Distorted helix ferroelectric liquid crystal cell

Information

  • Patent Grant
  • 6671028
  • Patent Number
    6,671,028
  • Date Filed
    Thursday, November 17, 1994
    30 years ago
  • Date Issued
    Tuesday, December 30, 2003
    20 years ago
Abstract
A liquid crystal display cell comprising a chiral ferroelectric smectic liquid crystal layer whose helix structure is influenced by the action of an electric field such that its optical anisotropy alters; a pair of transparent plates between which the liquid crystal is disposed and which have a surface structure for aligning the molecule of the liquid crystal and are provided with electrodes to produce an electric field therein; and one polarizer each before and after the liquid crystal, such that a ratio d/p of the thickness d of the liquid crystal layer to the pitch height p of the helical twisting is greater than 5, the smectic tilt angle θo between 0.39 radians and 0.87 radians and the product d·θ2·Δn·1/λ (phase factor) of the thickness d, the square of the tilt angle θ°, the value of the birefringence Δn and the reciprocal of the wavelength λ of light bending is greater than 0.45 radians2.
Description




BACKGROUND OF THE INVENTION




1. Field of the Invention




This invention relates to ferroelectric liquid crystal displays and compounds and mixtures for use in such displays.




More particularly, the invention relates to a liquid crystal display cell having a chiral ferroelectric smectic liquid crystal layer whose helix structure is so influenced by the action of an electric field that its optical anisotropy alters; a pair of transparent plates between which the liquid crystal is disposed and which have a surface structure aligning the molecules of the liquid crystal and are provided with electrodes to produce an electric field therein; and one polariser each before and after the liquid crystal. The invention also relates to chiral or optically active compounds and liquid crystal mixtures for use in the cell and the use of the compounds for electro-optical purposes.




2. Description




The effect of distorting a helix structure of a ferroelectric liquid crystal cell hereinbefore set out by an electric field has been described in Ostrovski, B. I., Advances in Liquid Crystal Research and Applications, Oxford/Budapest, 1980, pp. 469 et seq. The effect is sometimes referred to in the literature by the abbreviation DHF for “distorted helix ferroelectric”. The article of Ostrovski considers the possibility of modulating a light beam at a frequency of 1 kHz and using an electric field of less than 6×10


3


V/cm. Subsequently, however, it was apparently found that this effect does not lead to an electro-optical cell which is usable in practice.




A known effect, but of a different kind, is Lagermall and Clark's surface stabilized ferroelectric liquid crystal (SSFLC) in which ferroelectric liquid crystals are used in an untwisted configuration. This effect has been described in Mol. Crystal. Liq. Crystal. 94 (9183), 213-234 and 114 (1984), 151-187.




SUMMARY




As described hereinbelow, the present invention provides a distorted helix ferroelectric (DHF) cell which has not only the known advantages of the DHF effect but also the properties necessary for practical use as a light shutter or display cell.




According to the invention, this is achieved by a DHF cell of the kind hereinbefore set out wherein the ratio d/p of the thickness d of the liquid crystal layer to the pitch height p of the helical twisting is greater than 5, the smectic tilt angle θ


o


is between 22.5° and 50° and the product d·θ


o


2·Δn·1/λ is greater than 0.1 (radians)


2


. Δn denotes the birefringence and λ denotes the wavelength of the light.











BRIEF DESCRIPTION OF THE DRAWINGS




Embodiments of the invention will be described hereinafter with reference to the accompanying drawings wherein:





FIG. 1

is a diagrammatic perspective illustration of a small portion of a liquid crystal cell according to a preferred embodiment of the invention, and





FIG. 2

is a graph in which storage time is plotted against applied voltage.











DESCRIPTION OF THE PREFERRED EMBODIMENT




As shown in

FIG. 1

, the liquid crystal cell according to the invention comprises a liquid crystal layer


1


disposed between two plates


2


,


3


which are disposed in substantially plane-parallel relationship to one another and which are made of a transparent material such as glass, acrylic glass, plastics, foils or the like. A polariser


4


is disposed before the front plate


2


and is preferably disposed or secured thereto, for example, by sticking. This is also known as the input-side polariser. A polariser


5


is correspondingly associated with the rear plate


3


. The plates are spaced apart from one another by a distance d (d not indicated on FIG.


