissolved manganese content of about 0.01 ppm to about 10 ppm, or a dissolved sulfate content of about 50 ppm to 20,000 ppm (e.g., about 100 ppm, about 350 ppm, or about 600 ppm) such as about 2000 to about 15,000 ppm. As used herein “TDS” refers to the total amount of non-polymeric minerals, salts, metals, anions, and cations dissolved in a given volume of water. Some water sources may include soft water, municipal water, balanced water, high-chloride/sulfate water, well water, produced water, surface water, connate, waste water such as runoff water, “gray” water, treated or partially treated waste water, brackish water, sea water, or a combination of two or more such water sources as determined by context. In some embodiments, a water source includes one or more salts, ions, buffers, acids, bases, surfactants, or other dissolved, dispersed, or emulsified compounds, materials, components, or combinations thereof. In some such embodiments, the total dissolved solids are substantially non-polymeric solids. In some such embodiments, the dissolved solids comprise, consist essentially of ionic compounds. In some examples, and as determined by context, the term “water source” may include high TDS water sources (e.g., water sources having a TDS content above about 4000 ppm such as seawater, connate, produced water, or brackish water) and/or high temperature (e.g., 40 degrees Celsius and above) water. A “water source” may alternatively or additionally include fresh water such as tap water, distilled water, soft water, balanced water, high-chloride/sulfate water, or any other low TDS water (e.g., water having a TDS below about 4000 ppm). In some embodiments, the low TDS water is, was, or will be concentrated to contain the high TDS content disclosed above for a high TDS water source. For example, fresh water having a relatively low TDS content may be used in a cooling system having a cooling tower, wherein the relatively low TDS content of the fresh water is inherently corrosive and may also become increasingly concentrated over time due to evaporation of water on the cooling tower.


As used herein, the term “soft water” refers to a water source having a total dissolved solids content of about 100 ppm to about 1000 ppm such as about 100 ppm to about 550 ppm, or 400 ppm to about 700 ppm, or about 550 ppm; a calcium content of 10 ppm to about 150 ppm such as about 10 ppm to about 100 ppm; a magnesium content of about 10 ppm to about 100 ppm such as about 10 ppm to about 50 ppm; a carbonate alkalinity content of about 50 ppm to 150 ppm such as about 50 ppm to about 100 ppm; a chloride content of about 10 ppm to about 300 ppm such as about 10 ppm to about 200 ppm; a sulfate content of about 10 ppm to about 200 ppm such as about 50 ppm to about 100 ppm; and a pH between about 7.5 and about 8.2 such as about 8.2. Further dissolved solids (e.g., sodium, potassium, etc.) may be present in the soft water, which may increase the TDS content of soft water disclosed above.


As used herein, the term “balanced water” refers to a water source having a total dissolved solids content of about 450 ppm to about 1800 ppm such as about 800 ppm to about 1600 ppm or about 1365 ppm; a calcium content of 100 ppm to about 500 ppm such as about 100 ppm to about 400 ppm; a magnesium content of about 50 ppm to about 250 ppm such as about 50 ppm to about 165 ppm; a carbonate alkalinity content of about 100 ppm to 350 ppm such as about 100 ppm to about 250 ppm; a chloride content of about 50 ppm to about 400 ppm such as about 100 ppm to about 200 ppm; a sulfate content of about 150 ppm to about 350 ppm such as about 350 ppm; and a pH between about 8.0 and about 8.8 such as about 8.5 to about 8.8. Further dissolved solids (e.g., sodium, potassium, etc.) may be present in the balanced water, which may increase the TDS content of the balanced water disclosed above.


As used herein, the term “high-chloride/sulfate water” refers to a water source having higher chloride and/or sulfate content than soft water or balanced water (e.g., in the ranges below), and, a total dissolved solids content of about 1000 ppm to about 4000 ppm such as about 1000 ppm to about 3000 ppm, about 1000 ppm to about 2550 ppm, or about 2330 ppm; a calcium content of 100 ppm to about 700 ppm such as about 100 ppm to about 550 ppm; a magnesium content of about 50 ppm to about 500 ppm such as about 50 ppm to about 380 ppm; a carbonate alkalinity content of about 100 ppm to 300 ppm such as about 100 ppm to about 200 ppm; a chloride content of about 400 ppm to about 800 ppm such as about 400 ppm to about 600 ppm; a sulfate content of about 350 ppm to about 800 ppm such as about 400 ppm to about 600 ppm; and a pH between about 8.0 and about 8.8 such as about 8.5 to about 8.8. Further dissolved solids (e.g., sodium, potassium, etc.) may be present in the high-chloride/sulfate water, which may increase the TDS content of the high-chloride/sulfate water disclosed above.


As used herein, the term “dosage” refers to the concentration of a polymer in a water source, such as in parts per million (ppm). Dosage includes the as-mixed amount of polymer in the water source.


As used herein, “cycles of concentration (‘COC’)” refers to the ratio of the concentration of dissolved solids (e.g., TDS) in the blowdown water as compared to the concentration of dissolved solids in make-up water of a particular water containing system. Notwithstanding the differences in TDS content between blow-down water and make-up water, typically, COC is measured using the same water source for all of the water associated therewith (e.g., fresh water or saltwater from the same source makes up the water in the system (blow-down) and the make-up water). The specific TDS content associated with a COC varies with the TDS content of the particular water source in use.


As used herein, “water containing system” refers to a system having one or more hard parts (e.g., metal parts) that conduct, hold, contain, filter, or otherwise come in contact with a water source. Exemplary water containing systems include cooling systems (e.g., cooling towers, radiators, heat pipes, etc.), pipes, drilling equipment (e.g., drill strings, drilling mud, etc.), fracking equipment, paper or pulp processing systems, wastewater treatment systems, water purification systems, ware washing, evaporators, condensers, filtration equipment, membranes, mining equipment, water softening systems, kamyr digesters, pumps, storage vessels, or any other systems using water sources that contact one or more surfaces therein. Such surfaces may include the interior of pipes, storage vessels, radiators, heat pipes, filters, digesters, condensers, etc.; the exterior of cooling towers; or any other surface that contacts a water source. The surfaces of the water containing systems disclosed herein may include metals, such as iron, steel (e.g., stainless steel, carbon steel, or galvanized steel), copper, lead, zinc (e.g., anodized pipes), aluminum, or any other metal suitable for use in water containing systems; plastics, such as polyethylene (e.g., PEX), polypropylene, polytetrafluoroethylene, polyvinyl chlorides, acrylonitrile butadiene styrene, etc.; glass (e.g., glass storage vessels), rubber or latex (rubber hoses or tubes); fiberglass; concrete or stone; or any other material suitable to hold, transport, or filter water.


As used herein, the term “carbon steel” means steel in which the main alloying component with iron is carbon, wherein the carbon steel comprises between about 0.1% to about 2.1% by weight of carbon.


As used herein, the term “molecular weight” refers to the weight average molecular weight (MW) unless otherwise recited or by context.


The terms “comprise(s),” “include(s),” “having,” “has,” “can,” “contain(s),” and variants thereof, as used herein, are intended to be open-ended transitional phrases, terms, or words that do not necessarily but may preclude the possibility of additional acts or structures. The singular forms “a,” “and,” and “the” include plural references unless the context clearly dictates otherwise. The present disclosure also contemplates other embodiments “comprising,” “consisting of,” and “consisting essentially of,” the embodiments or elements presented herein, whether explicitly set forth or not. Generally and as determined by context, the term “includes,” as used in the specification, may be interpreted to mean any of “comprising,” “consisting of,” or “consisting essentially of.”


As used herein, the term “optional” or “optionally” means that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances in which it does not.


As used herein, the term “about” modifying, for example, the quantity of an ingredient in a composition, concentration, volume, process temperature, process time, yield, flow rate, pressure, and like values, and ranges thereof, employed in describing the embodiments of the disclosure, refers to variation in the numerical quantity that can occur, for example, through typical measuring and handling procedures used for making compounds, compositions, concentrates or use formulations; through inadvertent error in these procedures; through differences in the manufacture, source, or purity of starting materials or ingredients used to carry out the methods, and like proximate considerations. The term “about” also encompasses amounts that differ due to aging of a formulation with a particular initial concentration or mixture, and amounts that differ due to mixing or processing a formulation with a particular initial concentration or mixture. Where modified by the term “about” the claims appended hereto include equivalents to these quantities.


As used herein, the word “substantially” or “consisting essentially of” modifying, for example, the type or quantity of an ingredient in a composition, a property, a measurable quantity, a method, a position, a value, or a range, employed in describing the embodiments of the disclosure, refers to a variation that does not affect the overall recited composition, property, quantity, method, position, value, or range thereof in a manner that negates an intended composition, property, quantity, method, position, value, or range. Examples of intended properties include, solely by way of non-limiting examples thereof, flexibility, partition coefficient, rate, solubility, temperature, and the like; intended values include thickness, yield, weight, concentration, and the like. The effect on methods that are modified by “substantially” or “consisting essentially of” include the effects caused by variations in type or amount of materials used in a process, variability in machine settings, the effects of ambient conditions on a process, and the like wherein the manner or degree of the effect does not negate one or more intended properties or results; and like proximate considerations. Where modified by the term “substantially” or “consisting essentially of” the claims appended hereto include equivalents to these types and amounts of materials.


Discussion


Polymer Compositions


We have found new polymer compositions (e.g., composite polymers) capable of inhibiting corrosion formation in a water containing system without the use of phosphorous containing moieties or residues. Polymer compositions including acrylic acid (“AA”), maleic acid (“MA”), methacrylic acid (“MAA”), conjugate bases thereof, or salts thereof, and at least one additional monomer may inhibit corrosion in water containing systems. Such corrosion may be due to corrodents (e.g., corrosion inducing components such as acids or dissolved alkaline salts (e.g., alkaline metals or alkaline earth metals) in solution or solid form (e.g., suspended or dissolved solids) and counter ions thereof (e.g., carbonate, sulfate, phosphate, chloride, etc.), dissolved gasses such as carbon dioxide, hydrogen sulfide, etc.) in a water source and/or a high temperatures of the water source. The polymer compositions and polymer mixtures disclosed herein inhibit corrosion, in water containing systems without the use of phosphorous or phosphorous containing compounds (e.g., phosphates) that tend to foul ground water or watersheds. The polymers herein may be used in any water containing system including a water source having high TDS, such as connate, produced water, or saltwater (e.g., brackish water or seawater) systems; or a system having low TDS water source (e.g., less than 4000 ppm TDS) such as freshwater, soft water, balanced water, high-chloride/sulfate water, municipal water, or cooling water. Suitable applications for the polymers herein may include scale or corrosion inhibition in freshwater systems; municipal waste treatment systems; municipal potable water treatment systems or delivery lines; cooling systems employing low TDS water (e.g., less than about 4000 ppm TDS, such as freshwater, soft water, balanced water, high-chloride/sulfate water, municipal water, or cooling water); desalination systems; cooling systems employing salt, brine, or seawater; drilling systems utilizing aqueous drilling fluids or produced water; pulp processing; or any other water containing system in which corrosion and/or scale inhibition is desired.


The corrosion inhibitors herein are beneficial in that they permit the use of carbon steel components rather than the much more expensive high nickel, cobalt, and chromium alloys or other materials either more expensive than carbon steel and/or which inherently entail other disadvantages in suitability for the purpose of liquid containment. Corrosion inhibitors may be added to the liquids and dissolved gasses which come into contact with metal surfaces and such inhibitors prevent, retard, delay, reverse, and/or otherwise inhibit the corrosion of metal surfaces such as carbon-steel metal surfaces in water containing systems. While highly desirable for this purpose, their use entails additional cost for the operator. Further, such corrosion inhibitors must ultimately be disposed in the environment. It is therefore advantageous to provide the corrosion inhibiting polymers disclosed herein which are effective in low amounts and provide compositions containing the corrosion inhibiting polymers at the lowest concentrations, wherein the corrosion inhibiting polymers provide effective corrosion inhibition at the relatively low amounts disclosed herein.


In embodiments, produced water is reused in an injectate wherein the injectate comprises, consists of, or consists essentially of the produced water, the injectate is reinjected into a pipe leading to a subterranean reservoir, and a crude oil/recycled produced water is subsequently recovered from a subterranean reservoir. If such injectate contains corrosion inhibitor, some of the corrosion inhibitor remains in the ground, some is returned as part of the recycled produced water, or both. If some of the corrosion inhibitor remains in the ground, this is a loss to the operator. Further, the corrosion inhibitor remaining in the ground, depending on its chemical nature and concentration, can be environmentally deleterious. It is therefore also advantageous to use the corrosion inhibitors herein which are effective in lowest amount (e.g., less than 100 ppm, or less than 20 ppm, or less than 5 ppm) and to provide compositions containing corrosion inhibitors effective at the lowest concentrations, wherein the corrosion inhibitors provide effective corrosion inhibition using the least amounts of corrosion inhibitor.


The polymer compositions herein can include at least two monomers, such as a copolymer including an AA residue and a 2-acrylamido-2-methylpropane sulfonic acid (“ATBS”) residue. The polymers disclosed herein may inhibit corrosion when used at relatively low concentrations in water sources, such as below about 200 ppm. For example, the copolymers, terpolymers, tetrapolymers, and pentapolymers disclosed below may facilitate selective inhibition of corrosion in systems utilizing corrodent containing water source(s), without the presence of phosphorous containing moieties. Such corrosion can be due in part to one or more of pH, temperature, or dissolved solids content and/or species in the water source or system.


