1. Field of the Invention
The present invention relates to an Echelle diffraction grating, an excimer laser using the same, and their manufacturing methods.
2. Description of the Related Art
A diffraction grating used for the wavelength selection (or narrow band) in an excimer laser serves as an optical element of a laser resonator, and thus needs a high diffraction efficiency and durability for a long-term service. One applicable diffraction grating is an Echelle diffraction grating (blazed diffraction grating) that has an asymmetrical triangular shape on a grating section.
For example, Japanese Patent No. 4,549,019 proposes a method for protecting an Al reflective film surface from being oxidized and deformed, by layering a protective film containing Al2O3 on the reflective film of each grating in the reflective Echelle diffraction grating. In order to propose a method of realizing a high initial value of the diffraction efficiency in the laser installation, U.S. Patent Application Publication No. 2009/0027776 adjusts a thickness of a protective film and U.S. Patent Application Publication No. 2010/0328775 adjusts a groove shape of a diffraction grating.
It is found that a ratio of the diffraction efficiency (orientation ratio) between the blazed order and an order lower by one than the blazed order after a laser beam is irradiated onto the Echelle diffraction grating is different from that before the laser irradiation. This difference means a deformation of a grating groove, and causes the diffraction efficiency of the blazed order to lower. The methods of U.S. Patent Application Publication Nos. 2009/0027776 and 2010/0328775 are insufficient as solutions for this problem.
The present invention provides an Echelle diffraction grating that can maintain diffraction efficiency for a long-term service, an excimer laser using the same, and their manufacturing methods.
A manufacturing method of an excimer laser that includes a light source configured to emit ultraviolet light, and a reflective Echelle diffraction grating in which each grating has an asymmetrical triangular shape on a section in which a plurality of gratings are arranged includes the steps of obtaining information of a wavelength of a light source, a blazed order set for incident light having the wavelength, a repetitive pitch of the grating, a material of the grating, and an orientation ratio B/A that is a ratio between that a diffraction efficiency A of the blazed order and a diffraction efficiency B of an order lower by one order than the blazed order which satisfies: 0.025≦B/A≦0.400, and presenting an available range of an initial value of a blaze angle that is an angle between a blazed surface and a lattice plane of each grating.
Further features of the present invention will become apparent from the following description of exemplary embodiments with reference to the attached drawings.
Each grating includes a blazed surface 3 that is a facet with a short side of an asymmetrical triangular shape on the section illustrated in
An angle between the blazed surface 3 and a lattice plane (grating plane) 4 is referred to as a blaze angle 5. An angle between the blazed surface 3 and the counter surface 8 is referred to as an apex angle 6. Reference numeral 7 denotes a repetitive pitch. While the apex angle 6 is not particularly limited in the present invention, the apex angle 6 of this embodiment is set to an angle smaller than 90° (in particular in a range between 85° and 90°). This is because the incident light 2 reaches the counter surface 8 when a sum of the apex angle 6 and the blaze angle 5 is larger than a sum of the incident angle θ of the light and 90°, and thus this configuration attempts to prevent the light from entering the counter surface when the effective blaze angle 5 and incident angle θ are considered.
An order having the highest diffraction energy amount is referred to as a “blazed order” among light fluxes in a certain usable order range of a predetermined wavelength incident at a predetermined incident angle upon the Echelle diffraction grating 1. A configuration of the Echelle diffraction grating in which the incident light and the diffracted light of the blazed order have equal paths is referred to as a “Littrow configuration.” The Echelle diffraction grating 1 has the Littrow configuration. While this embodiment discusses the Echelle diffraction grating having a Littrow configuration in an example, the present invention is not limited to this embodiment and is applicable, for example, to an Echelle diffraction grating having a Czerny-Turner mounting configuration.
As illustrated, in the Echelle diffraction grating 1 having the Littrow configuration, the incident angle θ of the incident light having the blazed order is equal to an angle between the incident light 2 and a grating normal 9 perpendicular to the lattice plane 4. The incident light 2 may perpendicularly enter the blazed surface 3, but enters the blazed surface 3 slightly obliquely in this embodiment. Therefore, in this embodiment, the angle θ of the blazed order is close to but is not equal to the blaze angle 5.
It is known that the following conditional expression is satisfied in the Echelle diffraction grating 1 having the Littrow configuration, where m is a blazed order, λ is a wavelength of the light source of the incident light 2 (therefore which is 193.3 nm in this case), d is a repetitive pitch 7, and θ is an angle of the blazed order:
mλ=2d·sin θ (1)
It is understood from Expression 1 that the order m is uniquely determined once the angle θ if the incident light 2, the repetitive pitch 7, and the wavelength λ of the incident light source are selected. The incident light 2 enters the blazed surface 3 so that Expression 1 is satisfied.
