The present disclosure is directed, in general, to a system and method for repairing and manufacturing high-temperature superalloy components, and more specifically to such a system and method for the repair and manufacturing of gas turbine blades and vanes.
The difficulties associated with the additive manufacture (AM) of nickel-base gas turbine components with high gamma-prime (γ′) content makes the process unsuitable for large scale manufacturing or repair. In particular, attempts to additively manufacture components using a CM 247 LC branded superalloy, or to repair such components often result in grain boundary melting and cracking. Alternatively, the components are repaired with another inferior nickel base alloy that is less prone to cracking, resulting in poor performance of the component.
Variously disclosed embodiments include systems and methods that may be used to facilitate additively manufacturing components (or portions thereof) made from one or more superalloys. In an aspect, a method of additively manufacturing includes successively depositing and fusing together layers of a superalloy powder mixture comprised of a base material powder and a eutectic powder, to build up an additive portion. The eutectic powder has a solidus temperature lower than the solidus temperature of the base material powder. In addition, the method includes heat treating the additive portion at a temperature greater than 1200° C. to heal cracks and/or fill pores and to homogenize the alloy of which the additive portion is comprised. The additive portion alloy has a chemistry defined by the superalloy powder mixture. Also, the base material powder is formed of a nickel-base superalloy with an aluminum content by weight of at least 1.5%.
In a further aspect, the method may in include removing a damaged portion from a component to leave a first interface; printing a replacement portion via successively the depositing and fusing together layers of the superalloy powder mixture, which replacement portion has a second interface surface; and attaching the second interface surface to the first interface surface to replace the damaged portion of the component.
Further aspects may include the superalloy powder mixture comprised of at least 76% by weight of the base material alloy and at least 6% by weight of the eutectic powder.
In aspects, the eutectic powder may be a nickel-base alloy including by weight about 6% to about 11% chromium, about 5% to about 9% titanium, and about 9% to about 13% zirconium, with balance nickel and optional incidental elements and unavoidable impurities.
The foregoing has outlined rather broadly the technical features of the present disclosure so that those skilled in the art may better understand the detailed description that follows. Additional features and advantages of the disclosure will be described hereinafter that form the subject of the claims. Those skilled in the art will appreciate that they may readily use the conception and the specific embodiments disclosed as a basis for modifying or designing other structures for carrying out the same purposes of the present disclosure. Those skilled in the art will also realize that such equivalent constructions do not depart from the spirit and scope of the disclosure in its broadest form.
Also, before undertaking the Detailed Description below, it should be understood that various definitions for certain words and phrases are provided throughout this specification and those of ordinary skill in the art will understand that such definitions apply in many, if not most, instances to prior as well as future uses of such defined words and phrases. While some terms may include a wide variety of embodiments, the appended claims may expressly limit these terms to specific embodiments.
Before any embodiments of the invention are explained in detail, it is to be understood that the invention is not limited in its application to the details of construction and the arrangement of components set forth in the following description or illustrated in the following drawings. The invention is capable of other embodiments and of being practiced or of being carried out in various ways. Also, it is to be understood that the phraseology and terminology used herein is for the purpose of description and should not be regarded as limiting.
Various technologies that pertain to systems and methods will now be described with reference to the drawings, where like reference numerals represent like elements throughout. The drawings discussed below, and the various embodiments used to describe the principles of the present disclosure in this patent document are by way of illustration only and should not be construed in any way to limit the scope of the disclosure. Those skilled in the art will understand that the principles of the present disclosure may be implemented in any suitably arranged apparatus. It is to be understood that functionality that is described as being carried out by certain system elements may be performed by multiple elements. Similarly, for instance, an element may be configured to perform functionality that is described as being carried out by multiple elements. The numerous innovative teachings of the present application will be described with reference to exemplary non-limiting embodiments.
Also, it should be understood that the words or phrases used herein should be construed broadly, unless expressly limited in some examples. For example, the terms “including,” “having,” and “comprising,” as well as derivatives thereof, mean inclusion without limitation. The singular forms “a”, “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. Further, the term “and/or” as used herein refers to and encompasses any and all possible combinations of one or more of the associated listed items. The term “or” is inclusive, meaning and/or, unless the context clearly indicates otherwise. The phrases “associated with” and “associated therewith,” as well as derivatives thereof, may mean to include, be included within, interconnect with, contain, be contained within, connect to or with, couple to or with, be communicable with, cooperate with, interleave, juxtapose, be proximate to, be bound to or with, have, have a property of, or the like. Furthermore, while multiple embodiments or constructions may be described herein, any features, methods, steps, components, etc. described with regard to one embodiment are equally applicable to other embodiments absent a specific statement to the contrary.