1


).




The plate surfaces near the liquid crystal have conventional electrode coatings which are segmented to represent characters or image dots. Referring to the cell portion shown in

FIG. 1

, a single electrode segment


5


is shown on plate


2


and an opposite electrode segment


7


is shown on rear plate


3


.




Also, the surfaces near the liquid crystal are so treated by conventional surface aligning technique so as to exert a directional effect on the adjacent liquid crystal molecules and thus to determine the direction of the director. This treatment consists, for example, or rubbing the surface in one direction to produce a planar orientation. Other possibilities are the use of oblique vapor coating of orienting layers, etc. The result of such treatment will be referred to for the purposes of this description as surface orientation. The surface orientation on the two plates is indicated by arrows on FIG.


1


. The surface orientation on the rear plate


3


is parallel to that on the front plate so as to obtain the characteristic planar orientation. As well as planar surface orientation, homeotropic orientation or combinations of both can be considered and are contemplated by the invention.




Polariser


4


associated with the front plate is so disposed as to include an angle β with the direction of the surface orientation or with the helix axis of the liquid crystal molecules. Polariser


3


associated with the rear plate is positioned at a 90° offset from the front polariser. This arrangement of the polarisers is a preferred embodiment. Other polariser arrangements which also gives satisfactory results are possible. Appropriate polarizer arrangements of various crossings can readily be determined by simple optimizing by a skilled artisan.




Liquid crystal


1


is a conventional chiral smectic ferroelectric liquid crystal often referred to in the literature as smectic C. Liquid crystals of this kind are known from the literature. Their distinguishing feature is that their molecules are arranged relatively to the smectic planes not perpendicularly but at a particular angle known as the smectic tilt angle θ


o


. The chirality resides in that the molecule directions are not parallel to one another in all the layers but are twisted relatively to one another from layer to layer to give overall a helical twisting. In the case of a planar surface orientation, the axis of this helical twisting is aligned parallel to the plates.

FIG. 1

shows one molecule


8


per smectic layer and illustrates the helical twisting of the molecules relatively to one another along a helix axis


9


, the twisting continuing from layer to layer. The smectic tilt angle θ


o


is the angle between the molecule longitudinal axis and the helix axis


9


. When no field is acting on the liquid crystal the pitch height of the helix is p


o


.




When a potential or voltage is applied to electrodes


6


and


7


, an electric field is produced in the liquid crystal which reorientates the molecules. In practice the symbolically indicated voltage source


10


of

FIG. 1

delivers periodic signals or trigger pulses which in the case of the present cell may be of opposite polarity, as will be described in detail hereinafter. In its normal state—i.e., in the absence of applied electric field—the cell has a particular light transmittance. The application of an electric field distorts the helix arrangement of the molecules so that the optical anisotropy and thus the light transmittance is altered. There is an optical contrast between the two states. Basically, the helix structure distortion produced by the electric field alters the pitch height.




Depending on the relationship between light intensity and applied voltage, two different forms of operation are possible in the on state, i.e., linear operation, in which light intensity is directly proportional to the applied voltage, and quadratic operation, in which light intensity is proportional to the square of the voltage.




The effect occurs when the light beam passing through the liquid crystalline structure encounters an aperture a corresponding to a number of periods p of the helical structure. The electrooptical output effect is transmitted in this way along the helix direction.




There are a number of important differences between the effects in which the helical structure is completely cancelled, such as the prior art SSFLC effect, and the effect of the present invention these differences are described below:




1. The operating voltage depends upon the smectic tilt angel θ


o


, the polarization in the untwisted state and the ratio d/p


o


of layer thickness to pitch height and is usually lower than the voltage Uu required to cancel the helix. The range of operating voltages can be widened by increasing the ratio d/p


o


and enlarging the smectic tilt angle θ


o


.