The resin layer 11 has a thickness between 2 μm and 10 μm, and the reflective coating layer 12 has a thickness between 120 μm and 500 μm. The structure illustrated in
As illustrated in
The conventional Echelle diffraction grating having an initial value of a blaze angle 5 of 80.49° has an initial value of the diffraction efficiency of 62.3% but its diffraction efficiency after irradiations of the twenty billion pulses of the laser beams drops down to 34.2%.
As a result of investigating this cause by addressing an orientation ratio B/A that is a ratio between that a diffraction efficiency “A” of the blazed order m and a diffraction efficiency “B” of an order (m−1) lower by one order than the blazed order, it is found that when the Echelle diffraction grating is used for the ArF excimer laser, the reflective coating layer of the blazed surface 3 or the resin layer under the blazed surface 3 deform and the orientation ratio B/A increases.
As a result of the deformation, a direction of a diffracted light flux changes and the diffraction efficiency lowers. Due to this efficiency deterioration and an efficiency deterioration caused by the surface composition change that is a cause different from the triangular shape, the diffraction efficiency lowers and deviates from a permissible range for the laser application when it is lowered down to 34.2% as described above.
The conventional Echelle diffraction grating initially has high diffraction efficiency. Nevertheless, its diffraction efficiency lowers when the laser irradiation amount become higher, and finally deviates from the permissible range.
According to the Echelle diffraction grating 1 of this embodiment, the initial grating shape is determined so that the orientation ratio B/A that is a ratio between that the diffraction efficiency “A” of the blazed order m and the diffraction efficiency “B” of an order (m−1) lower by one order than the blazed order can become between 0.025 (2.5%) and 0.400 (40%). In other words, in the initial shape, the orientation ratio “B/A” satisfies the following conditional expression. Thereby, the life of the Echelle diffraction grating 1 is extended. The grating shape contains the blaze angle 5, the apex angle 6, and the repetitive pitch 7, and the blaze angle 5 is set so that the following conditional expression is satisfied:
0.025≦B/A≦0.400 (2)
A value of the orientation ratio is set so that the efficiency can increase and then decrease due to the deformation in the laser irradiations. As described above, the conventional Echelle diffraction grating has a first blaze angle (80.49°) that maximizes the efficiency of the blazed order as an initial value of the blaze angle 5. On the other hand, this embodiment sets a second blaze angle smaller than the first blaze angle to the initial value of the blaze angle 5. In addition, Expression 2 is used to determine how much amount the second blaze angle is smaller than the first blaze angle.
The orientation ratio smaller than 0.025 weakens the restraining effect of the efficiency deterioration caused by the grating deformation, and the orientation ratio larger than 0.4 causes the initial diffraction efficiency to become remarkably low and the average diffraction efficiency lowers. This numerical range is obtained by investigating the blaze angle dependency of the orientation ratio upon the apex angle 6 and the repetitive pitch 7, then by limiting the apex angle 6 and repetitive pitch 7 to the actually usable ranges, and by finding a range in which the diffraction efficiency of the Echelle diffraction grating 1 is maintained for a long term.
By setting the blaze angle 5 utilizing the relationship illustrated in
The blazed surface 3 that receives the laser beam gradually deforms and the orientation ratio “B/A” changes as if the blaze angle increases in
In
The initial diffraction efficiency of 62.3% in the conventional Echelle diffraction grating is higher than the initial diffraction efficiency of 55.2% of the Echelle diffraction grating 1 of this embodiment. However, the diffraction efficiency of this embodiment after the 20 billion pulses becomes 48.0% and remarkably surpasses the conventional diffraction efficiency of 34.2% after the 20 billion pulses. For example, the laser irradiation amount that provides the diffraction efficiency of 35% is 19 billion pulses for the conventional diffraction grating but 36 billion pulses for the Echelle diffraction grating 1 of this embodiment. Therefore, the durability (life) improves 1.89 times. Referring now to
Regarding the efficiency variation amount during the irradiation, the initial efficiency of the conventional example decreases 62.3% to 34.2% which corresponds to 54.8% of the initial efficiency, and does not appear to correspond to about 70% of 80.49°+1.4°=81.89°. Apparently, this is due to a cause other than the shape change such as a composition change on the reflective surface. In other words, the reason why the calculation result does not perfectly accord with the actual efficiency change is regarded as influence of the efficiency drop caused by a physical phenomenon different from the deformation, such as surface oxidation.