Also, although the terms “first”, “second”, “third” and so forth may be used herein to refer to various elements, information, functions, or acts, these elements, information, functions, or acts should not be limited by these terms. Rather these numeral adjectives are used to distinguish different elements, information, functions or acts from each other. For example, a first element, information, function, or act could be termed a second element, information, function, or act, and, similarly, a second element, information, function, or act could be termed a first element, information, function, or act, without departing from the scope of the present disclosure.
In addition, the term “adjacent to” may mean: that an element is relatively near to but not in contact with a further element; or that the element is in contact with the further portion, unless the context clearly indicates otherwise. Further, the phrase “based on” is intended to mean “based, at least in part, on” unless explicitly stated otherwise. Terms “about” or “substantially” or like terms are intended to cover variations in a value that are within normal industry manufacturing tolerances for that dimension. If no industry standard as available a variation of 20 percent would fall within the meaning of these terms unless otherwise stated.
In one construction, the vanes 30 are manufactured from a nickel-base superalloy such as CM 247 LC superalloy.
During operation, the vanes 30 can become damaged. Damage can be caused by foreign object impacts, high temperature operation, fatigue, creep, oxidation, and the like. One area that is susceptible to damage is the leading edge 35 of the vane 30.
The process begins by mixing a high γ′ forming nickel-base powder 66 (base material) with a binder 67 and 3D printing or otherwise additively manufacturing a green form of the desired component 70, 75 to a near net shape. The green form component 70, 75 is then allowed to dry.
The next step is the placement of the green form component 70, 75 into a furnace or other heating device. The green form component 70, 75 is heated to burn or remove the binder 67. The remaining material defines a skeleton 85, 90 made up of the base material 66 and gaps or empty areas 68 formerly occupied by the binder material 67. In
As illustrated in
To produce the desired infiltration, the melting point depressant 100 is melted in a manner that assures that the liquid melting point depressant 100 is in contact with the skeleton 85, 90. Capillary action produced by the porosity in the skeleton 85, 90 pulls the liquid melting point depressant 100 into the pores 68 of the skeleton 85, 90 and can result in a completed component 60, 65 that is ninety-nine percent filled with material (i.e., one percent porosity).
The specific composition of the melting point depressant 100 is selected based at least in part on the quantity of titanium included in the base material. For example, in constructions that include 3.5 percent or more titanium by weight in the base material, the desired melting point depressant 100 includes at least one of Hf and Zr with the remainder being Ni and Cr. In constructions with 1.0 percent or less Ti in the base material, the preferred composition includes Ti with the balance being Ni and Cr. When the quantity of Ti is between 1.0 percent and 3.5 percent in the base material, the desired composition includes at least one of Zr, and Ti with the balance being Ni and Cr. The quantity of Ti, Zr, or Hf are selected such that the completed nickel-base component has less than 6.0 percent Ti (with other constructions being below 5.0 percent and still others below 4.0 percent).
Once the infiltration is complete, any features added for manufacturing requirements such as the gate 80 or a support structure illustrated in
The process described herein does not melt the base material powder 66. Rather, the powder 66 is mixed with the binder 67, 3D printed using a laser source or other energy source and dried. The binder 67 is burned out at low temperature (e.g., <500 C.). The remaining base material 66 is heated up to a sintering temperature that assures a maximum of twenty percent porosity is left in the sintered material.
For nickel-base alloys, the amount of titanium employed is preferably limited to around six percent (i.e., between four and eight percent) to reduce the likelihood of reduced mechanical properties. Due to this limitation, the level of porosity in the skeleton 85, 90 is determined, at least in part by the amount of titanium in the base material and in the braze material 100 (sometimes referred to as melting point depressant) with the goal being about six percent titanium in the finished component 60, 65. For example, in one construction, the base material or the skeleton 85, 90 may include no titanium. If a braze material that contains 22% titanium is employed, the total porosity of the skeleton 85, 90 would be limited to about 30% which leads to a completed component 60, 65 with about 6.6% titanium.
In another example, the skeleton 85, 90 includes 1% titanium. In this case, using the same braze material with 22% titanium, the skeleton 85, 90 should be limited to less than 20% porosity to arrive at a finished component 60, 65 having about 5.2% titanium.
In yet another example, the skeleton 85, 90 includes 2% titanium. In this case, using the same braze material with 22% titanium the skeleton 85, 90 should be limited to less than 15% porosity to arrive at a finished component 60, 65 having about 6.0% titanium.
As discussed, nickel-base gas turbine components, specifically CM 247 LC superalloy components, are difficult to repair or build-up with any method that involves melting of the component since the grain boundary melting (incipient melting) temperature is low with respect to the welding temperature such that the weld repair often generates cracks during the repair process.