2. The effect has a satisfactory modulation depth, a high contrast ratio and a grey scale approximately proportional to the applied voltage.




3. The effect permits a storage or memory effect controlled by the amplitude of the applied voltage. This is shown in

FIG. 2

wherein on the horizontal axis the applied voltage U relative to the voltage Uu to unwind the helix is given and on the vertical axis the return time t


r


for the helical structure to return to the initial state relative to the time t


o


for the return from a slightly disturbed to the initial state is given. t


o


is a material constant proportional to the 1/p


o




2


. The curve shows that the time ratio increases over-proportional with the voltage.




The times t


o


and t


r


taken for the structure to return to the original undisturbed helix shapes depend upon the viscosity and the elastic constants of the liquid crystal material and upon the pitch height of the helix. The storage time is also affected by surface conditions. For low pitch height values the storage time can be varied from very low values of approximately 10-100 μsec to high values of 5-10 sec.




4. The effect is based on minor variations of the director orientation and does not alter the disinclination walls in the indication zone. Consequently, there are no delay times in display operation.




5. In the planar configuration the effect is not sensitive to wall orientation. Conventional methods of wall orientation can be used as in nematic liquid crystals.




6. The effect permits the use of biopolar signals and of harmonic fields having a characteristic frequency f.




7. By means of appropriate control signals, optical phase differences can be so produced by the effect in the liquid crystal layer as to facilitate a color change over.




As previously stated, d/p


o


ratio parameters of greater than about 5 are preferred, those greater than about 10 being particularly preferred. The smectic tilt angle θ


o


is preferably from about 25° to about 40°. Also, the value of the so-called phase factor







d






θ
o
2


Δn

λ










is more than about 0.45 (radians)


2


and particularly preferably, more than about 1.




Preferably, the liquid crystal consists of the following mixture: 26.1 wt. % 5-octyl-2-[p-(octyloxy)phenyl] pyrimidine, 17.1 wt. % 5-octyl-2-[p-(nonyloxy)phenyl] pyrimidine, 24.5 wt. % 5-octyl-2-[p-(decyloxy)phenyl] pyrimidine, 32.3 wt. % of the chiral additive:











As a rule, there can be used as chiral additives compounds having the formula:











wherein R


1


and R


2


denote independently of one another alkyl having at least 2 to 20 carbon atoms and each C* denotes a chiral carbon atom.




The formula I and formula II compounds are novel and also are the subject of this invention. They induce a very high spontaneous polarization in the liquid crystal mixture and are chemically stable, colorless and readily soluble in conventional liquid crystal materials, more particularly in ferroelectric smectic liquid crystals.




The term “alkyl having at least 2 carbon atoms” covers straigh-chain and branched groups, more particularly straigh-chain alkyl having at least 2 carbon atoms and isoalkyl, such as ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, hexyl, heptyl, octyl, nonyl or the like. The alkyl groups R


1


, R


2


preferably each have 2-15, particularly preferably 2-9, carbon atoms. R


1


and R


2


may have different significance but preferably have the same significance.




The configuration at the chirality centers in formula II is preferably such that the chiral groups induce a spontaneous polarization in the same sense. Preferably, the two chiral carbon atoms are present in S-configuration or in R-configuration, more particularly when R


1


and R


2


have the same significance.




The formula II compounds can be prepared in a known manner by conventional esterification methods from 4,4″-p-terphenyldicarboxylic acid and 2-alkanols. The starting material are known compounds, analogues of known compounds or can be made from known compounds by convention techniques.




The formula II compounds are particularly suitable as chiral doping agents for liquid crystalline mixtures. The invention therefore also relates to a liquid crystalline mixture having at least two components, characterized in that at least one component is an optically active formula II compound. Preferably, the mixture contains a liquid crystal material having a tilted smectic phase and one or more optically active formula II compounds.