The polymer compositions herein may include two or more polymerized monomers, such as 2-10 monomers, 2-7 monomers, 2-5 monomers, 3-5 monomers, 2 monomers, 3 monomers, 4 monomers, 5 monomers, or more than 5 monomers, as described below. The polymer compositions herein may be substantially free of (e.g., having substantially no) phosphorous or phosphorous containing materials, such as phosphates, phosphonates, or the like.


Copolymers


In some embodiments, the corrosion inhibiting polymer composition is a copolymer. The copolymer may comprise, consist essentially of, or consist of a polymerized residue of 2 or more monomers. The two or more monomers may include a first monomer comprising, consisting essentially of, or consisting of a carboxylic acid or a residue thereof and a second monomer comprising, consisting essentially of, or consisting of a sulfonated acid or a residue thereof. The first monomer may include a carboxylic acid or a residue of a molecule having at least one carboxyl moiety, a salt thereof, or a conjugate base thereof. The carboxylic acid may include a single carboxyl moiety or a plurality of carboxyl moieties (e.g., dicarboxylic acids such as maleic acid, etc.).


Suitable carboxylic acids for use as the first monomer may comprise, consist essentially of, or consist of, by way of example, an alkyl acrylic acid such as MAA, a butenoic acid (e.g., crotonic acid), a pentenoic acid, propenoic acid (AA), or any other unsaturated monocarboxylic acid capable of polymerizing; dicarboxylic acids such as MA or maleic anhydride, fumaric acid, itaconic acid; glutaconic acid, muconic acid, succinic acid, or any other unsaturated dicarboxylic acid or anhydride thereof capable of polymerizing; tricarboxylic acids or greater, such as citric acid, aconitic acid, or any other carboxylic acid having three or more carboxylic acid moieties; or any other monomers having at least one carboxyl moiety; a salt of any of the foregoing, or a conjugate base of any of the foregoing. In some embodiments, the first monomer is formed from one of any of the foregoing carboxylic acids, a salt thereof, or a conjugate base thereof. For example, the first monomer may include a carboxylate (e.g., dicarboxylate) of any of the foregoing carboxylic acids. Carboxylic acid salts may include Lithium, Beryllium, Sodium, Magnesium, Potassium, Calcium, Zinc etc., salts.


The first monomer may constitute about 55 mol % of the copolymer or more, such as about 55 mol % to about 99 mol %, about 60 mol % to about 98 mol %, about 70 mol % to about 95 mol %, about 80 mol % to about 99 mol %, about 90 mol % to about 97 mol %, about 93 mol % to about 99 mol %, about 96 mol % to about 99 mol %, about 92 mol % to about 94 mol %, about 83 mol % to about 87 mol %, about 88 mol % to about 92 mol %, about 93 mol % to about 96 mol %, about 95 mol % to about 98.5 mol %, about 60 mol %, about 70 mol %, about 80 mol %, about 85 mol %, about 90 mol %, about 92.9 mol %, about 93.3 mol %, about 95 mol %, about 96 mol %, about 96.4 mol %, about 98.4 mol %, or about 98.5 mol % of the copolymer or less.


The first monomer may constitute about 50 wt % of the copolymer or more, such as about 50 wt % to about 95 wt %, about 60 wt % to about 90 wt %, about 70 wt % to about 85 wt %, about 80 wt % to about 95 wt %, about 85 wt % to about 90 wt %, about 90 wt % to about 95 wt %, about 73 wt % to about 77 wt %, about 78 wt % to about 82 wt %, about 83 wt % to about 87 wt %, about 88 wt % to about 92 wt %, about 93 wt % to about 96 wt %, about 60 wt %, about 70 wt %, about 80 wt %, about 85 wt %, about 90 wt %, about 95 wt %, or about 96 wt % of the copolymer or less.


In an embodiment, the second monomer of the copolymer comprises, consists essentially of, or consists of a sulfonated acid or a residue thereof. The sulfonated acid may include a sulfonated acid moiety, a salt thereof, or a conjugate base thereof. The sulfonated acid may include an amide moiety, such as in ATBS. Suitable sulfonated acids may include ATBS, sulfostyrene, vinylsulfonic acid, methallylsulfonic acid, a salt of the foregoing (e.g., sodium methallyl sulfonate or ATBS sodium salts), or a conjugate base of the foregoing (e.g., methallyl sulfonate).


The second monomer may constitute about 45 mol % of the copolymer or less, such as about 0.01 mol % to about 45 mol %, about 1 mol % to about 40 mol %, about 20 mol % to about 30 mol %, about 0.01 mol % to about 15 mol %, about 0.01 mol % to about 10 mol %, about 0.01 mol % to about 5 mol %, about 2 mol % to about 4 mol %, about 1 mol % to about 5 mol %, about 5 mol % to about 15 mol %, about 10 mol % to about 15 mol %, about 5 mol % to about 10 mol %, about 18 mol % to about 22 mol %, about 13 mol % to about 17 mol %, about 8 mol % to about 12 mol %, about 3 mol % to about 7 mol %, about 2 mol %, about 3 mol %, about 3.6 mol %, about 3.7 mol %, about 4 mol %, about 5 mol %, about 10 mol %, about 15 mol %, about 20 mol %, about 20 mol % or less, or about 10 mol % of the copolymer or less.


The second monomer may constitute about 50 wt % of the copolymer or less, such as about 0.01 wt % to about 50 wt %, about 10 wt % to about 40 wt %, about 20 wt % to about 30 wt %, about 0.01 wt % to about 15 wt %, about 0.01 wt % to about 10 wt %, about 0.01 wt % to about 5 wt %, about 5 wt % to about 15 wt %, about 10 wt % to about 15 wt %, about 5 wt % to about 10 wt %, about 18 wt % to about 22 wt %, about 13 wt % to about 17 wt %, about 8 wt % to about 12 wt %, about 3 wt % to about 7 wt %, about 5 wt %, about 10 wt %, about 15 wt %, about 20 wt %, about 20 wt % or less, or about 10 wt % of the copolymer or less.


In an embodiment, the first monomer of the copolymer comprises, consists essentially of, or consists of one or more of AA, MA, MAA, or residues thereof. In an embodiment, the second monomer of the copolymer comprises, consists essentially of, or consists of one or more of MA, ATBS, sulfostyrene, methallylsulfonic acid, or residues thereof, where the second monomer is chemically different (e.g., chemically distinct) from the first monomer. In an embodiment, the copolymer includes AA residue and ATBS residue. The AA residue may constitute about 90 mol % to about 99 mol % (e.g., about 95 mol % to about 98.5 mol %) of the copolymer and the ATBS residue may constitute at least a portion of the balance of the copolymer. In an embodiment, the copolymer is MA residue and ATBS residue. The MA residue may constitute about 90 mol % to about 99 mol % (e.g., about 95 mol % to about 98.5 mol %) of the copolymer and the ATBS residue may constitute at least a portion of the balance of the copolymer. In an embodiment, the copolymer is MAA residue and ATBS residue. The MAA residue may constitute about 90 mol % to about 99 mol % (e.g., about 95 mol % to about 98.5 mol %) of the copolymer and the ATBS residue may constitute at least a portion of the balance of the copolymer. In an embodiment, the copolymer comprises, consists essentially of, or consists of a first monomer including one of AA, MA, MAA, or residues thereof; and a second monomer including one of sulfostyrene residue, methallyl sulfonate, or residues thereof. For example, the first monomer may be AA or MA residue and the second monomer may be sulfostyrene residue. The AA residue may constitute about 90 mol % to about 99 mol % (e.g., about 95 mol % to about 98.5 mol %) of the copolymer and the sulfostyrene residue may constitute at least a portion of the balance of the copolymer.


As discussed in detail below, the copolymer can exhibit any of a wide range of molecular weights. As discussed in more detail below, the copolymer can be mixed in water (e.g., tap or distilled water) and/or a water source in any of a wide range of concentrations. Without wishing to be limited by theory, we believe that during use, one or more moieties (e.g., hydrophobes) present in the polymer may act to bond to a metal surface forming a passivating film on the metal surface and/or could act as a cathodic or anodic inhibitor, or otherwise render corrodents substantially ineffective or very slow to corrode equipment in water containing systems, such as cooling, desalination, or drilling equipment. As discussed in detail below, the copolymers herein may also include a tagging agent.


Terpolymers


In some embodiments, the corrosion inhibiting polymer composition is a terpolymer. The terpolymer may comprise, consist essentially of, or consist of a first monomer including a carboxylic acid or a residue thereof a second monomer including a sulfonated acid or a residue thereof, or a second, chemically different carboxylic acid or a residue thereof and a third monomer including a sulfonated acid or a residue thereof, a third, chemically different carboxylic acid (e.g., differing from the first and second carboxylic acids), or an alkylated molecule or a residue thereof. In an embodiment, each of the first, second, and third monomers are chemically different from each other.


In an embodiment, the first monomer comprises, consists essentially of, or consists of a (first) carboxylic acid or a residue thereof substantially as described above with respect to the copolymer. For example, suitable carboxylic acids may include, by way of example, alkyl acrylic acids such as MAA, a butenoic acid (e.g., crotonic acid), a pentenoic acid, propenoic acid (AA), or any other unsaturated monocarboxylic acid capable of polymerizing; dicarboxylic acids such as MA, fumaric acid, itaconic acid; glutaconic acid, muconic acid, succinic acid, or any other unsaturated dicarboxylic acid capable of polymerizing; tricarboxylic acids or greater, such as citric acid, aconitic acid, or any other unsaturated carboxylic acid having three or more carboxylic acid moieties (e.g., carboxyl groups); or any other molecule having at least one carboxyl moiety, a salt thereof, or a conjugate base thereof. In some embodiments, the first monomer includes one of any of the foregoing carboxylic acids, a salt thereof, or a conjugate base thereof. For example, the first monomer may include a carboxylate (e.g., dicarboxylate) of any of the foregoing carboxylic acid monomers. Carboxylic acid salts may include Lithium, Beryllium, Sodium, Magnesium, Potassium, Calcium, Zinc, etc., salts.


The first monomer may constitute about 55 mol % of the terpolymer or more, such as about 55 mol % to about 99 mol %, about 60 mol % to about 98 mol %, about 70 mol % to about 95 mol %, about 80 mol % to about 99 mol %, about 85 mol % to about 98 mol %, about 90 mol % to about 97 mol %, about 93 mol % to about 97 mol %, about 93 mol % to about 99 mol %, about 96 mol % to about 99 mol %, about 92 mol % to about 94 mol %, about 83 mol % to about 87 mol %, about 88 mol % to about 92 mol %, about 93 mol % to about 96 mol %, about 60 mol %, about 70 mol %, about 80 mol %, about 85 mol %, about 90 mol %, about 92.9 mol %, about 93.3 mol %, about 95 mol %, about 96 mol %, about 96.4 mol %, or about 98.4 mol % of the terpolymer or less.


The first monomer may constitute about 50 wt % of the terpolymer or more, such as about 50 wt % to about 95 wt %, about 60 wt % to about 90 wt %, about 70 wt % to about 85 wt %, about 75 wt % to about 90 wt %, about 80 wt % to about 95 wt %, about 85 wt % to about 90 wt %, about 90 wt % to about 95 wt %, about 78 wt % to about 82 wt %, about 83 wt % to about 87 wt %, about 88 wt % to about 92 wt %, about 60 wt %, about 70 wt %, about 80 wt %, about 85 wt %, about 90 wt %, or about 90 wt % of the terpolymer or less.


In an embodiment, the second monomer of the terpolymer comprises, consists essentially of, or consists of one or more of a sulfonated acid, a (second) carboxylic acid, or a residue of any of the foregoing, where the second monomer is chemically different from the first monomer. The sulfonated acid (e.g., sulfonic acids) may include a sulfonate moiety, a salt thereof, or a conjugate base thereof, substantially as described above with respect to the copolymer.


In an embodiment, the second monomer of the terpolymer comprises, consists essentially of, or consists of one or more of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the second monomer is chemically different (e.g., a different chemical species) from the carboxylic acid of the first monomer. For example, the second monomer may include MA or MAA residue while the first monomer includes AA residue, or vice versa.


The second monomer may constitute about 45 mol % of the terpolymer or less, such as about 0.01 mol % to about 45 mol %, about 10 mol % to about 40 mol %, about 20 mol % to about 30 mol %, about 0.01 mol % to about 15 mol %, about 0.01 mol % to about 10 mol %, about 0.01 mol % to about 5 mol %, about 1.5 mol % to about 4 mol %, about 2 mol % to about 5 mol %, about 5 mol % to about 15 mol %, about 10 mol % to about 15 mol %, about 5 mol % to about 10 mol %, about 18 mol % to about 22 mol %, about 13 mol % to about 17 mol %, about 8 mol % to about 12 mol %, about 3 mol % to about 7 mol %, about 10 mol %, about 1.6 mol %, about 2 mol %, about 3 mol %, about 3.6 mol %, about 3.7 mol %, about 4 mol %, about 5 mol %, about 10 mol %, about 15 mol %, about 20 mol %, about 20 mol % or less, about 10 mol % or less, or about 5 mol % of the terpolymer or less.


The second monomer may constitute about 50 wt % of the terpolymer or less, such as about 0.01 wt % to about 50 wt %, 5 wt % to about 50 wt %, about 10 wt % to about 40 wt %, about 20 wt % to about 30 wt %, about 5 wt % to about 15 wt %, about 10 wt % to about 15 wt %, about 0.01 wt % to about 15 wt %, about 0.01 wt % to about 10 wt %, about 0.01 wt % to about 5 wt %, about 5 wt % to about 10 wt %, about 18 wt % to about 22 wt %, about 13 wt % to about 17 wt %, about 8 wt % to about 12 wt %, about 3 wt % to about 7 wt %, about 5 wt %, about 10 wt %, about 15 wt %, about 20 wt %, about 20 wt % or less, or about 10 wt % of the terpolymer or less.