As discussed with regard to
The damaged portion 55 is removed and replaced with a close-fitting replacement component 105 made using additively manufactured (AM) material or a pre-sintered preform (PSP) that provides similar or better oxidation and rupture properties. When the replacement component 105 is a replacement for the leading edge 35 as illustrated in
To perform a repair of the leading edge 35 with a high oxidation resistant material, the damaged portion 55 of the leading edge 35 of the vane 30 is first removed. The removed damaged portion 55 is measured to determine the size and configuration of the replacement component 105 that will be installed. The replacement component 105 is then manufactured using an additive manufacturing process or as a PSP, such as a PSP made using a process as described with regard to
When the replacement component 105 is manufactured as a PSP the preferred material includes up to eighty percent (80%) superalloy (preferably matching the vane 30 being repaired), up to eight percent (8%) aluminum, and up to thirty percent (30%) braze material including Ti, Zr, and Hf as described above. As with the additively manufactured replacement component 105, the PSP replacement components 105 can include attachment structures 110 like those described above.
The material used to manufacture the PSP replacement component 105 is maintained at a temperature at least 50 degrees C. above the braze melting temperature for more than one hour to react a majority of the braze material with the base material powder. This prevents re-melting during the braze operation that attaches the replacement component 105 to the vane 30.
An attachment PSP 115, shown in
The replacement component 105 has sufficient mechanical properties and oxidation resistance due to the adjusted composition and the Ni—Cr—(Ti, Zr, Hf) braze composition. In addition, when using the additively manufactured replacement component 105, the columnar grains provide significant rupture capability over the base material of equiaxed grain structure.
It should be noted that the replacement component 105 can be manufactured in a number of different shapes and sizes and should therefore not be limited to the arrangement illustrated in
Specifically, and with reference to
With the damaged portion removed, the replacement piece 250 can be manufactured. The replacement piece 250 could be manufactured using any of the various processes described herein and is manufactured to include the replacement surface 255 that is curved to closely match the vane surface 275 formed in the vane 265 through the removal of the damaged portion 270. In addition, any cooling holes 285 or other internal features (e.g., ribs, etc.) are typically preformed in the replacement piece 250 before it is attached to the vane 265.
The replacement surface 255 illustrated in
As illustrated in
The replacement piece 250, and the PSP interface component 290, if needed are positioned as illustrated in
As will be described below, these processes and procedures can be applied to other components such as a tip 120 of the vane 30 or blade or some other component.
For example,
A closely fitting replacement tip 140 is formed to fill the space created by the removal of the damaged portion 135. The replacement tip 140 may also fill any spaces created during the removal of any cracks 125. Alternatively, the space opened during the removal of the cracks 125 can be filled with a powdered braze material during the attachment process for the replacement tip 140. The replacement tip 140 can be formed using an additive manufacturing (AM) process or can be formed from a pre-sintered preform (PSP) that provides similar or better oxidation and rupture properties than the removed portion 135.
The replacement tip 140, when manufactured using an AM process is preferably composed of a material similar to the base material of the blade 30 with the addition of up to eight percent (8%) aluminum to provide superior oxidation resistance. In addition, attachment structures 110 such as pins 145, illustrated in
In constructions in which a PSP is used in place of an AM replacement tip 140, the material is preferably made of up to eighty percent (80%) superalloy (matching the base material of the blade 30 being repaired), up to eight percent (8%) aluminum, and up to thirty percent (30%) braze material including Ti, Zr, and Hf as described above.
The material used to manufacture the PSP replacement tip 140 is maintained at a temperature at least 50 degrees C. above the melting temperature of the braze material for more than one hour to react a majority of the braze material with the base material powder. This prevents re-melting during the braze operation that attaches the replacement tip 140 to the blade 30 being repaired.
A tip attachment PSP 150, shown in
The replacement tip 140 has sufficient mechanical properties and oxidation resistance due to the adjusted composition and the Ni—Cr—(Ti, Zr, Hf) braze composition.
As discussed earlier, gas turbine components operate under a variety of localized conditions that can produce localized damage. This can be attributed to varied component conditions (e.g., temperatures, pressures, fluid properties, etc.) and engine conditions.
One example of localized operating conditions exists at the row one turbine blade 155 where localized distress on the blades 155 can cause damage in multiple areas including a leading edge 160 of the blade 155 and a tip 165 of the blade 155.
One type of damage occurs at the leading edge 160 of the first stage blade 155, as well as other blades where the ceramic coating adheres adjacent a series of cooling apertures 175. If the coating spalls, a leading edge burn out or loss is often observed. The other area where damage can occur is at the tip 165 of the blade 155 where the blade 155 can rub against a ring segment or other component radially outward of the blade 155. Heavy oxidation can also occur at the tip 165 of the blade 155 and cracks or tip cracks can form and propagate from cooling apertures 175 or from damage caused by other factors such as rubbing or oxidation.
