Abstract
A process for the preparation of potassium sulfate, sodium bicarbonate and sodium carbonate. The process involves the treatment of potash brines by the reaction of sodium chloride and potassium chloride with calcium sulfate and sodium sulfate. Syngenite precipitate (CaSO4.K2SO4χH2O) is produced and a first filtrate containing sodium chloride and potassium chloride. The syngenite precipitate is reacted with ammonium bicarbonate at between 70° C. and 100° C., with the result being calcium carbonate precipitate and a second filtrate containing ammonium sulfate and potassium sulfate. The second filtrate is cooled to a temperature of between 20° C. and 50° C. and treated with potassium chloride. A potassium sulfate precipitate results. The sodium bicarbonate is precipitated from the first filtrate by the addition of ammonium bicarbonate to the first precipitate. The sodium bicarbonate may be calcined to form sodium carbonate.
Description




FIELD OF THE INVENTION




The present invention relates to a method for formulating potassium sulfate, sodium bicarbonate and sodium carbonate and more particularly, the present invention relates to a method for formulating such compounds from spent potash brine.




BACKGROUND OF THE INVENTION




In a typical potash plant approximately between 85% and 90% of potassium chloride is recovered. The residual is lost due to washing with water sodium chloride from the sodium chloride during purification procedures. A second cause of the losses is occlusion of the potassium chloride in the sodium chloride tailings.




Tailing ponds are used to collect the excess brine of saturated sodium chloride and potassium chloride with the brine usually being deep well injected for disposal. As an example, for every 1,000,000 tonnes of potassium chloride produced, between 80,000 and 100,000 tonnes of potassium chloride is disposed of by deep well injection.




Generally known techniques are deficient in any clear teachings regarding the methodology set forth above having the following commercial and industrial advantages:




a) production of useful salts from material typically discarded;




b) avoidance of the requirement for deep well injection;




c) use of a nominal amount of energy to synthesize product;




d) use of common equipment widely employed in chemical engineering unit operations; and




e) environmentally friendly protocol devoid of operations which generate pollutants or otherwise adversely affect the soil or air.




There is, therefore, a clear need for a process having these desirable properties; the present invention addresses these needs in an elegant and environmentally conscious manner.




SUMMARY OF THE INVENTION




One object of the present invention is to provide an improved method for formulating useful alkali salts from waste potassium chloride.




A further object of one embodiment of the present invention is to provide a method for forming potassium sulfate from potash brines, comprising the steps of:




providing a source of sodium chloride and potassium chloride in a first step;




reacting the sodium chloride and potassium chloride with calcium sulfate and sodium sulfate;




forming a syngenite precipitate and a first filtrate;




treating the syngenite precipitate with ammonia and carbon dioxide at between 60° C. and 100° C.;




forming calcium carbonate precipitate and a second filtrate;




cooling the second filtrate to a temperature of between 0° C. and 40° C.;




treating the second filtrate with potassium chloride crystals; and




forming potassium sulfate precipitate and a third filtrate.




A further object of one embodiment of the present invention is to provide a method for forming potassium sulfate and sodium bicarbonate from potash brines, comprising the steps of:




forming potassium sulfate in a first phase and sodium bicarbonate in a second phase, the first phase, comprising the steps of:




providing a source of sodium chloride and potassium chloride in a first step;




reacting the sodium chloride and potassium chloride with calcium sulfate and sodium sulfate;




forming a syngenite precipitate and a first filtrate;




treating the syngenite precipitate with ammonia and carbon dioxide at between 50° C. and 100° C.;




forming calcium carbonate precipitate and a second filtrate;




cooling the second filtrate to a temperature of between 0° C. and 40° C.;




treating the second filtrate with potassium chloride solid;




forming potassium sulfate precipitate and a third filtrate, said second phase comprising the steps of:




treating the first filtrate with ammonia or ammonium ions and carbon dioxide; and




forming sodium bicarbonate precipitate.