In an embodiment, the third monomer of the terpolymer comprises, consists essentially of, or consists of one or more of one of a sulfonated acid, a (third) carboxylic acid, an alkylated molecule (e.g., molecule or residue thereof having one or more hydrophobic alkyl moieties) or a residue of any of the foregoing, where the third monomer is chemically different from the first monomer and the second monomer. The sulfonated acid (e.g., sulfonic acids) may include a sulfonate moiety, a salt thereof, or a conjugate base thereof as disclosed above.


In an embodiment, the alkylated molecule or residue thereof (e.g., alkylated acrylamide(s)) comprises at least one hydrophobic moiety such as an alkyl group of one or more carbons. Suitable alkylated molecules may include N-tert-butylacrylamide, N-isopropylacrylamide, butoxymethylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, dimethylamino ethyl methacrylate acid salts (including, but not limited to, sulfuric acid and hydrochloride acid salts), N-vinylpyrrolidone, analogues of any of the foregoing, residues of any of the foregoing, or any other molecule suitable for radical polymerization and being substantially as hydrophobic as the preceding examples.


In an embodiment, the third monomer comprises, consists essentially of, or consists of one or more of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the third monomer is chemically different (e.g., a different chemical species) from the carboxylic acid of the first monomer and the second monomer. For example, the third monomer may include itaconic acid or crotonic acid and the first and second monomers may include AA, MA, or MAA, respectively.


The third monomer may constitute about 10 mol % of the terpolymer or less, such as about 0.01 mol % to about 10 mol %, about 1 mol % to about 9 mol %, about 2 mol % to about 8 mol %, about 3 mol % to about 7 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 0.01 mol % to about 5 mol %, about 1 mol % to about 5 mol %, about 1 mol % to about 3 mol %, about 1.5 mol % to about 3.5 mol %, about 3 mol % to about 5 mol %, about 5 mol % to about 8 mol %, about 8 mol % to about 10 mol %, about 1.8 mol %, about 2 mol %, about 3 mol %, about 5 mol %, about 10 mol %, about 7 mol % or less, about 5 mol % or less, or about 3 mol % of the terpolymer or less.


The third monomer may constitute about 10 wt % of the terpolymer or less, such as about 0.01 wt % to about 10 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 0.01 wt % to about 5 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 5 wt %, about 10 wt %, about 7 wt % of the terpolymer or less, or about 5 wt % of the terpolymer or less.


In an embodiment, the first monomer of the terpolymer comprises, consists essentially of, or consists of one or more of AA, MA, MAA, or residues thereof. In an embodiment, the second monomer of the terpolymer comprises, consists essentially of, or consists of one or more of MA, MAA, ATBS, or residues thereof, where the second monomer is chemically different from the first monomer. In an embodiment, the third monomer of the terpolymer comprises, consists essentially of, or consists of one or more of ATBS, sulfostyrene, methallylsulfonic acid, tert-butylacrylamide, dimethylacrylamide, itaconic acid, crotonic acid, or residues thereof, where the third monomer is chemically different from the second monomer and the first monomer. In an embodiment, the terpolymer comprises, consists essentially of, or consists of one or more of AA residue, MA or MAA residue, and ATBS residue. The AA residue may constitute about 90 mol % to about 98 mol % of the terpolymer, the MA residue may constitute about 1 mol % to about 7 mol % of the terpolymer, and the ATBS residue may constitute at least a portion of the balance of the terpolymer (e.g., about 1 mol % to about 7 mol %). The AA residue may constitute about 90 mol % to about 98 mol % of the terpolymer, the MAA residue may constitute about 1 mol % to about 7 mol % of the terpolymer, and the ATBS residue may constitute at least a portion of the balance of the terpolymer (e.g., about 1 mol % to about 7 mol %). In an embodiment, the terpolymer comprises, consists essentially of, or consists of one or more of AA residue, ATBS residue, and itaconic acid or crotonic acid residue. The AA residue may constitute about 90 mol % to about 98 mol % of the terpolymer, the ATBS residue may constitute about 1 mol % to about 7 mol % of the terpolymer, and the itaconic acid or crotonic residue may constitute at least a portion of the balance of the terpolymer (e.g., about 1 mol % to about 7 mol %). In an embodiment, the terpolymer comprises, consists essentially of, or consists of one or more of AA residue, ATBS residue, and tert-butylacrylamide residue. The AA residue may constitute about 90 mol % to about 98 mol % of the terpolymer, the ATBS residue may constitute about 1 mol % to about 7 mol % of the terpolymer, and the tert-butylacrylamide residue may constitute at least a portion of the balance of the terpolymer (e.g., about 1 mol % to about 7 mol %). In an embodiment, the terpolymer comprises, consists essentially of, or consists of AA residue, ATBS residue, and dimethyl acrylamide residue. The AA residue may constitute about 90 mol % to about 98 mol % of the terpolymer, the ATBS residue may constitute about 1 mol % to about 7 mol % of the terpolymer, and the dimethylacrylamide residue may constitute at least a portion of the balance of the terpolymer (e.g., about 1 mol % to about 7 mol %).


As discussed in detail below, the terpolymer can exhibit any of a wide range of molecular weights. As discussed in more detail below, the terpolymer can be mixed (e.g., at least partially dissolved, dispersed, or suspended) in water and/or a water source in any of a wide range of dosages. Without wishing to be limited by theory, we believe that during use, one or more moieties (e.g., hydrophobic moieties) present in the polymer may bond to a metal surface forming a passivating film on the metal surface and/or could act as a cathodic or anodic inhibitor, or otherwise render corrodents substantially ineffective or very slow to corrode equipment in water containing systems, such as cooling, desalination, or drilling equipment. As discussed in detail below, the terpolymers herein may also include a tagging agent (e.g., fluorescent tag or marker).


Tetrapolymers


In some embodiments, the corrosion inhibiting polymer composition is a tetrapolymer (e.g., quaterpolymer or quadpolymer). The tetrapolymer may comprise, consist essentially of, or consist of a first monomer including a carboxylic acid or a residue thereof; a second monomer including a sulfonated acid or a residue thereof, or a second, chemically different carboxylic acid or a residue thereof; a third monomer including a sulfonated acid or a residue thereof, a third, chemically different carboxylic acid (e.g., chemically differing from the first and second carboxylic acids) or a residue thereof, or an alkylated molecule or a residue thereof and a fourth monomer including an alkylated molecule or a residue thereof, or a fourth, chemically different carboxylic acid or a residue thereof. In an embodiment, each of the first, second, third, and fourth monomers are chemically different from each other.


The first monomer may comprise, consist essentially of, or consist of a (first) carboxylic acid or a residue thereof substantially as described above with respect to the copolymer or terpolymer. For example, suitable carboxylic acids may include, by way of example, an alkyl acrylic acid such as AA, MA, or MAA, or any other unsaturated carboxylic acid capable of polymerizing; or any other unsaturated molecule having at least one carboxyl moiety; a salt of any of the foregoing, or a conjugate base of any of the foregoing. In some embodiments, the first monomer includes a residue of one of any of the carboxylic acids disclosed herein, a salt thereof, or a conjugate base thereof. Carboxylic acid salts may include Lithium, Beryllium, Sodium, Magnesium, Potassium, Calcium, Zinc, etc., salts.


The first monomer may constitute about 55 mol % of the tetrapolymer or more, such as about 80 mol % or more, about 55 mol % to about 99 mol %, about 65 mol % to about 95 mol %, about 75 mol % to about 94 mol %, about 80 mol % to about 95 mol %, about 85 mol % to about 93 mol %, about 90 mol % to about 98 mol %, about 80 mol % to about 90 mol %, about 90 mol % to about 95 mol %, about 85 mol % to about 90 mol %, about 91 mol % to about 95 mol %, about 65 mol %, about 75 mol %, about 85 mol %, about 90 mol %, about 93 mol %, about 95 mol %, about 93 mol % or less, or about 95 mol % of the tetrapolymer or less.


The first monomer may constitute about 50 wt % of the tetrapolymer or more, such as about 75 wt % or more, about 50 wt % to about 95 wt %, about 60 wt % to about 90 wt %, about 70 wt % to about 85 wt %, about 75 wt % to about 90 wt %, about 80 wt % to about 95 wt %, about 85 wt % to about 90 wt %, about 75 wt % to about 85 wt %, about 78 wt % to about 82 wt %, about 83 wt % to about 87 wt %, about 88 wt % to about 92 wt %, about 60 wt %, about 70 wt %, about 80 wt %, about 85 wt %, about 90 wt %, or about 85 wt % of the tetrapolymer or less.


In an embodiment, the second monomer of the tetrapolymer comprises, consists essentially of, or consists of a sulfonated acid, a (second) carboxylic acid, or a residue of any of the foregoing, where the second monomer is chemically different from the first monomer. The sulfonated acid (e.g., sulfonic acids) may include a sulfonate moiety, a salt thereof, or a conjugate base thereof as described above with respect to copolymer and terpolymer. For example, suitable sulfonated acids may include ATBS, sulfostyrene, vinylsulfonic acid, or methallylsulfonic acid, any other sulfonated acid, a salt of the foregoing, or a conjugate base of the foregoing, as described above.


In an embodiment, the second monomer comprises, consists essentially of, or consists of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the second monomer is chemically different from the carboxylic acid of the first monomer. For example, the second monomer may comprise, consist essentially of, or consist of one or more of MA or MAA residue while the first monomer includes AA residue, or vice versa.


The second monomer may constitute about 20 mol % of the tetrapolymer or less, such as about more than about 0.01 mol % to about 20 mol %, about 0.01 mol % to about 15 mol %, about 0.01 mol % to about 10 mol %, about 0.01 mol % to about 5 mol %, about 2 mol % to about 10 mol %, about 3 mol % to about 8 mol %, about 5 mol % to about 15 mol %, about 8 mol % to about 12 mol %, about 1 mol % to about 4 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, 0.01 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 2 mol % to about 4 mol %, about 3 mol % to about 5 mol %, about 5 mol % to about 8 mol %, about 8 mol % to about 10 mol %, about 10 mol % to about 15 mol %, about 1 mol %, about 2 mol %, about 3 mol %, about 3.5 mol %, about 4 mol %, about 5 mol %, about 10 mol % or less, or about 5 mol % of the tetrapolymer or less.


The second monomer may constitute about 20 wt % of the tetrapolymer or less, such as about more than about 0.01 wt % to about 20 wt %, 0.01 wt % to about 15 wt %, 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 2 wt % to about 18 wt %, about 3 wt % to about 12 wt %, about 5 wt % to about 15 wt %, about 8 wt % to about 12 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, 0.01 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 10 wt % to about 15 wt %, about 10 wt % or less, or about 5 wt % of the tetrapolymer or less.


In an embodiment, the third monomer of the tetrapolymer comprises, consists essentially of, or consists of one of a sulfonated acid, a (third) carboxylic acid, an alkylated molecule or a residue of any of the foregoing, where the third monomer is chemically different from the first monomer and the second monomer. The sulfonated acid may include a sulfonate moiety, a salt thereof, or a conjugate base thereof, as described above. The an alkylated molecule or monomer may comprise, consist essentially of, or consist of a molecule having at least one alkyl moiety, a residue thereof, a salt thereof, or a conjugate base thereof, as described above with respect to the terpolymer. The third monomer may comprise, consist essentially of, or consist of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the third monomer is chemically different from the carboxylic acid of the first monomer and the second monomer. For example, the third monomer may include itaconic acid or crotonic acid and the first and second monomers may include AA and MA, respectively.


The third monomer may constitute about 10 mol % of the tetrapolymer or less, such as about 0.01 mol % to about 10 mol %, about 1 mol % to about 8 mol %, about 2 mol % to about 6 mol %, about 1 mol % to about 3 mol %, about 3 mol % to about 5 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 3 mol % to about 7 mol %, about 7 mol % to about 10 mol %, about 1 mol %, about 1.8 mol %, about 2 mol %, about 3 mol %, about 5 mol %, about 10 mol %, about 7 mol % or less, about 5 mol % or less, or about 3 mol % of the tetrapolymer or less.


The third monomer may constitute about 10 wt % of the tetrapolymer or less, such as about 0.01 wt % to about 10 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 5 wt %, about 10 wt %, about 7 wt % or less, or about 5 wt % of the tetrapolymer or less.


In an embodiment, the fourth monomer of the tetrapolymer comprises, consists essentially of, or consists of a (fourth) carboxylic acid, an alkylated molecule, or a residue of any of the foregoing, where the fourth monomer is chemically different from the first, second, and third monomers. In an embodiment, the alkylated molecule includes at least one alkyl moiety, a residue thereof, a salt thereof, or a conjugate base thereof, as described above.


In an embodiment, the fourth monomer comprises, consists essentially of, or consists of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the fourth monomer is chemically different from the carboxylic acid of the first, second, and third monomers. For example, the fourth monomer may include itaconic acid or crotonic acid and one or more of the first, second, and third monomers may include or consist of AA, MA, and/or MAA, respectively.