As discussed previously, repairs to blade or vane tips 165 can include the removal of a portion of the blade tip 165 followed by replacement with a replacement tip 170. Similar repairs can also be made to blade or vane leading edges 160.
Additive manufacturing can be relied upon to manufacture replacement components or replacement tips 170 with brazing processes and special braze materials enhancing the operation of the repaired vane or blade 155.
One preferred additive manufacturing process well-suited to manufacturing replacement components or replacement tips 170 includes atomic diffusion.
With reference to
One method of forming the green-form component 185 includes a 3-D printing technique. A wire feedstock is prepared including the desired powder metal and the binder. The user is able to combine material chemistries or tailor chemistries as desired to achieve the desired material properties in the completed replacement tip 170 or replacement piece. In addition, different compositions can be used at different times during the forming of the replacement tip 170 to achieve different properties at the different locations within the replacement tip 170. For example, in one construction a composition intended to be a first or interfacing layer includes the desired base materials as well as braze material integrated into the wire feedstock.
To manufacture the replacement tip 170 or another component, the first or interfacing layer is deposited onto a support structure 190 or is formed independent of the support structure 190. The first surface in the example of
For example, the feedstock could be changed to a second material that does not include the braze material and rather, more closely matches the base material of the blade 155 or other component being repaired. As discussed above, some materials could be employed that enhance the performance of the replacement tip 170 or other component over that of the base material. Any of those materials could be employed in this process as well. For example, up to 8% aluminum could be employed to enhance oxidation resistance. As previously noted, the sintering process is designed to not melt the powdered material. Because the process is a non-melting process, no variation in chemistry is expected.
With continued reference to
This method does not experience the isotropy of layer-based AM techniques and because of its speed in producing the green-form component 185 and very low powder waste, reduces cost significantly over other AM techniques. In addition, as noted earlier this process of additive manufacturing can be used to form components other than replacement tips 170, including leading edge replacements or other components and can include advanced features such as attachment structures 110.
Another benefit with this approach is that the components can be made from other high temperature resistant materials (e.g., oxide dispersion strengthened (ODS) or advanced single crystal (CMSX8/René N5/PWA1484)) that have better strength, oxidation resistance, and coating adhesion.
In summary,
The green-form component 185 is next printed using feedstock of the appropriate makeup. The first layer, or the first few layers may use a feedstock that is part base material, part binder, and part braze material that ultimately is used during the attachment of the replacement tip 170 to the blade 155. After these initial layers are printed, the feedstock may be switched to a feedstock that includes the desired base metal chemistry (i.e., a chemistry closely matching the blade 155) and a binder, often in the form of a polymer. The chemistry of the subsequent feedstock may include an enhanced chemical make-up as discussed earlier to provide superior material properties such as oxidation resistance.
Upon completion of the 3-D printing process, the green-form component 185 is washed and sintered to remove the binder and to mechanically or metallurgically bond the remaining particles in the desired shape. The sintered replacement tip 170 is removed from the support structure 190 as illustrated in
As illustrated in
Current materials used for pre-sintered preforms (PSPs) and for brazing materials for use with nickel-base super alloy materials that operate in high temperature environments (e.g., 1000 degrees F., 538 degrees C.) are typically nickel (Ni) chromium (Cr) based.
The composition described herein is preferably applied to PSPs and/or braze materials that do not include boron. To improve the creep rupture life of boron-free PSPs and braze materials, rhenium (Re) or Ruthium (Ru) can be added to most nickel-base braze alloys. These two elements are potent creep resistance elevators that are added to base metal composition for creep-rupture life improvement. They increase the creep resistance of nickel-base alloys by up to a factor of ten. Their high melting point and large atomic diameter results in low atomic diffusion rates and enables Ni base materials to increase their creep resistance.
Rhenium (Re) and Ruthium (Ru) have not been added to boron-free braze materials to date as the need for creep resistance braze materials was not known.
To add Re or Ru, the materials are powdered and then mixed with a base material powder mixture prior to brazing. Re and Ru are added to boron free Ni—Cr—X braze/base material powder mixture prior to PSP making. Preferably, the Re and Ru have the smallest particle size possible for the powder. It is preferred that Re and Ru powder diameter is at least 50% or smaller than the base metal and braze metal powder to assure uniform mixing and homogeneous elemental distribution after brazing. Re and Ru powders are not melted during the brazing process. Rather they diffuse into the surrounding liquid braze material during braze. Since diffusion rates are high in liquid, these elements are transported uniformly within the braze material.