The proportion of formula II compounds in the mixtures according to the invention can vary within wide limits and can be, for example, approximately from about 0.5 to about 30 wt. %. A range of approximately 1-10 wt. %. is generally preferred and a range of approximately from about 3 to about 10 wt % is particularly preferred.




The liquid crystal material having a tilted smectic phase can consist of conventional materials. Materials having a smectic C-phase, such as derivatives of phenylpyrimidine, phenylpyridine, phenylbenzoate, benzoate acidbiphenylester and 4-biphenylcarboxylic acid-phenylester having a smectic C-phase are preferred.




In a preferred cell having this liquid crystal mixture, the pitch height p


o


is about 0.3 to about 0.4μ at 25° C. and the birefringence Δn is about 0.25. The smectic tilt angel θ


o


is approximately about 29° at room temperature (about 20° C.). The spontaneous polarization P


s


is approximately 7.10


−9


c/cm


2


at 25° C. Rotation viscosity is approximately 1 poise. The liquid crystal layer in the cell has a thickness of about 3.6 μm. The voltage Uu needed for complete cancellation of the helix structure is approximately 2 V. The response time for this cell is approximately 200 μsec. The response time for the entire applied voltage range O<U<Uu is approximately of the same length.




The approximate preferred values for the angel β are β=22.5° (π/8) or β=67.5° (3π/8) for linear operation, and β=0°, β=45° (π/8), or β=90° (π/2) for quadratic operation.




The resulting cell provides a contrast of more than 100:1. The following table lists the intensity values I for a series of voltage amplitudes by using the inventive cell. The voltage is in the form of rectangular pulses. The values are for linear operation.















TABLE











U[V]




I[%]



























0




1







0.15




10







0.25




20







0.45




35







0.5




55







1.0




90







1.5




99







1.75




98







2.0




97







2.45




80







2.6




65







2.95




50







3.3




40







4.0




35







5.15




35















The maximum intensity value is 100%. The first values in the 0-2 volts voltage range indicate the obtainable grey scale. Contrast decreases above 2 volts due to the higher smectic tilt angle. The helix unwinds completely at voltages above 4.0 volts.




The preparation of formulation II compound will be described hereinafter with reference to the following example.




EXAMPLE 1




A solution of 2 g of 4.4″-p-terphenyldicarboxylic acid dichloride (which can be prepared by conventional techniques by reacting 4,4″-p-terphenyldicarboxylic acid with thionyl chloride in pyridine at 80° C.) in 200 cc of dry pyridine was mixed with 1.59 g of S-(+)-2-oxtanol and agitated at 20° C. for 24 hours. This reaction mixture was then poured onto a mixture of ice and dilute dydrochloric acid. The crystalline product is filtered off, washed in water and dried in a high vacuum. Chromatographic purification and recrystallization yielded pure 4.4″-Di-[2(S)-octyloxycarbonyl]-p-terphenyl with a melting point of 81-82° C.




The following compounds can be prepared similarly:




4,4″-di-[2(S)-octyloxycarbonyl]-p-terphenyl;




4,4″-di-[2(R)-octyloxycarbonyl]-p-terphenyl;




4,4″-di-[2(S)-heptloxycarbonyl]-p-terphenyl;




4,4″-di-[2(R)-heptloxycarbonyl]-p-terphenyl;




4,4″-di-[2(R)-octyloxycarbonyl]-p-terphenyl;, melting point 81-82° C.;




4,4″-di-[2(S)-nonyloxycarbonyl]-p-terphenyl;




4,4″-di-[2(R)-nonyloxycarbonyl]-p-terphenyl;




4,4″-di-[2(S)-decyloxycarbonyl]-p-terphenyl;




4,4″-di-[2(R)-decyloxycarbonyl]-p-terphenyl;




Spontaneous polarization Ps was examined by means of a mixture of 5 wt. % 4.4″-di-[2(S)-octyloxycarbonyl]-p-terphenyl and 95 wt. % 4-octyloxybenzoic acid-4-hexyloxyphenylester. The mixture had a Ps value of 8.8 nC/cm


2


at 40° C. The extrapolated Ps value for 4,4″-di-[2(S)-octyloxycarbonyl]-p-terphenyl is 176 nC/cm


2


at 40° C.