The fourth monomer may constitute about 10 mol % of the tetrapolymer or less, such as about 0.01 mol % to about 10 mol %, 0.01 mol % to about 5 mol %, about 1 mol % to about 7 mol %, about 2 mol % to about 6 mol %, about 3 mol % to about 5 mol %, about 1 mol % to about 4 mol %, about 1 mol % to about 3 mol %, about 1.5 mol % to about 3 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 3 mol % to about 5 mol %, about 5 mol % to about 8 mol %, about 8 mol % to about 10 mol %, about 5 mol %, about 10 mol %, about 7 mol % or less, about 5 mol % or less, or about 3 mol % of the tetrapolymer or less.


The fourth monomer may constitute about 10 wt % of the tetrapolymer or less, such as about 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 5 wt %, about 10 wt %, about 7 wt % or less, or about 5 wt % of the tetrapolymer or less.


In an embodiment, the first monomer of the tetrapolymer comprises, consists essentially of, or consists of one of AA, MA, MAA, or residues thereof. The second monomer of the tetrapolymer comprises, consists essentially of, or consists of one of MA, MAA, ATBS, or residues thereof, where the second monomer is chemically different from the first monomer. The third monomer of the tetrapolymer may comprises, consists essentially of, or consists of one of ATBS, sulfostyrene, methallylsulfonic acid, tert-butylacrylamide, dimethylacrylamide, itaconic acid, crotonic acid or residues thereof, where the third monomer is chemically different from the second monomer and the first monomer. In an embodiment, the fourth monomer of the tetrapolymer is one of tert-butylacrylamide, dimethylacrylamide, itaconic acid, crotonic acid, or residues thereof, where the fourth monomer is chemically different from the first, second, and third monomers.


In an embodiment, the tetrapolymer comprises, consists essentially of, or consists of AA residue, MA residue, ATBS residue, and tert-butylacrylamide residue. The AA residue may constitute about 85 mol % to about 95 mol % of the tetrapolymer, the MA residue may constitute about 1 mol % to about 7 mol % of the tetrapolymer, the ATBS residue may constitute about 1 mol % to about 7 mol % of the tetrapolymer, and the tert-butylacrylamide residue may constitute at least a portion of the balance of the tetrapolymer (e.g., about 1 mol % to about 7 mol %). The AA residue may constitute about 93 mol % of the tetrapolymer, the MA residue may constitute about 2 mol % of the tetrapolymer, the ATBS residue may constitute about 3.5 mol % of the tetrapolymer, and the tert-butylacrylamide residue may constitute about 1.5 mol % of the tetrapolymer.


In an embodiment, the tetrapolymer comprises, consists essentially of, or consists of one or more of AA residue, ATBS residue, itaconic acid or crotonic acid residue, and tert-butylacrylamide residue. The AA residue may constitute about 80 mol % to about 95 mol % of the tetrapolymer, the ATBS residue may constitute about 1 mol % to about 7 mol % of the tetrapolymer, the itaconic acid or crotonic acid residue may constitute about 1 mol % to about 7 mol % of the tetrapolymer, and the tert-butylacrylamide residue may constitute about 1 mol % to about 7 mol % of the tetrapolymer. An any of the above embodiments, MA or MAA may be used in place of the AA, where the MA is chemically different from each of the monomers in the tetrapolymers. In an embodiment, the AA residue may constitute about 75 mol % to about 80 mol % of the tetrapolymer, the ATBS residue may constitute about 7 mol % to about 12 mol % of the tetrapolymer, the itaconic acid or crotonic acid residue may constitute about 7 mol % to about 12 mol % of the tetrapolymer, and the tert-butylacrylamide residue may constitute about 1 mol % to about 5 mol % of the tetrapolymer. For example, the AA residue may constitute about 78 mol % of the tetrapolymer, the ATBS residue may constitute about 10% of the tetrapolymer, the itaconic acid or crotonic acid residue may constitute about 10 mol % of the tetrapolymer, and the tert-butylacrylamide residue may constitute about 2 mol % of the tetrapolymer. In any of the above embodiments, MA or MAA may be used in place of the AA, where the MA is chemically different from each of the monomers in the tetrapolymers.


As discussed in detail below, the tetrapolymer can exhibit any of a wide range of molecular weights. As discussed in more detail below, the tetrapolymer can be mixed in water and/or a water source in any of a wide range of dosages. Without wishing to be limited by theory, we believe that during use, one or more moieties present in the polymer (e.g., one or more hydrophobic moieties) may bond to a metal surface forming a passivating film on the metal surface and/or could act as a cathodic or anodic inhibitor, or otherwise render corrodents substantially ineffective or very slow to corrode equipment in water containing systems, such as cooling, desalination, or drilling equipment. As explained in detail below, the tetrapolymers herein may also include a fluorescent tag or marker.


Pentapolymers


In some embodiments, the corrosion inhibiting polymer composition is a pentapolymer. The pentapolymer may comprise, consist essentially of, or consist of a first monomer including a carboxylic acid or a residue thereof; a second monomer including a second, chemically different carboxylic acid or a residue thereof; a third monomer including an alkylated molecule or a residue thereof; a fourth monomer including a fourth, chemically different carboxylic acid or a residue thereof; and a fifth monomer including a fifth, chemically different carboxylic acid or a residue thereof (“fourth” and “fifth” correspond to the monomeric designation of the monomer but not necessarily the total amount of carboxylic acids in the polymer). In an embodiment, each of the first, second, third, fourth, and fifth monomers are chemically different from each other.


The first monomer may comprise, consist essentially of, or consist of a (first) carboxylic acid or a residue thereof substantially as described above with respect to the copolymer, terpolymer, or tetrapolymer. For example, suitable carboxylic acids may include, any carboxylic acid disclosed herein, such as AA, MA, or MAA, or any other unsaturated carboxylic acid capable of polymerizing; or any other molecule having at least one carboxyl moiety; a salt of any of the foregoing, or a conjugate base of any of the foregoing. In some embodiments, the first monomer includes a residue of one of any of the carboxylic acids disclosed herein, a salt thereof, or a conjugate base thereof. Carboxylic acid salts may include Lithium, Beryllium, Sodium, Magnesium, Potassium, Calcium, Zinc, etc., salts.


The first monomer may constitute about 55 mol % of the pentapolymer or more, such as about 75 mol % or more, about 55 mol % to about 97 mol %, about 70 mol % to about 95 mol %, about 80 mol % to about 90 mol %, about 85 mol % to about 95 mol %, about 90 mol % to about 96 mol %, about 92 mol % to about 96 mol %, about 80 mol % to about 95 mol %, about 78 mol % to about 82 mol %, about 83 mol % to about 87 mol %, about 88 mol % to about 92 mol %, about 60 mol %, about 70 mol %, about 80 mol %, about 85 mol %, about 90 mol %, about 91 mol %, about 93 mol %, about 95 mol %, about 96 mol %, or about 95 mol % of the pentapolymer or less.


The first monomer may constitute about 50 wt % of the pentapolymer or more, such as about 75 wt % or more, about 50 wt % to about 95 wt %, about 60 wt % to about 90 wt %, about 70 wt % to about 85 wt %, about 75 wt % to about 90 wt %, about 80 wt % to about 95 wt %, about 85 wt % to about 90 wt %, about 75 wt % to about 85 wt %, about 78 wt % to about 82 wt %, about 83 wt % to about 87 wt %, about 88 wt % to about 92 wt %, about 60 wt %, about 70 wt %, about 80 wt %, about 85 wt %, about 90 wt %, or about 85 wt % of the pentapolymer or less.


In an embodiment, the second monomer of the pentapolymer comprises, consists essentially of, or consists of another (second) carboxylic acid or a residue of thereof, where the second monomer is chemically different from the first monomer. The second monomer may include any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the second monomer is chemically different from the carboxylic acid of the first monomer. For example, the second monomer may comprise, consist essentially of, or consist of MA or MAA residue while the first monomer includes AA residue, or vice versa.


The second monomer may constitute about 20 mol % of the pentapolymer or less, such as about more than about 0.01 mol % to about 20 mol %, about 0.01 mol % to about 15 mol %, about 0.01 mol % to about 10 mol %, about 0.01 mol % to about 5 mol %, about 1 mol % to about 3 mol %, about 1 mol % to about 7 mol %, about 2 mol % to about 8 mol %, about 3 mol % to about 7 mol %, about 5 mol % to about 15 mol %, about 8 mol % to about 12 mol %, about 1 mol % to about 4 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, 1.5 mol % to about 4 mol %, about 1 mol % to about 5 mol %, about 2 mol % to about 4 mol %, about 3 mol % to about 5 mol %, about 5 mol % to about 8 mol %, about 8 mol % to about 10 mol %, about 10 mol % to about 15 mol %, about 1 mol %, about 1.5 mol %, about 2 mol %, about 3 mol %, about 3.5 mol %, about 4 mol %, about 5 mol %, about 10 mol % or less, or about 5 mol % of the pentapolymer or less.


The second monomer may constitute about 10 wt % of the pentapolymer or less, such as about 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 5 wt %, about 10 wt %, about 7 wt % or less, or about 5 wt % of the pentapolymer or less.


In an embodiment, the third monomer of the pentapolymer comprises, consists essentially of, or consists of an alkylated molecule or a residue of thereof. The alkylated molecule may be similar or identical to the alkylated molecule(s) described above with respect to the terpolymer or tetrapolymer. For example, suitable alkylated molecules may include hydrophobic acrylamides or derivatives thereof, such as methacrylamide, N-tert-butylacrylamide, dimethylacrylamide, residues of any of the foregoing, or any other alkylated molecule or residue thereof disclosed herein.


In an embodiment, the third monomer constitutes about 10 mol % of the pentapolymer or less, such as about 0.01 mol % to about 10 mol %, 0.01 mol % to about 5 mol %, about 1 mol % to about 7 mol %, about 2 mol % to about 6 mol %, about 3 mol % to about 5 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 1 mol % to about 4 mol %, about 1 mol % to about 3 mol %, about 3 mol % to about 5 mol %, about 5 mol % to about 8 mol %, about 8 mol % to about 10 mol %, about 1 mol %, about 1.2 mol %, about 1.5 mol %, about 1.8 mol %, about 2 mol %, about 3 mol %, about 4 mol %, about 5 mol %, about 10 mol %, about 7 mol % or less, or about 5 mol % of the pentapolymer or less.


In an embodiment, the third monomer constitutes about 10 wt % of the pentapolymer or less, such as about 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 5 wt % to about 8 wt %, about 8 wt % to about 10 wt %, about 5 wt %, about 10 wt %, about 7 wt % or less, or about 5 wt % of the pentapolymer or less.


In an embodiment, the fourth monomer comprises, consists essentially of, or consists of any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the fourth monomer is chemically different from the carboxylic acid of the first monomer, the second monomer, and the third monomer. For example, the fourth monomer may include itaconic acid or crotonic acid and one or more of the first, second, and third monomers may include or consist of AA, MA, and/or MAA, respectively.


The fourth monomer may constitute about 10 mol % of the pentapolymer or less, such as about 0.01 mol % to about 10 mol %, 0.01 mol % to about 5 mol %, about 1 mol % to about 7 mol %, about 2 mol % to about 6 mol %, about 1 mol % to about 3 mol %, about 2 mol % to about 4 mol %, about 3 mol % to about 5 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 1 mol %, about 1.2 mol %, about 1.5 mol %, about 1.8 mol %, about 2 mol %, about 3 mol %, about 3.5 mol %, about 4 mol %, about 5 mol %, about 10 mol %, about 5 mol % or less, or about 3 mol % of the pentapolymer or less.


The fourth monomer may constitute about 10 wt % of the pentapolymer or less, such as about 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 2 wt % to about 4 wt %, about 3 wt %, about 5 wt %, about 10 wt %, about 5 wt % or less, or about 3 wt % of the pentapolymer or less.


In an embodiment, the fifth monomer comprises, consists essentially of, or consists of a (fifth) carboxylic acid such as any of the carboxylic acids or residues thereof disclosed above with respect to the first monomer, so long as the carboxylic acid of the fifth monomer is chemically different from a carboxylic acid of the first monomer, the second monomer, the third monomer, and/or the fourth monomer. For example, the fifth monomer may include MAA and one or more of the first, second, third, and fourth monomers may include or consist of AA, MA, itaconic acid, or crotonic acid, respectively.


The fifth monomer may constitute about 10 mol % of the pentapolymer or less, such as about 0.01 mol % to about 10 mol %, 0.01 mol % to about 5 mol %, about 1 mol % to about 7 mol %, about 2 mol % to about 6 mol %, about 1 mol % to about 3 mol %, about 3 mol % to about 5 mol %, about 4 mol % to about 6 mol %, about 5 mol % to about 10 mol %, about 1 mol % to about 5 mol %, about 6 mol % to about 8 mol %, about 1 mol %, about 1.5 mol %, about 2 mol %, about 2.5 mol %, about 3 mol %, about 3.5 mol %, about 4 mol %, about 5 mol %, about 7 mol %, about 10 mol %, about 8 mol % or less, about 5 mol % or less, or about 3 mol % of the pentapolymer or less.


The fifth monomer may constitute about 10 wt % of the pentapolymer or less, such as about 0.01 wt % to about 10 wt %, 0.01 wt % to about 5 wt %, about 1 wt % to about 9 wt %, about 2 wt % to about 8 wt %, about 3 wt % to about 7 wt %, about 4 wt % to about 6 wt %, about 5 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 3 wt % to about 5 wt %, about 6 wt % to about 8 wt %, about 3 wt %, about 5 wt %, about 7 wt %, about 10 wt %, about 8 wt % or less, or about 7 wt % of the pentapolymer or less.