Re and Ru are added such that they make up 3-6 percent of the total composition of the braze or PSP regardless of the proportion of base metal to braze powder in the braze.
For example, the repair of a component manufactured from CM 247 LC superalloy may employ a PSP that is manufactured from powders in which 74-77 percent matches the CM 247 LC superalloy composition, 20 percent matches a desired braze material (sometimes referred to as a melting point depressant), and 3-6 percent is one or both of Re or Ru.
Suitable braze materials are typically nickel-base and include nickel, chromium, and at least one of titanium, zirconium, and hafnium. Some specific braze compositions include a composition that includes 6.5% Cr, 11% Zr, 7.5% Ti, and the remainder Ni. Another composition could include 5.0% Cr, 10% Hf, 10% Zr, and the remainder Ni. Yet another composition could include 17% Cr, 22% Ti, and the remainder Ni.
Each of the three components, the base material (74-77 percent), the braze material (20 percent), and the Re or Ru (3-6 percent) are powdered and mixed together for sintering. During any melting steps (i.e., brazing processes), the Re and Ru are not melted. Rather, they disperse through any melt pools during the melting process.
Nickel-base superalloys that include more than about two percent aluminum are known to be particularly difficult to weld or to form using present additive manufacturing techniques. Components, parts of components, or preforms using these materials can be manufactured using a process similar to that described above. In one example, a preform (e.g., preforms 105, 250, etc.) with a nickel-base superalloy that may include at least 4.5 percent aluminum is formed. Of course, the system and process can be used with virtually any desired material. In one process, illustrated in
The micro-dispensing AM system is then operated to dispense the mixture in a series of layers that define the desired shape of the PSP (step 515) (e.g., replacement piece 250, PSP interface component 290, etc.). Preferably, each layer is between 20 microns and 100 microns in thickness with other thicknesses being possible. The use of the micro-dispensing AM system allows for very fine control including the use of a CNC model to drive the positioning of the layers to improve the accuracy and finish of the final component.
Once the micro-dispensing AM process is completed, the component is removed from the device and is heated to a temperature less than 500 degrees C. but hot enough to remove the binder from the component (step 520). At the completion of this process, a component skeleton is formed that includes base material and braze material in the ratio selected for the mixture and gaps where the binder material was prior to its removal in the first heating process.
The component skeleton is then heated to a solid-state sintering temperature that for this material falls within the range of 1000 degrees C. to 1250 degrees C. (step 525). Typically, the solid-state sintering process requires less than 60 minutes to complete. Of course, other materials or mixtures having different ratios of the base material and braze material may have different solid-state sintering temperatures and may require more time to complete the solid-state sintering.
A second sintering process is then performed on the now sintered component skeleton (step 530). Specifically, the component is heated to a braze temperature greater than 1200 degrees C. such as a range of between 1250 degrees C. and 1300 degrees C. for less than 60 minutes to melt all or some of the braze material, but not the base material, thereby completing a liquid-phase sintering process. Of course, other materials or mixtures having different ratios of the base material and braze material may have different liquid-phase sintering temperatures and may require more time to complete the solid-state sintering.
To complete the formation of the skeleton component, the skeleton component is again heated to a solution treatment temperature range greater than 1200 degrees C. such as a range between 1230 degrees C. and 1300 degrees C. for between 1 and 12 hours to complete a homogenization/diffusion annealing process (step 535). Of course, other materials or mixtures having different ratios of the base material and braze material may have different diffusion annealing temperatures and may require more time to complete the diffusion annealing process.
Following these steps allows for the sintering of the component without melting and solidifying the base material (high γ′ forming nickel-base superalloy powder) such that the component is not prone to cracking.
One variation of the process just described, illustrated in
In another variation, of the just-described process, the component is covered or partially covered with either a 100 percent braze material binder mixture or a base material powder, a braze material powder, and a binder mixture. The sintered skeleton is ultimately infiltrated by the braze to obtain a near 100 percent dense component.
In all the processes just described, the braze material is preferably one of a Ni—Cr—Ti or a Ni—Cr—Ti—Zr braze. In addition, the aforementioned processes generally allow for the avoidance of a HIP (Hot Isostatic Pressing) operation as the liquid phase infiltration results in a near 100 percent dense structure (typically at least 99.9 percent).
As discussed, the above processes can be used to form components using high γ′ forming superalloy powder which does not melt in this process such that residual stresses that cause cracking and may be created during solidification are not present.
The micro-dispensing AM process can produce layers having thicknesses as low as 10 microns. In addition, PSP components or panels can be built and used to join nickel and cobalt base alloys including Ni—Cr—Ti and Ni—Cr—Ti—Zr. In addition, these materials and the micro-dispensing AM process can be used to produce foils having a total thickness of 50 microns or less (e.g., PSP interface component 290). In addition, the micro-dispensing AM process allows for the production of near net shape components using high γ′ forming materials without cracking. While an 80/20 (base material/braze material) powder mix is preferred for gas turbine applications, some applications may include up to 30 percent braze material.