Having thus described the invention, reference will now be made to the accompanying drawing illustrating preferred embodiments.











BRIEF DESCRIPTION OF THE DRAWINGS





FIG. 1

illustrates an overall schematic representation of the method according to one embodiment of the present invention; and





FIG. 2

is a detailed schematic of FIG.


1


.











Similar numerals employed in the text denote similar elements.




DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS




Referring now to

FIG. 1

, shown is an overall schematic representation of the process according to one embodiment. All amounts are expressed on a percentage by weight basis unless otherwise indicated.




In the embodiment shown, approximately 20% sodium chloride and 10% potassium chloride are added to a mixer


10


together with hydrated calcium sulfate and sodium sulfate. The mixture is filtered in filter


12


, with the filtrate


14


undergoing subsequent treatment (discussed herein after). The precipitate


16


comprises syngenite, CaSO


4


—K


2


SO


4


xH


2


O, and is reacted in vessel


18


with ammonia and carbon dioxide, as an example. The syngenite may also be reacted with ammonium bicarbonate. The reaction preferably is conducted at a temperature of between 30° C. and 100° C. and most desirably at 90° C. The mixture is filtered in filter


20


, with the precipitate comprising calcium carbonate high grade having a brightness of at least +80. The calcium carbonate is subsequently treated by further unit operations to be discussed herein after.




The filtrate from filter


20


is cooled to a temperature of between 20° C. and 40° C. and most desirably at 30° C. Once cooled, the filtrate is reacted in vessel


22


with potassium chloride and filtered in filter


24


to provide a potassium sulfate precipitate and a filtrate containing potassium chloride and ammonium chloride.




Referring now to

FIG. 2

, the filtrate containing potassium chloride and ammonium chloride is concentrated in an evaporator


26


and filtered in filter


28


. The precipitate comprising potassium chloride is recycled to vessel


10


and the filtrate comprising approximately 25% ammonium chloride is passed into vessel


28


. Calcium carbonate from the filtration step at filter


20


is calcined to yield lime and added to vessel


28


. Ammonia gas formed is recycled to ammonium bicarbonate and the mixture is filtered in filter


30


. The precipitate of calcium sulfate is reused and the filtrate, comprising calcium chloride (25%) is disposed of by, for example, deep well injection.




The filtrate from filter


12


(approximately 28% sodium chloride and 2% potassium chloride) is reacted with ammonium bicarbonate (ammonia and carbon dioxide) in vessel


32


and filtered in filter


34


. The result is a precipitate of sodium bicarbonate and ammonium chloride filtrate. The sodium bicarbonate is, for example, calcined to yield sodium carbonate.




As a illustration of the efficacy of the technology set forth herein, the following is representative of the quantitative result.




EXAMPLE




Sample Calculation












Feed






Brine




@





21

%





NaCl











10

%





Kcl




}

&AutoRightMatch;






At





1.24





5.6





















Basis: One (M)


3


of Feed Brine












tonnes





of





NaCl



=




1
×
1.24
×
0.21

=

0.260





t












tonnes





of





KCl



=




1
×
1.24
×
0.10

=

0.124





t












tonnes





of






H
2


O



=





0.856





t






_










Total


=




1.24





t


















Reaction with CaSO


4


.2H


2


O+Na


2


SO


4


+KCl→Ca


2


SO


4


.K


2


SO


4


.x+H


2


O+NaCl0.1 t KCl enter into the reaction














CaSO
4

·
2



H
2


O





required



=





0.1

74


(
2
)



×
172

=


0.116





t

_













Na
2



SO
4






required



=





0.1

74


(
2
)



×
142

=


0.096





t

_














Syngenite produced: (as) Ca


2


SO


4


K


2


SO


4


.4H


2


O








0.1

74


(
2
)



×
382

=



0.258





t

_






of





wet





cake

















The





filtered





exit





brine





contains


:





0.024





t





KCl











0.338





t





NaCl







%





NaCl

=
27.7






0.856





t

_







H
2


O







%





KCl





=




2.0





1.218
_






_



t
_














Syngenite conversion @+90° C.