While the invention has been described in conjunction with certain embodiments, it is understood that various modifications and changes may be made with out departing from the spirit and scope of the invention.



Claims
  • 1. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 10, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians.
  • 2. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is about 0.5 radians.
  • 3. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians, and further wherein the product of the thickness d, the square of the tilt angle θo, the value of the birefringence Δn, and the reciprocal of the wavelength λ of light is greater than about 1 radians2.
  • 4. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians, and further wherein the angle β between a helix axis of the liquid molecules and the polarization axis of the front polarizer is about 22.5°, or about 67.5° when the cell is operated in a form in which the intensity of the transmitted light is proportional to the applied potential.
  • 5. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians, and further wherein the angle β between a helix axis of the liquid molecules and the polarization axis of the front polarizer is about 0°, or about 45°, or about 90° when the cell is operated in a form in which the intensity of the transmitted light is proportional to the square of the applied potential.
  • 6. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians, and further wherein the surface orientation means aligns the liquid crystal molecules planarly.
  • 7. An electro-optical cell comprising:a) front and rear transparent plate means; b) means for applying an electric potential to the plate means; c) a chiral ferroelectric smectic liquid crystal layer disposed between the plate means and having a helical structure which is influenced by the action of the electric potential means so as to alter its optical anisotropy; and d) surface orientation means disposed on each surface of the plate means adjacent the liquid crystal so as to align the molecules of the liquid crystal in a predetermined manner; and e) front and rear polarizers disposed respectively on the surface of the front and rear plate means opposite to the surface orientation means, wherein a ratio d/p of the thickness d of the liquid crystal layer to a pitch height p of a helical twisting is greater than about 5, and a smectic tilt angle θo is between about 0.39 radians and about 0.87 radians, and further wherein the polarizers are disposed on the two plate means such that the polarization direction of each polarizer are crossed.
  • 8. The cell of claim 7 wherein the polarizers are disposed on the plate means such that the polarization direction of each polarizer are crossed at about 90°.
Priority Claims (4)
Number Date Country Kind
3607/87 Sep 1987 CH
3640/87 Sep 1987 CH
3722/87 Sep 1987 CH
1555/88 Apr 1988 CH
Parent Case Info

This is a continuation of U.S. application Ser. No. 08/200,939, filed Feb. 23, 1994 now abandoned, which is a continuation of U.S. application Ser. No. 08/076,487, filed Jun. 14, 1993, now abandoned, which is a continuation of U.S. application Ser. No. 07/964,482, filed Oct. 21, 1992, now abandoned, which is a continuation of U.S. application Ser. No. 07/771,824, filed Oct. 7, 1991, now abandoned, which is a continuation of U.S. application Ser. No. 07/641,953, filed Jan. 16, 1991, now abandoned, which is a continuation of U.S. application Ser. No. 07/243,756, filed Sep. 13, 1988, now abandoned.