It should be noted that while the foregoing examples describe the formation of PSP components separate from the components being repaired, some repairs may include printing the PSP preform directly onto the component being repaired. Thus, the invention should not be limited to PSPs that are formed separate from the component they are being made to repair.
In addition, it should be appreciated that the braze material powders described herein may be used to produce superalloy components (or portions thereof) via other types of additive manufacturing and welding processes that use metal powders to build up parts, including selective laser melting (SLM), laser powder deposition (LPD), laser metal deposition (LIVID), directed energy deposition (DED), and laser wire deposition (LWD). In such embodiments the braze material powder may correspond to a eutectic powder that is mixed with a base material powder to form a superalloy powder mixture. This superalloy powder mixture may then be used by a 3D printer to produce a new part (or portion thereof).
As discussed previously, the base material powder (mixed with the braze/eutectic powder to form the superalloy powder mixture) may correspond to a nickel-base superalloy. Such a superalloy may include by weight greater than 40% nickel and greater than 4% in total of aluminum and optional titanium content. In particular, such a base material powder may comprise by weight about 4% to about 23% chromium, about 4% to about 20% cobalt, 0% to about 8% titanium, about 1.5% to about 8% aluminum, 0% to about 11% tungsten, 0% to about 4% molybdenum, 0 to about 13% tantalum, 0% to about 0.2% carbon, 0% to about 1% zirconium, 0% to about 4% hafnium, 0% to about 4% rhenium, 0% to about 0.1% yttrium and/or cerium, 0% to about 0.04% boron, 0% to about 2% niobium and balance nickel as its primary components. For example, the base material powder may correspond to or be similar to commercially available difficult-to-weld high γ′ prime forming superalloys with chemistries such as the CM 247 LC superalloy discussed previously or other commercially available superalloys such as those listed in the following Table I (as well as other superalloys).
It should also be appreciated that such base material powder superalloys may include additional components such as 0% to 1.5% option incidental elements and/or unavoidable impurities such as listed and subsequently described with respect to Table VII. Further, superalloys sold under each of the brand names or trademarks listed in Table IV may be supplied with chemistries that vary in weight percent from those listed.
In example embodiments, the additive manufacturing process may be carried out by successively depositing and fusing together layers of a superalloy powder mixture of the base material powder and the eutectic powder to build up an additive portion. For SLM type printers, such fusing may be carried out via a laser selectively melting portions of the superalloy alloy mixture deposited on a powder bed. For LIVID type printers, a welding wire may provide the superalloy powder which is melted by a laser to build up each layer. Such a weld wire may be comprised of a nickel or a nickel alloy foil sheath which includes therein the superalloy powder mixture.
When superalloys (in particular difficult-to-weld high γ′ forming superalloys with an aluminum content of at least 4.5% by weight) are used as the base material powder in the superalloy powder mixture, the additive manufacturing process may initially form an additive portion with extensive amounts of solidification cracks and pores. However, during subsequent heat treatment, portions of the additive portion formed from the eutectic powder in the superalloy mixture may have a sufficiently low solidus temperature that it is capable of at least partially liquefying and filling in solidification cracks and pores (referred to herein as crack healing) without degradation of the shape of the additive portion and without the need for a HIP operation to collapse such cracks and pores.
In an example embodiment, the superalloy powder mixture may be comprised of at least 76% by weight of the base material powder and at least 6% by weight of the eutectic powder, to build up an additive portion. The base material powder and eutectic powder may each have a nickel content by weight greater than 40%. The base material powder (as well as the additive portion formed from the described superalloy alloy powder mixture) may have an aluminum content by weight greater than 1.5%. In addition, the eutectic powder may have a solidus temperature that is more than 220° C. below the solidus temperature of the base material powder. Further, the eutectic powder may have a liquidus temperature below 1300° C. In example embodiments, the eutectic powder may be comprised of a Ni—Cr—Ti—Zr powder or a Ni—Cr—Ti powder or other eutectic powder with the previously described properties.
In a first example of this crack healing process, a base material powder corresponding to CM 247 LC superalloy and a Ni—Cr—Ti—Zr eutectic powder with the respective chemistries shown in Table II, were mixed together in about a 90:10 ratio by weight respectively, to form a superalloy powder mixture. In this example, the liquidus temperature of the Ni—Cr—Ti—Zr eutectic powder is about 1225° C.
This superalloy powder mixture may be usable in this described crack healing additive manufacturing process to produce parts having operational characteristics (e.g., in a gas turbine) similar to casted CM 247 LC superalloy.