0.258





t







CaSO
4

·

K
2





SO
4

·
4







H
2






O

+





NH
3

+







CO
2










+

H
2



O
















CaCO
3



+


(

NH
4

)

2





SO
4


+


K
2



SO
4


+


H
2


O










NH
3






required

=



0.258
382

×

(
2
)

×
17

=

0.023





t










CO
2






required

=



0.258
382

×
44

=

0.030





t









CaCO3





produced

=



0.258
382

×
100

=


0.067
_






t











(

NH
4

)

2



SO
4






produced

=



0.258
382

×
132

=


0.089
_






t










K
2



SO
4






produced

=



0.258
382

×
174

=


0.137
_






t















Filtered Solution









0.137
0.18


=

0.761
|





of














H
2


O

_











Brine





make


-


up





is

=





0.137





t






K
2



SO
4













0.089





t







(

NH
4

)

2



SO
4














0.761
_






t






H
2


O












0.987





t





Brine








%






K
2



SO
4


=





13.88

%








%







(

NH
4

)

2



SO
4


=






9.00
_


%








Total





salts

=





22.88

%














Conversion of (NH


4


)


2


SO


4


to K


2


SO


4






The solution is cooled to 30° C.




KCl that reacts with (NH


4


)


2


SO


4


=0.100 t




This makes 0.070 t NH


4


Cl.




Solubility of Cl salts @ 25° C. is 24%




7.09% is NH


4


Cl, 17% needs to added.











Solid





KCl





addition





1

)






0.010





t





for





reaction







2
)








0.168





t

_






for





common





ion





crystallization






Total
=





0.178





t





KCl














K


2


SO


4


Crystallization






Brine





Composition





at





Exit







0.168





t





KCl






0.070





t






NH
4


Cl






0.020





t






K
2



SO
4









0.761





t






H
2


_



O
_







1.019





t





Brine













K


2


SO


4


Production




0.137 t+0.118−0.02=0.235 t




Recovery of KCl from (NH4)Cl brine







at





30

%






NH
4


Cl

,



KCl





is





1

%












0.07





t


(

0.761
-
x

)



=
0.30





0.07
=

0.2283
-

0.3

x







x
=
0.527















Therefore: 0.527 tonnes of H


2


O is to evaporated for every 0.237 t of K


2


SO


4


production.




Evaporative hood 2.22 tonnes H


2


O per tonne of K


2


SO


4






KCl solid is recycled to the K


2


SO


4


production step.




The ammonium chloride is now reacted with lime. (CaO)




0.07 t NH


4


Cl+0.038 t CaO→0.074 t CaCl


2


+0.023 t NH


3







0.023 t of NH


3


gas is recycled and a 30% brine of CaCl


2


is sold or disposed of.




The CaCO


3


precipitated from this process maybe washed and sold as high grade precipitated CaCO


3


for paper coatings or recycled by drying and calcining to produce CaO. The CO


2


may be recovered and recycled using conventional amines.










The





exit





brine





from





the





syngenite





conversion

,

namely





the


:






27.7

%





NaCl








S
.
G
.





1.218




@




25



°






C
.
















2.0

%





KCl

_














Solid NaCl may be added to upgrade saturation, but this is not critical.




This brine is cooled to between 0 and 10° C. and reacted with NH


3


and excess CO


2


or NH


4


HCO


3


.




The process will react with about 90% of the NaCl.









27.7
×
0.9


=

24.93

%





NaCl





reacts





to





produce


:










1.218
×
0.2493

58

×
84

=

0.440





t






NaHCO
3

















Solubility of NaHCO


3


@ 0° C. is 5%.