In an embodiment, a sulfonated acid may be used in place of any of the above listed second, third, fourth, or fifth monomers in the pentapolymer. For example, ATBS may be used instead of the second carboxylic acid of the second monomer as described above. The sulfonated acid may be present in the same mol % or wt % as the respective monomer it substitutes for, as respectively disclosed above. For example, if ATBS were used in place of the second carboxylic acid, the ATBS may be present in the same mol % or wt % as the second carboxylic acid of the second monomer.


In an embodiment, the pentapolymer comprises, consists essentially of, or consists of AA residue, MA residue, tert-butylacrylamide residue, itaconic acid or crotonic acid residue, and methacrylic acid residue. The AA residue may constitute about 80 mol % to about 96 mol % of the pentapolymer, the MA residue may constitute about 1 mol % to about 7 mol % of the pentapolymer, the tert-butylacrylamide residue may constitute about 1 mol % to about 7 mol % of the pentapolymer, the itaconic acid or crotonic acid residue may constitute about 1 mol % to about 5 mol % of the pentapolymer, and the MAA residue may constitute at least a portion of the balance of the pentapolymer (e.g., about 1 mol % to about 10 mol %). In an embodiment, the AA residue constitutes about 90 mol % of the pentapolymer, the MA residue constitutes about 3 mol % of the pentapolymer, the tert-butylacrylamide residue constitutes about 1.5 mol % of the pentapolymer, the itaconic acid or crotonic acid residue constitutes about 2 mol % of the pentapolymer, and the MAA residue constitutes about 3.5 mol % of the pentapolymer.


As discussed in detail below, the pentapolymer can exhibit any of a wide range of molecular weights. As discussed in more detail below, the pentapolymer can be mixed water and/or in a water source in any of a wide range of dosages. Without wishing to be limited by theory, we believe that during use, one or more moieties (e.g., hydrophobic moieties) present in the polymer may bond to a metal surface forming a passivating film on the metal surface and/or could act as a cathodic or anodic inhibitor, or otherwise render corrodents substantially ineffective or very slow to corrode equipment in water containing systems, such as cooling, desalination, or drilling equipment. In some embodiments and as explained in detail below, a fluorescent tag or marker may be added to the pentapolymer.


Polymer Composition Characteristics


The embodiments of polymers (e.g., corrosion inhibiting polymer compositions) disclosed herein exclude phosphorous or phosphorous containing moieties. The above described polymers may substantially inhibit or prevent corrosion in water containing systems having low TDS water sources (e.g., less than about 4000 ppm, such as about 500 ppm to about 2550 ppm) and/or having high TDS water sources (e.g., about 4,000 ppm-to about 350,000). In some embodiments, the polymers described herein may inhibit corrosion without the use of phosphorous or phosphorous containing molecules or moieties therein. In some embodiments, the polymers described herein may be used to inhibit corrosion in combination with phosphorous or phosphorous containing molecules or moieties, such as a phosphonate or phosphate containing molecules, ions, or moieties. The polymers herein may be formed in a liquid, semi-liquid (e.g., gel), or solid form, depending on the specific polymer, monomeric make-up, and/or molecular weight thereof. The polymer solutions disclosed herein may exhibit a viscosity of about 100-200 cps as measured by a Brookfield viscometer at 25 degrees Celsius with a #3 spindle at 30 rpm. The viscosity of any of the polymer compositions disclosed herein, prior to mixing in water and/or a water source, may be about 250 cps or less, such as about 50 cps to about 250 cps, about 100 cps to about 200 cps, about 120 cps to about 180 cps, about 140 cps, to about 160 cps, about 80 cps to about 120 cps, about 120 cps to about 150 cps, about 150 cps to about 180 cps, or about 180 cps to about 200 cps.


The molecular weight (Mw) of any of the polymers disclosed herein, prior to mixing in water and/or a water source, may be at least about 500 g/mol, such as about 500 g/mol to about 50,000 g/mol, about 1000 g/mol to about 20,000 g/mol, about 2,000 g/mol to about 12,000 g/mol, about 500 g/mol to about 3,000 g/mol, about 2,000 g/mol to about 8,000 g/mol, about 3,000 g/mol to about 6,000 g/mol, about 6,000 g/mol to about 9,000 g/mol, about 8,000 g/mol to about 10,000 g/mol, about 9,000 g/mol to about 12,000 g/mol, about 8,000 g/mol to about 15,000 g/mol, about 12,000 g/mol to about 15,000 g/mol, about 15,000 g/mol to about 20,000 g/mol, about 18,000 g/mol to about 22,000 g/mol, 15,000 g/mol to about 25,000 g/mol, about 20,000 g/mol to about 30,000 g/mol, about 30,000 g/mol to about 40,000 g/mol, about 40,000 g/mol to about 50,000 g/mol, or about 1,000 g/mol, about 2,000 g/mol, about 3,000 g/mol, about 4,000 g/mol, about 5,000 g/mol, about 7,000 g/mol, about 10,000 g/mol, about 11,000 g/mol, about 12,000 g/mol, about 14,000 g/mol, about 15,000 g/mol, about 18,000 g/mol, about 20,000 g/mol, about 22,000 g/mol, about 25,000 g/mol or less, or about 30,000 g/mol or less.


Additive Components


In some embodiments, any of the embodiments of polymers (e.g., corrosion inhibiting polymer compositions) disclosed herein can include one or more additive components, such as one or more metallic components or one or more additional polymers. The one or more metallic components can include at least one metal, such as at least on transition metal, at least one metalloid, ions thereof, alloys of any of the foregoing, or combinations of any of the foregoing. In some embodiments, the one or more metallic components can include a metal or an ion thereof such as aluminum, vanadium, chromium, manganese, zinc, molybdenum, tin, tantalum, tungsten, cerium, silicon, any other metal or metalloid, ions thereof (e.g., a molybdate, a silicate, etc.), or alloys of any of the foregoing. In some embodiments, the one or more metallic components can include a metal or an ion thereof such as one or more of zinc, tin, tungsten, molybdenum, cerium, silicon, tin, aluminum, or vanadium metal or an ion thereof, or alloys of any of the foregoing. Metal ions are generally added to the composition or provided in a composition in the form of a corresponding metal salt. Thus, for example, Zn as divalent ion is advantageously added to the composition or provided in a composition as zinc chloride, zinc acetate, zinc sulfate, or another zinc salt selected by the user. Where ppm of a metal ion is recited, the ppm refers to the metal ion itself. Thus, for example, 5 ppm of zinc is provided to a composition by adding an amount of the zinc salt corresponding to 5 ppm of the zinc cation.


In some embodiments, the corrosion inhibiting polymer mixture can be combined with one or more additional polymers or copolymers such as one or more oligomers of maleic acid, a homopolymer of acrylic acid, or copolymers of sulfonated monomers with acrylic acid. Such combinations can be about 1000:1 to about 1:1000 corrosion inhibiting polymer mixture to additional polymer or any other ranges therebetween, such as 1000 parts corrosion inhibiting polymer mixture to 1 part oligomer of maleic acid, or 1 part corrosion inhibiting polymer mixture to 1000 parts oligomer of maleic acid.


In some embodiments, each additive component or the sum of the one or more additive components can be present in the polymer mixture (or in some embodiments, the polymer composition) in a concentration of about 0.05 ppm to about 1000 ppm (e.g., 0.05 ppm to about 50 ppm) of the corrosion inhibiting polymer mixture, such as about 0.05 ppm to about 10 ppm, about 0.05 ppm to about 3 ppm, about 0.05 ppm to about 5 ppm, about 1 ppm to about 5 ppm, about 2 ppm to about 10 ppm, about 5 ppm to about 20 ppm, about 15 ppm to about 30 ppm, about 20 ppm to about 40 ppm, about 30 ppm to about 50 ppm, about 50 ppm to about 100 ppm, about 1 ppm to about 30 ppm, about 10 ppm to about 100 ppm, about 50 ppm to about 500 ppm, about 100 ppm to about 1000 ppm, less than about 1000 ppm, less than about 500 ppm, less than about 100 ppm, less than about 30 ppm, less than about 10 ppm, or less than about 5 ppm. The additive component(s) can be admixed with the corrosion inhibiting polymer mixture prior to application in the water containing system, contemporaneously therewith, or after addition of the corrosion inhibiting polymer composition into the water containing system.


Tagging Agents


In some embodiments, the polymers disclosed above include an additional tagging agent therein. For the purposes of categorizing polymers in this disclosure, such tagging agents are not counted as a monomeric unit of the polymer for determining the categorical name of said polymer. For example, a copolymer having AA, ATBS, and a tagging agent (e.g., a monomer capable of fluorescing) therein, is still referred to as a copolymer rather than adding the additional monomeric tagging agent for the purposes of the category/title and describing the polymer as a terpolymer.


In some embodiments, the corrosion inhibiting polymer compositions disclosed above are tagged (e.g., polymerized) with a tagging agent for monitoring the polymer composition in feedstocks and/or blowdown water (e.g., used coolant or produced water having the polymer therein). The tagging agent can be polymerized into any of the polymers disclosed herein. Suitable tagging agents may include one or more monomers that are naphthalene-containing, anthracene-containing, quinoline-containing, isoquinoline-containing, indole-containing, pyrene-containing, benzimidazole-containing, coumarin-containing, fluorescein-containing, quinoxaline-containing, xanthylium-containing, boron-dipyrromethene-containing, bimane-containing, rhodamine-containing, or naphthalimide-containing. Specific monomers that can be used to fluorescently tag a polymer include but are not limited to 4-methoxy-N-(3-N′,N′-dimethylaminopropyl)naphthalimide (quaternary salt), N-allyl-4-(2-N′,N′-dimethylaminoethoxy)naphthalimide (methyl sulfate quaternary salt), 4-methoxy-N-(3-N′,N′-dimethylaminopropyl) naphthalimide (allyl chloride quaternary salt), 5-allyloxy-4′-carboxy-1,8-naphthoylene-1′,2′-benzimidazole, 6-Vinylbenzyloxy-4′-carboxy-1,8-naphthoylene-1′,2′-benzimidazole, 4-methoxy-N-(3-N′,N′-dimethylaminopropyl)naphthalimide (2-hydroxy-3-allyloxypropyl quat), quaternary ammonium salt of dimethylaminopropylmethacrylamide and 2-(chloromethyl)quinoline, quaternary ammonium salt of dimethylaminopropylmethacrylamide and 9-(chloromethyl)anthracene, quaternary ammonium salt of dimethylaminopropylmethacrylamide and 2-(chloromethyl)benzimidazole, quaternary ammonium salt of dimethylaminopropylmethacrylamide and 4-(bromomethyl)pyrene, quaternary ammonium salt of dimethylaminopropylmethacrylamide and 1-(chloromethyl)naphthalene, any additional quaternary ammonium salt of dimethylaminopropylmethacrylamide and halo-alkyl derivative of the fluorescent chromophores previously listed, or any other fluorescent molecule capable of polymerizing with any of the above described corrosion inhibiting polymers. The tagging agent may constitute less than about 10 mol % of the any of the polymers disclosed herein, such as less than about 1 mol %, less than about 0.1 mol %, or less than about 0.01 mol % of the polymer. The tagging agent may constitute less than about 10 wt % of the any of the polymers disclosed herein, such as about 0.01 wt % to about 10 wt %, about 1 wt % to about 3 wt %, about 4 wt % to about 6 wt %, about 7 wt % to about 10 wt %, 2 wt % to about 5 wt %, less than about 5 wt %, less than about 3 wt %, less than about 1 wt %, about 0.01 wt % to about 1 wt %, about 0.01 wt % to about 0.1 wt %, or less than about 0.1 wt % of the polymer.


When the corrosion inhibiting polymers herein are tagged with a tagging agent, one can determine how much corrosion inhibiting polymer composition is being delivered in the water source and/or how much corrosion inhibiting polymer composition is being exhausted during use. A fluorometer, UV spectrometer, or other fluorescent material detecting apparatus may be used to determine the amount of fluorescent tag in a water source, and by extension, the amount of tagged polymer therein. Such equipment can be used to constantly monitor the concentration of a tagged polymer in a system or can be used to monitor said concentrations on demand (e.g., randomly or at selected intervals).


Additional Monomers


In some embodiments, the corrosion inhibiting polymer compositions disclosed above alternatively or additionally include one or more additional monomers. Additional monomers may include hydrogen bonding or cationic monomers. For example, a polymer composition may additionally include a monomer or residue formed from a hydrogen bonding molecule and/or a cationic molecule. Such compositions may include 2-10 different monomers. Suitable hydrogen bonding molecules include, by way of example, acrylamide, methacrylamide, N-vinyl formamide, methylene bis acrylamide, triallylamine and acid salts thereof, ethylene glycol dimethacrylate, hydroxymethylacrylate, hydroxyethylacrylate, hydroxypropylacrylate, hydroxypropylmethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethylacrylate, polyethylene glycol dimethacrylate, glycidyl methacrylate, vinyl alcohol, vinyl acetate, derivatives of any of the foregoing, salts of any of the foregoing, or analogues of any of the foregoing. Suitable cationic molecules include, by way of example, dimethylaminoethyl acrylate methyl chloride tetranary salts, dimethylaminoethyl acrylate benzyl chloride tetranary salts, dimethylaminoethyl acrylate methyl sulfate tetranary salt, dimethylaminoethyl methacrylate methyl sulfate tetranary salt, dimethylaminoethyl acrylamide methyl sulfate tetranary salts, dimethylaminopropyl acrylamide methyl sulfate tetranary salts, dimethylaminopropyl methacrylamide methyl sulfate tetranary salts, diallyldimethyl ammonium chloride, dimethylaminoethyl methacrylate methyl chloride tetranary salt, dimethylaminoethyl methacrylate benzyl chloride tetranary salt, methacrylamidopropyl trimethyl ammonium chloride, acrylamidopropyl trimethyl ammonium chloride, dissociated species of any of the foregoing, or analogues of any of the foregoing. In some embodiments, any of the above listed species may be used to supply a polymerized monomer having a desired moiety (e.g., carboxylate groups) to the polymer composition. One or more of the above additional monomer species may be used in place of or in addition to any of the first, second, third, fourth, or fifth monomers disclosed herein. The additional monomers may be about 5 mol % or less of the polymer composition, such as 4 mol % or less, 3 mol %, or less, 2 mol % or less, or about 0.01 mol % to about 5 mol %, or more than about 1 mol % of the polymer composition including the same.