For comparison purposes to illustrate the crack healing aspects of this described embodiment,
It should also be appreciated that CM 247 LC superalloy (as well as the other superalloys such as those listed in Table I) may have element weight percent's that vary depending on the source of the superalloy. For example, nominal ranges for the chemistry of CM 247 LC superalloy are shown in Table III:
Further alternative embodiments of the superalloy alloy powder mixture may be comprised of other types of base material powders that are similar to or vary from those listed in Table I. For example, the superalloy alloy powder mixture may be comprised of a base material powder having a chemistry similar to René 142, René N5, and PWA 1484 branded superalloys with the following example chemistry shown in Table IV:
In these cracking healing examples, the heat treatment (during which crack healing occurs) may, for example, include a step of heating the sample block in a furnace above 1200° C. for at least 12 hours to homogenize the resulting crack healed alloy that forms the additive portion. The heat treatment process for this described crack healing additive manufacturing process may also include one or more heat treatment steps to achieve sufficient homogenization and high γ′ volume fractions (e.g., greater than 30%), such as those described previously. However, it should be appreciated that this cracking healing heat treatment may be carried out with more or less steps or different steps, temperatures, heating/cooling rates, and time ranges depending the extent of crack healing (and homogenization) that is needed for the particular part that is being produced and/or depending on chemistries of the particular base material powder and eutectic powder that were used to create the resulting alloy of the additive portion.
The following example chemistries shown in Table V of a Ni—Cr—Ti—Zr eutectic powder chemistry (when used to form a superalloy powder mixture in combination with a base material powder such as CM 247 LC superalloy illustrated in Table III, or other difficult-to-weld superalloys) may be capable of achieving the reductions in microcracking that were illustrated in the sample block 2802 shown in
Alterative embodiments may be carried out with a Ni—Cr—Ti Eutectic powder having a chemistry such as illustrated in the following Table VI:
It should be appreciated that these example Ni—Cr—Ti—Zr and Ni—Cr—Ti eutectic powder chemistries shown in Tables V and VI may also be used as braze materials for the other examples described herein. In addition, example embodiments of the superalloy chemistries described and claimed throughout this application may include one or more optional incidental elements and/or unavoidable impurities. In some example embodiments, the amount by weight of the total of any optional incidental elements may be between 0% and 1.5%. In further examples, the optional incidental elements may include one or more of the following in the indicated maximum amounts in weight % or ppm according to Table VII:
Also, in some example embodiments the amount by weight of the total of any unavoidable impurity elements may be between 0% and 0.01%. In further examples, unavoidable impurities may typically be within the maximum amounts listed in Table VII for these respective elements and for any other element that maximum may be about 0.001 in weight %. However, it should be appreciated that in further embodiments, one or more of such optional incidental elements and/or unavoidable impurities may exceed these described ranges, provided that such optional incidental elements and/or unavoidable impurities do not interfere with the ability of the described processes to produce additive portions with material properties after heat treatment (e.g., tensile strength, creep resistance) that meet the requirements for gas turbine hot gas path parts or other high temperature applications and are usable to replace corresponding parts made of an CM 247 LC superalloy or other hard-to-weld superalloys via casting processes.
Example embodiments may further include a methodology that facilitates additively manufacturing a superalloy component according to the example crack healing AM process described herein. The methodology may include an act of successively depositing and fusing together layers of a superalloy powder mixture comprised of a base material powder and a eutectic powder, to build up an additive portion. The eutectic powder has a solidus temperature lower than the solidus temperature of the base material powder. The methodology may also include an act of heat treating the additive portion at a temperature greater than 1200° C. to heal cracks and/or fill pores and to homogenize the alloy of which the additive portion is comprised. The additive portion alloy has a chemistry defined by the superalloy powder mixture.
In example embodiments, the base material powder may be a nickel-base superalloy with a nickel content by weight greater than 40% and with an aluminum content by weight of at least 1.5%. The eutectic powder may be a nickel-base alloy including by weight about 6% to about 11% chromium, about 5% to about 9% titanium, about 9% to about 13% zirconium, and greater than 40% nickel.
In example embodiments, the methodology may include an act of removing a damaged portion from a component to leave a first interface. The act of successively depositing and fusing together layers of the superalloy powder mixture may print a replacement portion that has a second interface surface. In addition, the methodology may include an act of attaching the second interface surface to the first interface surface to replace the damaged portion of the component.
In example embodiments of the methodology, heat treating may include heat treating the additive portion at a temperature at or above 1230° C.
In further examples, the ratio of the base material powder to the eutectic powder by weight in the superalloy powder mixture is between about 94:06 and about 76:24, and in particular between about 94:06 and about 85:15.