∴ 1.218×0.05=0.061 t NaHCO


3


(liquid)










yield





of






NaHCO
3






crystals

=

0.44
-
0.061







=


0.379





t






NaHCO
3


_










NaHCO
3






yield

=



0.379
0.44

×
100

=


86.1

%

_












Ammonium Chloride Brine Produced












1.218
×
0.2493

58

×
52

=





0.272





t






NH
4


Cl








1.218
×
0.0277

=





0.034





t





NaCl








1.218
×
0.02

=





0.024





t





KCl








1.218
×
0.05

=





0.061





t






NaHCO
3















0.827





t






H
2


_



O
_













1.218






t
_















Lime required










1
)






for






NH
4


Cl





0.272

53


(
2
)



×
56



=





0.144





t

_






lime







2
)






for






NaHCO
3






0.061


(
84
)



(
2
)



×
56



=





0.020





t

_






lime










Total


=




0.164





t





lime

_













CaCl
2






brine





produced

_

=





0.282





t






CaCl
2








=





0.076





t





NaCl







=





0.024





t





KCl








23.3

%






CaCl
2


=







0.827





t

_







H
2


O













1.209





t

_














This brine can be combined with the exit from the KCl recovery step and further processed to sell CaCl


2


or disposed of.




Ammonia Recycled








0.272
53

×
17

=

0.0872





t






NH
3












The requirements for CO


2


can be made up by recovering CO


2


from calcining CaCO


3


or by using amine stripping units to recover CO


2


from exhaust gas streams.




Key Numbers for Processing






One







(
m
)

3






of





1.24






S
.
G
.




brine






of





saturated





KCl





and





NaCl









K
2



SO
4






produced

=





0.235





t









NaHCO
3






produced

=





0.379





t








Lime





used





as





CaO

=





0.202





t








as






CaCO
3


=






0.361





t

_









Evaporative





load





2.2





t






H2O
_















t






K
2



SO
4








Recycle






NH
3


=

0.157





t
















Although embodiments of the invention have been described above, it is not limited thereto and it will be apparent to those skilled in the art that numerous modifications form part of the present invention insofar as they do not depart from the spirit, nature and scope of the claimed and described invention.