Polymer Mixtures


The corrosion inhibiting polymers disclosed herein may be mixed in water (e.g., tap or distilled water) and/or a water source to form a corrosion inhibiting polymer mixture to inhibit corrosion (e.g., pitting, oxidation, or erosion of a material due to chemical interactions), such as on one or more surfaces that contact the water source. The water source may include a low TDS water source (e.g., having a TDS content below 4000 ppm) such as soft water, balanced water, high-chloride/sulfate water, cooling water (e.g., a low TDS water source used to cool a system and that has not been concentrated to have a TDS above 4000 ppm), municipal water (e.g., potable water). In some embodiments, the water source may additionally or alternatively include sea water, connate, produced water, brackish water, brine, a synthetic version of any of the foregoing, combinations of any of the foregoing, or any other water source having a high TDS content (e.g., about 4000 ppm to about 350,000 ppm). In some embodiments, a water source can include TDS levels higher than 4,000 ppm, such as about 5,000 ppm or more (e.g., brackish water), about 10,000 ppm or more, about 15,000 ppm or more (e.g., saline water), about 30,000 ppm or more (e.g., salt water), or about 40,000 ppm or more (e.g., brine). In some embodiments, a water source (e.g., soft water) includes concentrations of certain dissolved solids, such as dissolved solids likely to form scales, cause corrosion, or solids having corrodent components likely to induce corrosion as disclosed herein. For example, the water source may include at least about 400 ppm of calcium, at least about 390 ppm of potassium, at least about 1200 ppm of magnesium, and/or identical ppm dosages of counter-ions of any of the foregoing (e.g., chloride, fluoride, sulfate, or ions) such as in seawater. The polymers disclosed herein may be particularly useful in inhibiting corrosion in soft water, balanced water, high-chloride/sulfate water, or any other water source having corrodents therein. Some water sources may have varying concentrations of different dissolved solids than soft water, balanced water, or high-chloride/sulfate water.


The water source may include one or more corrodents therein, wherein the one or more corrodents comprises, consists essentially of, or consists of carbon dioxide, hydrogen sulfide, organosulfur compounds, metal cations, metal complexes such as aqueous metal cations, metal chelates and/or organometallic complexes, aluminum ions, ammonium ions, barium ions, chromium ions, cobalt ions, cuprous ions, cupric ions, calcium ions, ferrous ions, ferric ions, hydrogen ions, lead ions, magnesium ions, manganese ions, molybdenum ions, nickel ions, potassium ions, sodium ions, strontium ions, titanium ions, uranium ions, vanadium ions, zinc ions, bromide ions, carbonate ions, chlorate ions, chloride ions, chlorite ions, dithionate ions, fluoride ions, hypochlorite ions, iodide ions, nitrate ions, nitrite ions, oxide ions, perchlorate ions, peroxide ions, phosphate ions, phosphite ions, sulfate ions, sulfide ions, sulfite ions, hydrogen carbonate ions, hydrogen phosphate ions, hydrogen phosphite ions, hydrogen sulfate ions, hydrogen sulfite ions, carbonic acid, hydrochloric acid, nitric acid, sulfuric acid, nitrous acid, sulfurous acid, peroxy acids, phosphoric acid, ammonia, bromine, carbon dioxide, chlorine, chlorine dioxide, fluorine, hydrogen chloride, hydrogen sulfide, iodine, nitrogen dioxide, nitrogen monoxide, oxygen, ozone, sulfur dioxide, hydrogen peroxide, polysaccharide, or combinations thereof. In embodiments, the one or more corrodents comprises insoluble particulates such as metal oxides, sands, clays, silicon dioxide, titanium dioxide, muds, and other insoluble inorganic and/or organic particulates, which in embodiments act as abrasives when entrained in a water flow contacting a metal. In embodiments, the one or more corrodents comprises, consists of, or consists essentially of an oxidizing agent. Each corrodent or the total amount of one or more corrodents in the water source may be present in a concentration of at least about 10 ppm, such as at least about 50 ppm, at least about 100 ppm, at least about 300 ppm, at least about 500 ppm, at least about 1000 ppm, at least about 2000 ppm, at least about 5000 ppm, at least about 10,000 ppm, at least about 20,000 ppm, or less than about 100,000 ppm. For example, the water source can include oxygen, sulfur, corrodent(s) containing one or more forms of the same (e.g., sulfides), or any other corrodent(s) in a concentration of about 100 ppm to about 350,000 ppm, about 200 ppm to about 20,000 ppm, about 500 ppm to about 100,000 ppm, about 10 ppm to about 10,000 ppm, about 100 ppm to about 1000 ppm, about 50 ppm to about 500 ppm, or less than about 5000 ppm. In embodiments, the corrodent comprises, consists of, or consists essentially of a chelating agent. In embodiments, the corrodent comprises an alcohol. In embodiments, the corrodent comprises an organochlorine compound. In embodiments, the produced water comprises, between 1000 ppm and 200000 ppm of chloride ions. In embodiments, the one or more corrodents comprises, consists of, or consists essentially of an acid. In embodiments, the one or more corrodents comprises, consists of, or consists essentially of an alkali.


In any of the embodiments, the pH of the water source is between 7 and 14. In embodiments, the pH of the water source is between about 7 and about 10. In embodiments, the pH of the water source is between about 10 and 14. In embodiments, the pH of the water source is between about 9 and about 11. In embodiments, the pH of the water source is between about 7 and about 9, such as between about 7 and about 8. In embodiments, the pH of the water source is between about 8 and about 9. In embodiments, the pH of the water source is between about 9 and about 10. In embodiments, the pH of the water source is between about 10 and about 11. In embodiments, the pH of the water source is between about 11 and about 12. In embodiments, the pH of the water source is between about 12 and about 13. In embodiments, the pH of the water source is between about 13 and 14. In embodiments, the pH of the water source is between 0 and 7. In embodiments, the pH of the water source is between about 1 and about 6. In embodiments, the pH of the water source is between 5 and 6. In embodiments, the pH of the water source is between 4 and 5. In embodiments, the pH of the water source is between 3 and 4. In embodiments, the pH of the water source is between 2 and 3. In embodiments, the pH of the water source is between 1 and 2. In embodiments, the pH of the water source is between 0 and 1.


Corrosion may be due to corrosive chemical(s) and/or conditions, such as the presence of basic or acidic chemicals and/or conditions, the presence or absence of oxidizers, the presents or absence of reducers, including the presence of components such as metals, alkaline metals, or alkaline earth metals in solution or solid form (e.g., suspended and/or dissolved solids) and counter ions thereof (e.g., oxides, sulfides, carbonates, bicarbonates, sulfates, bisulfates, phosphates, bisphosphates, phosphates, hydroxides, etc.) in the water source. For example, seawater may have a relatively high concentration of calcium and carbonate ions as compared to freshwater, whereby use of untreated seawater in a water containing system may result in relatively greater amounts of corrosion on the equipment that contact the seawater, such as due to under deposit corrosion or microbial corrosion due in part to scaling and/or basic or acidic water conditions. In some examples, soft, balanced, or high-chloride/sulfate water sources may have a saturation index less than 0, and therefore may be more likely to induce corrosion than high TDS water sources (e.g., sea water, produced water, or brackish water). The polymers and polymer mixtures disclosed herein may inhibit corrosion, such as corrosion caused by contact of a surface with a water source containing corrodents or corrosive conditions which may cause corrosion. The polymers and polymer mixtures herein may also inhibit formation of scale such as scale formed from calcium carbonate; magnesium carbonate; calcium sulfate; barium sulfate; barium carbonate; calcium fluoride; silicates of calcium, magnesium, aluminum, or iron; etc.; or any other scales known to form in aqueous systems. The polymer compositions disclosed above inhibit corrosion without the use of phosphorous or phosphorous containing compounds (e.g., phosphates).


In some embodiments, the polymer compositions disclosed herein may be used in combination with additional phosphorous containing molecules, moieties, or ions, such as phosphates or phosphonates (e.g., a polymethylene phosphonate derivative). Such phosphorous containing molecules, ions or moieties may be present in any of the above polymer compositions at about 0.1 mol % to about 5 mol %, such as about 1 mol % to about 3 mol %, about 0.5 mol % to about 1.5 mol %, about 1.5 mol % to about 3 mol %, or about 3 mol % to about 5 mol %.


In use, the polymer compositions herein may be mixed in water and/or a water source to result in a polymer mixture. For example, any of the polymer compositions disclosed herein may be dispersed in water (e.g., tap or deionized water) and then may be mixed in a water source. The polymer compositions herein may be mixed directly into a water source. The polymers herein may be delivered to a water source in powder form or mixed in water, and then may be mixed into the water source. Any of the polymer compositions disclosed herein may be emulsified in a water source. The polymer compositions herein may be mixed into water and/or a water source by one or more of batch-wise, continuous (e.g., drip feed), or incremental addition(s) of the polymer composition, in an as-formed polymer composition or mixed into water, to the water source. In some embodiments, a water source having one or more of the corrosion inhibiting polymer compositions is recirculated through a portion of a water containing system such as a cooling tower, radiator, or drill string and may be augmented with an additional or supplemental amount of corrosion inhibiting polymer composition. Such augmentation may be monitored and controlled by tracking one or more tagging agents in the polymers as described above.


One or more of the corrosion inhibiting polymer compositions may be mixed in the water source in any one of various dosages. For example, a polymer composition may be mixed in water and/or a water source to arrive at a dosage of about 0.01 ppm or more, such as about 0.01 ppm to about 1000 ppm, about 0.05 ppm to about 200 ppm, about 0.1 ppm to about 100 ppm, about 0.2 ppm to about 50 ppm, about 0.01 ppm to about 1 ppm, about 1 ppm to about 5 ppm, about 3 ppm to about 8 ppm, about 5 ppm to about 10 ppm, about 5 ppm to about 15 ppm, about 7 ppm to about 12 ppm, about 12 ppm to about 18 ppm, about 10 ppm to about 20 ppm, about 20 ppm to about 30 ppm, about 30 ppm to about 40 ppm, about 40 ppm to about 50 ppm, about 50 ppm to about 80 ppm, about 80 ppm to about 100 ppm, about 100 ppm to about 200 ppm, about 200 ppm to about 500 ppm, about 0.01 ppm to about 10 ppm, about 0.1 ppm to about 20 ppm, or about 0.5 ppm to about 10 ppm. The dosage may be more than about 0.01 ppm and less than about 200 ppm, such as less than about 100 ppm, less than about 50 ppm, less than about 20 ppm, less than about 10 ppm, less than about 5 ppm, or less than about 2 ppm. Any of the above listed dosages may be an effective amount to substantially inhibit or prevent corrosion in a water containing system utilizing a water source having high TDS therein. The polymer compositions may be mixed into water and/or the water source in batch-wise or continuous feeds in amount less than the dosage, such as in a fraction of the dosage per unit time. Examples of such a mixing scheme may include adding one tenth of the total dosage over ten evenly spaced intervals (e.g., 1 to 10 minute intervals); adding half of the dosage at a beginning point and the other half after an interval has passed; a continuous feed configured to arrive at the desired dosage after a selected amount of time, such as about 1 hour to about 1 day; or the like. The polymer compositions or polymer compositions mixed in water may be mixed in the make-up water source fed into the system or may be mixed into the water source in the system (in-situ).


Systems


The corrosion inhibiting polymer compositions and polymer mixtures disclosed herein may be used in a water containing system. For example, the corrosion inhibiting polymer compositions and polymer mixtures disclosed herein may be used in any water containing system, such as desalination systems, cooling systems (e.g., cooling towers, radiators, heat pipes, etc.), pipes, drilling equipment (e.g., drill strings, drilling mud, etc.), fracking and fracking equipment, paper or pulp processing systems, wastewater treatment systems, water purification systems, ware washing, evaporators, condensers, filtration, mining, water softening, kamyr digesters, pumps, storage vessels, or any other systems using water sources or that contact one or more surfaces therein. During use, as the scale and/or forming and/or corrosion promoting content of the water sources concentrate (e.g., through evaporation) and/or thermal shock occurs, corrosive conditions intensify, corrosion initiates, and scale deposits on the surfaces of water containing systems from the water sources in contact therewith. Such surfaces may include the interior of pipes, storage vessels, radiators, heat pipes, filters, digesters, condensers, the exterior of cooling towers, or any other surface that contacts a water source. The surfaces of the water containing systems may include metals, plastics, glass, rubber or latex, fiberglass, concrete or stone, or any other material suitable to hold, transport, or filter water.