Also in example embodiments, at least 95% by weight of the additive portion alloy is formed from the base material powder and the eutectic powder.
In addition, the base material powder may include greater than 4% in total of aluminum and optional titanium content by weight. Further, the base material powder may include at least 4.5% aluminum by weight. Also, the eutectic powder may include at maximum 1% aluminum by weight. In addition, the base material powder may include at least 5.5% aluminum by weight and greater than 45% nickel by weight.
The balance of the eutectic powder by weight may include nickel and optional incidental elements and unavoidable impurities. The eutectic powder may include by weight at maximum 1.5% of one or more incidental elements. Also, the eutectic powder may include by weight at maximum 0.01% of one or more unavoidable impurities.
In addition, the solidus temperature of the eutectic powder may be more than 220° C. below the solidus temperature of the base material powder. Further, the eutectic powder may have a liquidus temperature below 1300° C.
In this example methodology, the additive portion alloy (after one or more heat treatments) has γ′ volume fractions greater than 30%, alternatively greater than 50%, and alternatively greater than 70%.
Further the additive portion may form at least a portion of a turbine blade or turbine guide vane.
In example embodiments, the superalloy powder mixture may be deposited and fused together via a SLM 3D printer to form the additive portion.
In alternative embodiments, the superalloy powder mixture may be deposited and fused together via a LWD system, which employs a welding wire to provide the superalloy powder mixture. The welding wire may be comprised of a nickel or a nickel alloy foil sheath including therein the superalloy powder mixture.
In addition, it should also be appreciated that this described methodology may include additional acts and/or alternative acts corresponding to the features described previously with respect to the crack healing process, braze materials, and other additive manufacturing processes described herein.
None of the description in the present application should be read as implying that any particular element, step, act, or function is an essential element, which must be included in the claim scope: the scope of patented subject matter is defined only by the allowed claims. Moreover, none of these claims are intended to invoke a means plus function claim construction unless the exact words “means for” are followed by a participle.
| Number | Name | Date | Kind |
|---|---|---|---|
| 4910098 | Lee et al. | Mar 1990 | A |
| 5240491 | Budinger et al. | Aug 1993 | A |
| 5725692 | Deluca et al. | Mar 1998 | A |
| 6171417 | Kawai | Jan 2001 | B1 |
| 6454885 | Chesnes et al. | Sep 2002 | B1 |
| 6503349 | Pietruska | Jan 2003 | B2 |
| 6575702 | Jackson | Jun 2003 | B2 |
| 8034154 | Singer et al. | Oct 2011 | B2 |
| 8640942 | Ozbaysal et al. | Feb 2014 | B1 |
| 8986604 | Green | Mar 2015 | B2 |
| 9388479 | Green | Jul 2016 | B2 |
| 9765623 | Kottilingam | Sep 2017 | B2 |
| 9863249 | Shinn | Jan 2018 | B2 |
| 10076811 | Ozbaysal et al. | Sep 2018 | B2 |
| 10279438 | Ozbaysal | May 2019 | B2 |
| 10392938 | Ghunakikar | Aug 2019 | B1 |
| 10577679 | Wessman et al. | Mar 2020 | B1 |
| 10752978 | Hardy et al. | Aug 2020 | B2 |
| 10753211 | Cui et al. | Aug 2020 | B2 |
| 10800108 | Mark et al. | Oct 2020 | B2 |
| 10919119 | Srinivasan | Feb 2021 | B2 |
| 11072044 | Ozbaysal et al. | Jul 2021 | B2 |
| 11090770 | Srinivasan | Aug 2021 | B2 |
| 11203064 | Ozbaysal | Dec 2021 | B2 |
| 20150290747 | Ozbaysal | Oct 2015 | A1 |
| 20170197283 | Perez | Jul 2017 | A1 |
| 20180347013 | Szuromi et al. | Dec 2018 | A1 |
| 20210140015 | Engeli et al. | May 2021 | A1 |
| 20210331239 | Izumi | Oct 2021 | A1 |
| 20210402475 | Taneike | Dec 2021 | A1 |
| Number | Date | Country |
|---|---|---|
| 3257956 | Dec 2017 | EP |
| 3131697 | Mar 2021 | EP |
| 2486046 | Dec 2012 | GB |
| 2021021231 | Feb 2021 | WO |
| 2021021232 | Feb 2021 | WO |
| Number | Date | Country | |
|---|---|---|---|
| 20220234101 A1 | Jul 2022 | US |
| Number | Date | Country | |
|---|---|---|---|
| 63286202 | Dec 2021 | US | |
| 63229753 | Aug 2021 | US | |
| 63142540 | Jan 2021 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 17577607 | Jan 2022 | US |
| Child | 17649281 | US |