US Referenced Citations (14)
Number Name Date Kind
3972587 Scheffer Aug 1976 A
4592623 Yamamoto et al. Jun 1986 A
4668051 Mourey et al. May 1987 A
4715688 Harada et al. Dec 1987 A
4753752 Raynes et al. Jun 1988 A
4813767 Clark et al. Mar 1989 A
4832462 Clark et al. May 1989 A
4852978 Davey et al. Aug 1989 A
4917475 Meyer et al. Apr 1990 A
4927244 Bahr et al. May 1990 A
4966727 Ichihashi et al. Oct 1990 A
4988459 Scherowsky et al. Jan 1991 A
5046830 Nakanowatari Sep 1991 A
5381253 Sharp et al. Jan 1995 A
Foreign Referenced Citations (9)
Number Date Country
219480 Oct 1986 EP
0 283 916 Sep 1988 EP
2198743 Jun 1988 GB
58-173718 Oct 1983 JP
60-60625 Apr 1985 JP
61-241724 Oct 1986 JP
62-159118 Jul 1987 JP
62-160420 Jul 1987 JP
8706021 Oct 1987 WO
Non-Patent Literature Citations (20)
Entry
Lagerwall et al “Ferroelectric Liquid Crystals For Displays” 1985 International Display Research Conference IEEE-Oct. 85-pp. 213-221.*
F. Allan “The Optimization of Twisted Nematic Display Thickness” Information Display—Oct. 1983—pp. 14 and 16.*
F. Sears et al “University Physics” Sixth Edition Chapter 1—Section 1-3 “Unit Consistency and Conversions” pp. 4 and 5.*
Beresnev et al “Electro-Optical Response of a Thin Layer of a Ferroelectric Liquid Crystal With a Small Pitch and High Spontaneous Polarization” Ferroelectrics, sep. 1988, vol. 85, pp. 173-186 or pp. 561-574, Sep. 1988.*
Clark, et al., Mol. Cryst. Liq. Crst., vol. 94, pp. 213-233 (1983).
Brunet, et al., “Optical Properties of a Twisted Smectic C”, Physics Abstracts, 7(130) pp. 1-321-324.
Lagerwall, et al., Mol. Cryst. Liq. Crst., vol. 114, pp. 151-187 (1984).
Beresnev, et al., “Fast Optoelectronic Switch Using a Type C Smectic Doped With a Chiral Impurity”, American Institute of Physics, pp. 1296-1297 (1985).
Inuko, Patent Abstracts of Japan, vol. 7, No. 131 (C-169), p. 1276 (Jun. 1983), Abstract of Jap. Pat. 58-46040.
Satou, Patent Abstracts of Japan, vol. 7, No. 14 (C-146), p. 119 (Jan. 20, 1983), Abstracts of Japan Pat. 56-56504.
Sugimori, Patent Abstracts of Japan, vol. 9, No. 1 (C-259), p. 1724 (Jan. 5, 1985) Abstract of Jap. Pat. 59-157056.
Lagerwall, et al., “Ferroelectric Liquid Crystals For Displays” 1985 International Display Research Conference, IEE-Oct. 85, pp. 213-221.
Ostrovski, et al., “Behavior of Ferroelectric Smectic Liquid Crystals in Electric Field”, Advances in Liquid Crystal Research and Applications, 1980, pp. 469-482.
Clark et al., Mol. Cryst. Liq. Crst., vol. 94, pp. 213-233 (1983).
Brunet et al., “Optical Proper of a Twisted Smectic C” Physics Abstracts, 7(130) pp. 1-321-324.
Lagerwall et al., Mol. Cryst. Liq Cryst., vol. 114, pp. 151-187 (1984).
Beresnev et al., “Fast Optoelectronic Switch Using a Type C Smectic Doped with a Chiral Impurity”, American Institute of Physics pp. 1296-1297 (1985).
Inuko, Patent Abstracts of Japan, vol. 7, No. 131 (C-169), p. 1276 (Jun. 8, 1983), Abstract of Jap. Pat. 58-46040.
Satou, Patent Abstracts of Japan, vol. 7, No. 14 (C-146), p. 119 (Jan. 20, 1983), Abstract of Jap. Pat. 56--56504.
Sugimori, Patent Abstracts of Japan, vol. 9, No. 1 (C-259), p. 1724 (Jan. 5, 1985), Abstract of Jap. Pat. 59-157056.
Continuations (6)
Number Date Country
Parent 08/200939 Feb 1994 US
Child 08/340816 US
Parent 08/076487 Jun 1993 US
Child 08/200939 US
Parent 07/964482 Oct 1992 US
Child 08/076487 US
Parent 07/771824 Oct 1991 US
Child 07/964482 US
Parent 07/641953 Jan 1991 US
Child 07/771824 US
Parent 07/243756 Sep 1988 US
Child 07/641953 US