In an embodiment, the water source is soft water, balanced water, high-chloride/sulfate water, seawater, connate, produced water, or brine and the water containing system utilizing one or more of the corrosion inhibiting polymer compositions is a cooling system including one or more of a water jacket, radiators, pipes, heat pipes, pumps, a cooling tower, etc. As the water source circulates through the water containing system and is evaporated on one or more portions thereof, the TDS content gradually concentrates with each cycle through the system. The corrosive materials therein may reach a concentration where they begin to corrode the surfaces in contact therewith, if left untreated. In some embodiments, the water source may initially include (e.g., without concentrating the water source) sufficient concentrations of one or more corrodents to initiate corrosion upon contact of a surface of a water containing system. One or more of the corrosion inhibiting polymer compositions or polymer mixtures may be added therein and function to inhibit or prevent corrosion (e.g., pitting or oxidation) caused by the make-up (e.g., pH and/or dissolved solids) of the water source. Such a polymer mixture may prevent or inhibit corrosion in pipes, pumps, compressors, heat exchange surfaces (e.g., radiators or water jackets), or any other parts of the water containing system.


In an embodiment, the water source includes fresh water (e.g., tap water) and the water containing system utilizing one or more of the corrosion inhibiting polymer compositions is a cooling system including one or more of a water jacket, radiators, pipes, heat pipes, at least one pump, a cooling tower, etc. As the fresh water circulates through the water containing system and is evaporated in one or more portions thereof, the relatively low TDS content gradually concentrates with each cycle through the system. The corrosion forming materials therein may reach a TDS concentration of a water source as defined above and/or reach a concentration where they begin to corrode the surfaces in contact therewith, if left untreated. One or more of the corrosion inhibiting polymer compositions or polymer mixtures may be added therein and function to inhibit or prevent corrosion from corrodents and/or scale (e.g., calcium carbonate or calcium sulfate scale) formation caused by the dissolved solids in the fresh water. Such a polymer mixture may prevent or inhibit calcium carbonate or other scaling or deposition in pipes, pumps, compressors, heat exchange surfaces (e.g., radiators or water jackets), or any other parts of the water containing system.


The water source and corrosion inhibiting polymer composition may be maintained in a closed system or an open system, augmented with additional water from outside the system (e.g., make-up water), and/or may be circulated out of the system (e.g., blow-down water) and replaced with additional water and/or corrosion inhibiting polymer composition from outside the system. Such maintenance, augmentation, and removal of the water source and/or polymer mixture allows a user to selectively control the concentration of polymer composition in the water source and/or amount or rate of corrosion in the water containing system.


Methods


In an embodiment, a method of inhibiting corrosion includes providing or forming a corrosion inhibiting polymer composition (e.g., a composite polymer), such as any of those disclosed herein. The method may include providing a water source, such as any water source disclosed herein. The method may include mixing one or more of the corrosion inhibiting polymers in the water source. Mixing may include forming one or more of a dispersion, an emulsion, or a solution of the corrosion inhibiting polymer composition and water. Mixing may include forming one or more of a dispersion, an emulsion, or a solution of the corrosion inhibiting polymer composition and the water source, or may include mixing the corrosion inhibiting polymer composition in water and then mixing the same into the water source. Mixing may include one or more of batch wise (e.g., an individual aliquot), continuous (e.g., drip-feed, spray feed), or incremental (e.g., supplemental, on-demand, or monitored) additions. Mixing may include disposing one or more corrosion inhibiting polymers in the water source in any of the dosages disclosed herein. Mixing may include disposing one or more corrosion inhibiting polymers in water and then into the water source in any of the dosages disclosed herein.


The method may include applying the corrosion inhibiting polymer mixture to a water containing system. Applying the corrosion inhibiting polymer mixture may include circulating the polymer mixture through the water containing system, such as any water containing system or component thereof disclosed herein. For example, the polymer mixture may be circulated through a water jacket or piping. In an embodiment, the method includes recirculating the polymer mixture through the water containing system and selectively augmenting the corrosion inhibiting polymer content and/or water in the system to maintain, decrease, or increase the concentration of the corrosion inhibiting polymer in the polymer mixture. The composition of the corrosion inhibiting polymer mixture may be monitored, during use, by use of tagging agent (e.g., fluorescent tag) and equipment (e.g., fluorometer) to determine the concentration of polymer composition in the water source. Forming a corrosion inhibiting polymer may include any of the techniques disclosed below in the working examples.


The corrosion inhibiting polymers herein may be used to tolerate one or more selected species of corrosive ions in a water containing system without any corrosion, and optionally, at a particular dosage of the polymer composition or mixture thereof. For example, the method of inhibiting corrosion may include maintaining substantially no or at least 50% reduced corrosion (e.g., as compared to a system having no scale inhibitor therein). The dosage for tolerating corrosive species in the water containing system without corrosion (or 50% reduced corrosion) may include any of those dosages disclosed herein, such as about 0.1 ppm to about 50 ppm, about 10 ppm or less, or about 1 ppm or less, by way of example. The corrosion inhibiting polymer compositions disclosed herein unexpectedly prevented corrosion in relatively low dosages compared to commercially available corrosion inhibitors.


In some embodiments, even when corrosion is observed, the extent of the corrosion may be reduced at a specific corrodent concentration compared to other corrosion inhibiting compositions, and at lower dosages, when any of the polymer compositions described above are mixed therein. Such dosages may be similar or identical to any of those disclosed herein.


As described in U.S. provisional patent application No. 62/198,312 filed on Jul. 29, 2015, the disclosure of which is incorporated herein by this reference, in its entirety, for any reason; in some embodiments, any of the corrosion inhibiting polymers herein in any dosages disclosed herein can alternatively or additionally be used to prevent scale deposition of one or more surfaces in water containing systems. For example, the corrosion inhibiting polymers herein may prevent scale deposition on metal surfaces, such as steel (e.g., carbon steel or stainless steel) a galvanized metal, aluminum, copper, cast iron, etc.; plastic surfaces; or any other surface in a water containing system. Such scale inhibition can include applying any of the corrosion inhibiting polymer mixtures herein to a water containing system. In some embodiments, the water containing system can include one or more metal surfaces as disclosed above. In some embodiments, the corrosion (and/or scale) inhibiting polymer mixture (e.g., water source and corrosion inhibiting polymer composition) can be used to inhibit both scale deposition and corrosion. For example, in some embodiments, the corrosion inhibiting polymers disclosed herein can be used to prevent or inhibit scale formation and/or corrosion in water containing systems having more than 1 COC, such as about 1.1 COC or more.


Working Examples 1-12


Various working examples were synthesized for corrosion inhibiting tests. Some of the working examples were synthesized as described below. Working examples were synthesized using active polymers.


Active polymer 1, a corrosion inhibiting (composite) polymer, was formed as described below. Deionized water (283.47 g) was added to a one and a half liter reactor vessel fitted with overhead paddle stirring, a nitrogen inlet, and a condenser. The deionized water was stirred at 700 rpm, heated to 95 degrees Celsius, and purged with nitrogen gas at 1.5 L/min for 30 minutes. A solution of SPS (7.87 g) in water (20.0 g) was prepared by stirring. Four semi-batch feeds were prepared for addition to the reactor. The SPS solution was added to the reactor over 205 minutes, a 40% SMBS (171.70 g) was added to the reactor over 185 minutes, the AA (331.15 g) was added to the reactor over 180 minutes, and a 50% ATBS solution (70.30 g) was added to the reactor over 180 minutes.


Addition of the SPS and SMBS solution feeds was started. After five minutes, the AA feed and the ATBS feed were started. The AA feed, ATBS feed, and SMBS feed all finished at about the same time (about 185 minutes elapsed). The SPS feed continued for 20 minutes after the other feeds finished. After completion of the SPS feed (205 minutes elapsed), the reaction temperature was held at 95 degrees Celsius for 30 minutes and then cooled to room temperature. The resulting corrosion inhibiting polymer (working example 4) consisted of residues of AA (96.4 mol %) and ATBS (3.6 mol %), with a molecular weight of about 9,400 g/mol.


Active polymer 2, a corrosion inhibiting (composite polymer), was formed by combining 6 ppm of polymaleic acid with 9 ppm of active polymer 1.


Active polymer 3, a corrosion inhibiting (composite) polymer, was formed as described below. Deionized water (226.37 g), itaconic acid (12.00 g), and 50% sodium hydroxide solution (15.46 g) were added to a one and a half liter reactor vessel fitted with overhead paddle stirring, a nitrogen inlet, and a condenser. The deionized water, itaconic acid, and sodium hydroxide solution was stirred at 700 rpm, heated to 95 degrees Celsius, and purged with nitrogen gas at 1.5 L/min for 30 minutes. A solution of SPS (8.36 g) in water (20.0 g) was prepared by stirring. A mixture of tert-butylacrylamide (8.00 g) in AA (338.0 g) was prepared by stirring.


Four semi-batch feeds were prepared for addition to the reactor; the times of addition for each feed are as follows. The SPS solution was added to the reactor over 205 minutes, a 40% SMBS solution (182.76 g) was added to the reactor over 185 minutes, the AA/tert-butyl acrylamide mixture was added to the reactor over 180 minutes, and a 50% ATBS solution (84.06 g) was added to the reactor over 180 minutes.


Addition of the SPS and SMBS solution feeds was started. After five minutes, the AA/tert-butyl acrylamide feed and the ATBS feed were started. The AA/tert-butyl acrylamide feed, ATBS feed, and SMBS feed all finished at about the same time (about 185 minutes elapsed). The SPS feed continued for 20 minutes after the other feeds finished. After completion of the SPS feed (205 minutes elapsed), the reaction temperature was held at 95 degrees Celsius for 30 minutes and then cooled to room temperature. The resulting corrosion inhibiting polymer (active polymer 3) consisted of residues of AA (93.3 mol %), ATBS (3.7 mol %), itaconic acid (1.8 mol %), and tert-butyl acrylamide (1.2 mol %), with a molecular weight of about 14,000 g/mol.









TABLE 1







Compositions of active polymers 1 and 3 (in mol %) and the


corresponding molecular weights of each polymer composition.










Polymer composition (mol %)













Active

2nd


MW,


Polymer #
1st Monomer
Monomer
3rd Monomer
4th Monomer
g/mol





1
Acrylic acid
ATBS


18,000



(96.4)
(3.6)


3
Acrylic acid
ATBS
Itaconic acid
tert-Butyl
14,000



(93.3)
(3.7)
(1.8)
acrylamide






(1.2)









Working examples were formed using one or more of active polymers 1 and 3. All working examples were dispersed in a soft water solution. The soft water solution included 100 ppm of calcium, 50 ppm of magnesium, 100 ppm of alkalinity, 200 ppm of dissolved chloride, 100 ppm of sulfate, and a pH of 8.2. Each of working examples 1-12 were mixed into the soft water solution to provide the concentrations of the components noted below in Table 2.


Working example 1 comprises 20 ppm active polymer 1. Working example 2 comprises 6 ppm (active) polymaleic acid and 9 ppm active polymer 1 (i.e. 15 ppm active polymer 2). Working example 3 comprises 20 ppm active polymer 3. Working example 4 comprises 30 ppm active polymer 3. Working example 5 includes 20 ppm of active polymer 3 and 5 ppm of active polymer 1. Working example 6 includes 20 ppm of active polymer 3, 5 ppm of active polymer 1, and 2 ppm of zinc as zinc chloride. Working example 7 includes 20 ppm of active polymer 3 and 20 ppm of hydrolyzed polymaleic acid. Working example 8 includes 20 ppm of active polymer 3 and 20 ppm of Belclene® 200, a commercially available corrosion inhibitor comprising polymaleic acid and hydrolyzed polymaleic acid. Working example 9 includes 20 ppm of active polymer 3 and 20 ppm of dissolved molybdate. Working example 10 includes 20 ppm of active polymer 3 and 20 ppm of dissolved silicate. Working example 11 includes 20 ppm of active polymer 3 and 2 ppm of tin. Working example 12 includes 20 ppm of active polymer 3 and 2 ppm of cerium.









TABLE 2







Components and concentrations thereof of each of working examples 1-12 in soft water.










Corrosion inhibitor composition (mol %)

















Amt. of

Amt. of

Amt. of
Approx.


Working

1st Comp.

2nd Comp.

3rd Comp.
Corrosion


Example

active

active

active
Rate


#
1st Comp.
(ppm)
2nd Comp.
(ppm)
3rd Comp.
(ppm)
(mpy)

















1
Active
20




≈15



polymer 1


2
Active
9
polymaleic
6


≈15



polymer 1

acid


3
Active
20




2.7



polymer 3


4
Active
30




2.0



polymer 3


5
Active
20
Active
5


4.0



polymer 3

polymer 1


6
Active
20
Active
5
Zinc
2
0.7



polymer 3

polymer 1


7
Active
20
Hydrolyzed
20


3.5



polymer 3

polymaleic





acid


8
Active
20
Belclene ®
20


4.0



polymer 3

200


9
Active
20
Molybdate
20


3.5



polymer 3


10
Active
20
Silicate
20


3.0



polymer 3


11
Active
20
Tin
2


1.5



polymer 3


12
Active
20
Cerium
2


3.0



polymer 3









Each of working examples 1-12 were tested for corrosion inhibition under halogenation (e.g., bleach) conditions using the Gamry electrochemical instrument and related software. The Gamry electrochemical instrument and associated software measure polarization resistance over time to determine a corrosion rate versus time curve from which steady state corrosion is determined. The soft water solution was prepared for the corrosion testing. The soft water solution included 0.147 g of CaCl2·2H2O, 0.123 g MgSO4·7H2O, 0.168 g of NaHCO3, 0.077 g of Na2SO4, and 0.213 g NaCl, all dissolved in one liter of deionized water. Approximately 800 ml of the soft water solution was used in a 1 L round bottom glass flask and was heated using a temperature controller to 120° F. and the solution was simultaneously purged with air (very low rate). The study was done in well aerated system and the pH was maintained at 8.0-8.2 with CO2. Throughout the study the corrosion inhibitor was dosed at 10-30 PPM as active chemical as disclosed below.