In addition, the employed blazed order never changes and is constant irrespective of the grating deformations caused by the irradiations. This is because this angle is maintained constant once the incident angle θ of the incident light 2 illustrated in
A deforming direction may be reversed in
This embodiment also serves as a manufacturing method of an excimer laser having a reflective Echelle diffraction grating 1. This excimer laser includes a light source (not illustrated) configured to emit ultraviolet light having a wavelength, such as 193.3 nm, 248.4 nm, 308 nm, or 351 nm, and the Echelle diffraction grating 1. The incident light from the light source enters the blazed surface 3 so as to satisfy Expression 1.
This manufacturing method includes some steps, and each step can be implemented as a program (software) configured to instruct a computer (processor), such as a PC, to execute a function of each step.
Initially, a user operates an input unit of the computer, and inputs a wavelength λ of a light source of Expression 1 (such as 193.3 nm), a blazed order m, and a repetitive pitch d. The applicable wavelength λ of the light source can be 193.3 nm of the ArF excimer laser, 248.4 nm of the KrF excimer laser, etc. An example of the applicable blazed order m can be selected from a range between 96th order and 114th order for the ArF excimer laser, or between 74th order and 89th order for the KrF excimer laser.
Next, a user determines an orientation ratio B/A between the diffraction efficiency “A” of the blazed order and the diffraction efficiency “B” of the order (m−1).
In addition, the user inputs information of a material of the diffraction grating (such as a base, a resin layer, a reflective coating layer, and a protective coating layer).
When this information is input (obtained), the computer displays (presents) an available range based upon the set orientation ratio and the deformation tendency of the blazed surface 3 in a map (not illustrated) which illustrates a relationship between the blaze angle (abscissa axis) and the apex angle (ordinate axis). The map (not illustrated) is previously stored in a memory (storage) (not illustrated) of the computer. In response, the user determines (selects) the apex angle 6 and the blaze angle 5 in that range.
When the apex angle 6 is previously determined, the blaze angle 5 may be determined from the graph illustrated in
In the Echelle diffraction grating 1 of the first working example, the repetitive pitch 7 is 10.7081 μm (93.3636 per 1 mm), the blazed order is 109th order, and the apex angle 6 is 85.50°. The light having a wavelength of 193.3 nm emitted from the light source of the ArF excimer laser is irradiated onto the blazed surface 3. The Echelle diffraction grating 1 is used as a reflective diffraction grating for the narrow band in the ArF excimer laser and has a Littrow configuration in which the incident angle and the exit angle are both 79.60°.
Before the laser irradiation, the blaze angle 5 is set so that the orientation ratio B/A can be 0.0889 between the diffraction efficiency “A” of the 109th order as the blazed order and the 108th order on the one order lower side concurrent with the 109th order.
While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments. The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.
This application claims the benefit of Japanese Patent Applications Nos. 2011-222366, filed Oct. 6, 2011, and 2012-198065, filed Sep. 10, 2012, which are hereby incorporated by reference herein in their entirety.
Number | Date | Country | Kind |
---|---|---|---|
2011-222366 | Oct 2011 | JP | national |
2012-198065 | Sep 2012 | JP | national |
Number | Name | Date | Kind |
---|---|---|---|
6067197 | Blasiak et al. | May 2000 | A |
6511703 | Pan et al. | Jan 2003 | B2 |
20020001672 | Pan et al. | Jan 2002 | A1 |
20090027776 | Schall et al. | Jan 2009 | A1 |
20100226014 | Taira et al. | Sep 2010 | A1 |
20100328775 | Kleemann | Dec 2010 | A1 |
20110222042 | Iizuka et al. | Sep 2011 | A1 |
Number | Date | Country |
---|---|---|
4549019 | Sep 2010 | JP |
Entry |
---|
Dmitriy L. Voronov, et al., “5000 groove/mm multilayer-coated blazed grating with 33% efficiency in the 3rd order in the EUV wavelength range”, Advances in X-Ray/EUV Optics and Components IV, Proc. of SPIE, vol. 7448 (Dec. 31 2009), pp. 74480J-1 through 74880J-11. |
Mar. 15, 2013 European Search Report in European Patent Appln. No. 12006853.1. |
Number | Date | Country | |
---|---|---|---|
20130089118 A1 | Apr 2013 | US |