The Gamry electrochemical instrument operated through a rotary electrode principle and contained a rotating cylinder electrode, for which the rotator speed was between about 180 rpm and about 500 rpm. The experiment continued for 48 hours, during which in the first 24 hours the data was collected in an as-mixed state. Next, the oxidizing biocide (bleach) was dosed for next 24 hours. Gamry software collected the data through polarization resistance (Rp) measurements at a potential scan rate of 0.1 mV/second within 20 mV of the corrosion potential (Ecorr) from the cathodic region to the anodic region. A corrosion rate (mpy) versus time curve was plotted using the Gamry software, as shown for example in FIG. 1, and the steady state corrosion rate was determined with this plot.


Working example 1 exhibited a steady corrosion rate that of about 15 mpy after about 24 hours, and an average corrosion rate of about 15 mpy during a 48 hour test period. Working example 2 exhibited a steady corrosion rate of about (just under) 15 mpy during the 48 hour test period.


Working examples 3-12 exhibited an average corrosion rate below the water treatment industry standard for corrosion inhibition. Water treatment industry standards for corrosion inhibition key performance indicators (KPI) are rates that are less than about 5 mpy. Each of working examples 3-12 demonstrated corrosion inhibition rates exceeding the industry standard (KPI) as detailed below.


Working example 3 (20 ppm of tetrapolymer) exhibited an average corrosion rate of about 2.7 mpy during the 48 hour test. Working example 3 exhibited outstanding corrosion inhibition.


Working example 4 (30 ppm of tetrapolymer) exhibited an average corrosion rate of about 2.0 mpy during the 48 hour test. Working example 4 exhibited outstanding corrosion inhibition.


Working example 5 exhibited a steady corrosion rate of about 4.0 mpy (some individual intervals testing between about 4.0 mpy and about 5.0 mpy, with outliers below 4.0 mpy) after about 24 hours, and an average corrosion rate of about 4.0 mpy during the 48 hour test period.


Working example 6 (mixture of active polymer 3, active polymer 1, and zinc) exhibited outstanding corrosion inhibition with a steady corrosion rate of about 0.7 mpy during the 48 hour test period. Some of the individual intervals showed corrosion rates below 0.5 mpy.


Working example 7 exhibited a steady corrosion rate of about 3.7 mpy after about 24 hours, and an average corrosion rate of about 3.5 mpy during the 48 hour test period. Some individual intervals tested at about 4.0 mpy.


Working example 8 exhibited a steady corrosion rate of about 4.0 mpy after about 24 hours, and an average corrosion rate of about 4.0 mpy during a 48 hour test period. Some individual intervals tested above at or above 4.0 mpy.


Working example 9 exhibited a steady corrosion rate of just under 3.5 mpy during the initial 24 hours, a steady corrosion rate of just over 3.5 mpy after about 24 hours, and an average corrosion rate of about 3.5 mpy during the 48 hour test period. Some individual intervals tested above at or below about 3.0 mpy.


Working example 10 exhibited an average corrosion rate of about 3.0 mpy during the 48 hour test period.


Working example 11 (active polymer 3 and tin) exhibited outstanding corrosion inhibition, with an average corrosion rate of about 1.5 mpy.


Working example 12 (active polymer 3 and cerium) exhibited an average corrosion rate of about 3.0 mpy during the 48 hour test period.



FIG. 1 is a graph of corrosion rate versus time for individual test runs (procedures as detailed above) of working examples 4, 6, 11, and 12. As shown in FIG. 1, each of working examples 4, 6, 11, and 12 demonstrated corrosion inhibition well below industry standards. Each of working examples 4, 6, 11, and 12 demonstrated excellent corrosion inhibition without phosphorous, and with large molecule (e.g., polymer) corrosion inhibitors. Working example 4 (and the working examples having active polymer 3 therein) demonstrated unexpected corrosion resistance and extent thereof. Generally, corrosion inhibitors are small molecules. The polymer compositions tested includes relatively larger polymer molecules. But expectedly, exceptional corrosion inhibition was observed with the corrosion inhibiting polymer composition despite the relatively large size of the polymers (e.g., polymers that contain no phosphorous) compared to traditional corrosion inhibitors.


As shown in FIG. 1, an individual test run of working example 4 exhibited a steady corrosion rate of just over 1.5 mpy during the initial 24 hours, a steady corrosion rate slightly higher than in the initial 24 hours at about 2 mpy after about 24 hours, and an average corrosion rate of about just under 2.0 mpy during the 48 hour test period. The corrosion rate of working example 4 appeared to be increasing with time. As noted above, working example 6 showed the highest extent of corrosion inhibition, with an average corrosion rate of about 0.7 mpy, with some of the individual intervals of the test run in FIG. 1 showing corrosion rates below 0.5 mpy.


With respect to FIG. 1, working example 11 showed an average corrosion rate of about 1.5 mpy in the test run, with a corrosion rate of less than about 1.5 mpy during the initial 24 hours, an average corrosion rate slightly higher than in the initial 24 hours at about 2.0 mpy after the initial 24 hours. Individual intervals tested between about 0.5 mpy and about 1.5 mpy during the initial 24 hours, and between about 1.5 mpy and about 3.0 mpy during the second 24 hours, with a majority testing in the range of about 1.0 mpy to about 1.5 mpy. The corrosion rate of working example 11 steadily increased throughout the 48 hour period. Working example 12 exhibited a an average corrosion rate of about 3.0 mpy with individual intervals in the test run shown in FIG. 1 having corrosion rates between about 2.0 mpy and about 4.5 mpy. The corrosion rate of working example 12 steadily increased throughout the 48 hour period.


Working examples 3 and 4 were tested for scale inhibition, with inhibition of scale demonstrated the working examples as detailed in U.S. provisional patent application No. 62/198,312, which was previously incorporated herein. Working examples 3 and 4 demonstrated excellent scale inhibition in seawater.


Working Example 13


In order to more fully understand the performance of anticorrosion compositions under water flow dynamics and velocity as found in industrial water process systems, compositions for scale control were applied to a pilot cooling tower. The pilot cooling tower (PCT) is used to simulate actual industrial cooling water systems.


Electric heating rods were inserted inside mild steel metal tubes placed within the interior of the PCT water recirculation system to heat the water circulating throughout the PCT. Metal coupons and corrator probes (Nalco Corrosion Monitor, or NCM, available from Nalco Water of Naperville, IL) of mild steel metallurgy were placed in a coupon rack immersed within the water recirculation loop in order to subject them to the corrosion conditions within the loop.


To fill the recirculation loop, 200 L of synthetic soft water was applied to the loop. Synthetic soft water was prepared by combining deionized water with 0.147 g/liter of CaClz·2H2O, 0.123 g/liter MgSO4·7H2O, 0.168 g of NaHCO3, 0.077 g/liter of Na2SO4, and 0.213 g/liter NaCl. The soft water was recirculated for a period of time sufficient to reach constant conditions of 23 liters recirculation per minute at a return temperature of 45° C.±4° C. and pH of 8.2±0.1. Then 30 ppm of active polymer 3 and 2 ppm zinc ions (as zinc chloride) were added separately to the PCT through the PCT dosing pumps and the dosed water was recirculated through the cooling tower recirculation system using a pump for 4 cycles of concentration, corresponding to a duration of 14 days, under the conditions recited above. At the end of the recirculation period, the metal coupons and corrator probes were removed and analyzed for corrosion.


The combination of 30 ppm active polymer 3 with 2 ppm zinc exhibited outstanding corrosion inhibition as shown in FIG. 2. Thus, the excellent performance of active polymer 3, further in the presence of zinc, was reproduced in the PCT system based on the prediction of good performance in working examples 1-12.


The invention illustratively disclosed herein can be suitably practiced in the absence of any element which is not specifically disclosed herein. Additionally each and every embodiment of the invention, as described herein, is intended to be used either alone or in combination with any other embodiment described herein as well as modifications, equivalents, and alternatives thereof. In various embodiments, the invention suitably comprises, consists essentially of, or consists of the elements described herein and claimed according to the claims. It will be recognized that various modifications and changes may be made without following the example embodiments and applications illustrated and described herein, and without departing from the scope of the claims.

Claims
  • 1. A corrosion inhibiting mixture comprising an industrial process water source; andabout 0.05 ppm to about 200 ppm by weight of a polymer composition dispersed in the water source, the polymer composition comprising the residues of about 90 mol % to about 97 mol % of a first monomer, about 0.01 mol % to about 5 mol % of a second monomer that is chemically different from the first monomer, and about 0.01 mol % to about 5 mol % of a third monomer that is chemically different from the first and second monomers,wherein the first monomer is acrylic acid, a salt thereof, or a conjugate base thereof; maleic acid, a salt thereof, or a conjugate base thereof; or methacrylic acid, a salt thereof, or a conjugate base thereof,the second monomer is 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof; maleic acid, a salt thereof, or a conjugate base thereof; methacrylic acid, a salt thereof, or a conjugate base thereof; methallyl sulfonate; or sulfostyrene; andthe third monomer is 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof; itaconic acid, a salt thereof, or a conjugate base thereof; crotonic acid, a salt thereof, or a conjugate base thereof; tert-butylacrylamide; or dimethylacrylamide.
  • 2. The corrosion inhibiting mixture of claim 1, wherein the polymer composition further comprises about 0.01 mol % to about 5 mol % of a fourth monomer, wherein the fourth monomer is chemically different from the first monomer, the second monomer, and the third monomer; and wherein the fourth monomer is itaconic acid, a salt thereof, or a conjugate base thereof; crotonic acid, a salt thereof, or a conjugate base thereof; tert-butylacrylamide; or dimethylacrylamide.
  • 3. The corrosion inhibiting mixture of claim 2 wherein the polymer composition further comprises about 0.01 mol % to about 5 mol % of methacrylic acid, a salt thereof, or a conjugate base thereof; wherein the methacrylic acid, salt thereof, or conjugate base thereof is chemically different from the first monomer, the second monomer, the third monomer, and the fourth monomer.
  • 4. The corrosion inhibiting mixture of claim 1 further comprising about 0.05 ppm to about 10 ppm of one or more of zinc, molybdenum, silicone, tin, or cerium.
  • 5. The corrosion inhibiting mixture of claim 1 wherein the second monomer is 2-acrylamido-2-methylpropane sulfonic acid or a conjugate base thereof.
  • 6. The corrosion inhibiting mixture of claim 1 wherein the first monomer is acrylic acid or a conjugate base thereof.
  • 7. The corrosion inhibiting mixture of claim 1 wherein the third monomer is itaconic acid or a conjugate base thereof
  • 8. The corrosion inhibiting mixture of claim 2 wherein the fourth monomer is tert-butylacrylamide.
  • 9. The corrosion inhibiting mixture of claim 1, wherein the polymer composition comprises about 93 mol % to 94 mol % acrylic acid, about 3 mol % to 4 mol % 2-acrylamido-2-methylpropane sulfonic acid or a conjugate base thereof, about 1 mol % to 2 mol % itaconic acid or a conjugate base thereof, and about 1 mol % to 2 mol % tert-butylacrylamide.
  • 10. The corrosion inhibiting mixture of claim 1 wherein the water source comprises fresh water, soft water, balanced water, high-chloride/sulfate water, sea water, produced water, municipal water, brackish water, a synthetic version of any of the foregoing, or combinations of any of the foregoing, further wherein the water source comprises a corrodent.
  • 11. A method of inhibiting corrosion in water containing systems, the method comprising: adding about 0.05 ppm to 200 ppm of a corrosion inhibiting polymer composition to a water source to form a corrosion inhibiting polymer mixture, the corrosion inhibiting polymer composition comprising the residues of about 90 mol % to about 97 mol % of a first monomer, about 0.01 mol % to about 5 mol % of a second monomer that is chemically different from the first monomer, and about 0.01 mol % to about 5 mol % of a third monomer that is chemically different from the first and second monomers, wherein the first monomer is acrylic acid, a salt thereof, or a conjugate base thereof; maleic acid, a salt thereof, or a conjugate base thereof; or methacrylic acid, a salt thereof, or a conjugate base thereof, the second monomer is 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof; maleic acid, a salt thereof, or a conjugate base thereof; methacrylic acid, a salt thereof, or a conjugate base thereof; methallyl sulfonate; or sulfostyrene; and the third monomer is 2-acrylamido-2-methylpropane sulfonic acid, a salt thereof, or a conjugate base thereof; itaconic acid, a salt thereof, or a conjugate base thereof; crotonic acid, a salt thereof, or a conjugate base thereof; tert-butylacrylamide; or dimethylacrylamide; andapplying the corrosion inhibiting polymer mixture to a water source within a water containing system.
  • 12. The method of claim 11 wherein the corrosion inhibiting polymer mixture further comprises about 0.05 ppm to about 10 ppm of one or more of zinc, molybdenum, silicon, tin, cerium, aluminum, vanadium, or tungsten ions.
  • 13. The method of claim 11 wherein the water containing system includes one or more of a cooling tower, a radiator, one or more pipes, a water jacket, a desalination membrane, a condenser, an evaporator, a pump, or a storage vessel.
  • 14. The method of claim 11 wherein the applying includes recirculating for at least one cycle of concentration.
Provisional Applications (1)
Number Date Country
62368255 Jul 2016 US