Claims
  • 1. A method for forming potassium sulfate from potash brines, comprising the steps of:providing a source of sodium chloride and potassium chloride in a first step; reacting said sodium chloride and potassium chloride with calcium sulfate and sodium sulfate to form a syngenite precipitate and a first filtrate; treating said syngenite precipitate with ammonium bicarbonate at between 60° C. and 100° C. to form calcium carbonate precipitate and a second filtrate; cooling said second filtrate to a temperature of between 0° C. and 40° C.; and treating said second filtrate with potassium chloride crystals to form potassium sulfate precipitate and a third filtrate.
  • 2. The method as set forth in claim 1, wherein said syngenite precipitate is treated with ammonium bicarbonate at a temperature of 90° C.
  • 3. The method as set forth in claim 1, wherein said first filtrate contains sodium chloride and potassium chloride.
  • 4. The method as set forth in claim 3, further including the step of treating said first filtrate with ammonium bicarbonate to produce a sixth filtrate comprising ammonium chloride and a precipitate of sodium bicarbonate.
  • 5. The method as set forth in claim 4, further including the step of calcining said sodium bicarbonate to form sodium carbonate.
  • 6. The method as set forth in claim 1, wherein said second filtrate is cooled to a temperature of 30° C.
  • 7. The method as set forth in claim 1, wherein said third filtrate contains ammonium chloride and potassium chloride.
  • 8. The method as set forth in claim 7, further including the step of concentrating said third filtrate by evaporation to form a fourth filtrate and potassium chloride precipitate.
  • 9. The method as set forth in claim 8, further including the step of recycling potassium chloride precipitate to said first step.
  • 10. The method as set forth in claim 7, further including the step of calcining said calcium carbonate to form lime.
  • 11. The method as set forth in claim 10, wherein said fourth filtrate is treated with lime to produce a fifth filtrate comprising calcium chloride and a precipitate of calcium sulfate.
  • 12. The method as set forth in claim 1, wherein said calcium carbonate comprises high grade calcium carbonate having a brightness of between +80 and +95.
  • 13. A method for forming potassium sulfate and sodium bicarbonate from potash brines, comprising the steps of:forming potassium sulfate in a first phase and sodium bicarbonate in a second phase, said first phase, comprising the steps of: providing a source of sodium chloride and potassium chloride in a first step; reacting said sodium chloride and potassium chloride with calcium sulfate and sodium sulfate to form a syngenite precipitate and a first filtrate; treating said syngenite precipitate with ammonium bicarbonate at between 50° C. and 100° C. to form calcium carbonate precipitate and a second filtrate containing ammonium sulfate and potassium sulfate; cooling said second filtrate to a temperature of between 0° C. and 40° C.; treating said second filtrate with potassium chloride solid to form potassium sulfate precipitate and a third filtrate, said second phase comprising the steps of: treating said first filtrate with ammonium bicarbonate to form sodium bicarbonate precipitate.
  • 14. The method as set forth in claim 13, further including the step of calcining said sodium bicarbonate to sodium carbonate.
  • 15. The method as set forth in claim 13, wherein said second filtrate is cooled to a temperature of 30° C.
  • 16. The method as set forth in claim 13, wherein said syngenite is treated at a temperature of 90° C.
US Referenced Citations (57)
Number Name Date Kind
1824361 Morse Sep 1931 A
1922682 Holz Aug 1933 A
1936070 Ritchie et al. Nov 1933 A
1990896 Connell Feb 1935 A
2882128 Lafont Apr 1959 A
3206297 O'Connor Sep 1965 A
3369867 May Feb 1968 A
3429657 George et al. Feb 1969 A
3436175 Atwood Apr 1969 A
3502458 Schenk Mar 1970 A
3527592 McPherson et al. Sep 1970 A
3528767 Garrett Sep 1970 A
3533776 Coates Oct 1970 A
3539326 Otsuka et al. Nov 1970 A
3544296 Karcher Dec 1970 A
3578399 Boeglin May 1971 A
3617243 Neitzel Nov 1971 A
3656891 Chemtob Apr 1972 A
3687639 Barlow et al. Aug 1972 A
3711254 McGowan et al. Jan 1973 A
3728438 Nasygrov Apr 1973 A
3843772 Boeglin Oct 1974 A
3853490 Boeglin et al. Dec 1974 A
3872002 Musgrove Mar 1975 A
3892552 Gay, Jr. Jul 1975 A
3895920 Garrett Jul 1975 A
3998935 Adams et al. Dec 1976 A
4045543 Sardisco Aug 1977 A
4129642 Neitzel Dec 1978 A
4174382 Menche Nov 1979 A
4215100 Sokolov et al. Jul 1980 A
4268492 Sardisco et al. May 1981 A
4303619 Kobayashi et al. Dec 1981 A
4313753 Segawa et al. Feb 1982 A
4323386 Heggabo et al. Apr 1982 A
4342737 Iwashita et al. Aug 1982 A
4385920 Dancy et al. May 1983 A
4420468 Yamashita et al. Dec 1983 A
4440560 Nakamura et al. Apr 1984 A
4529434 Ashmead Jul 1985 A
4533536 Bichara et al. Aug 1985 A
4554139 Worthington et al. Nov 1985 A
4562058 Dancy et al. Dec 1985 A
4588573 Worthington et al. May 1986 A
4668242 Vitellaro et al. May 1987 A
4707347 Vajna et al. Nov 1987 A
4710219 Wahlberg et al. Dec 1987 A
4804401 Wahlberg et al. Feb 1989 A
5152821 Walter Oct 1992 A
5298050 McLaughlin et al. Mar 1994 A
5366534 Fischbein et al. Nov 1994 A
5449506 Berry et al. Sep 1995 A
5529764 Lampert et al. Jun 1996 A
5549876 Zisner et al. Aug 1996 A
5552126 Efraim et al. Sep 1996 A
5571303 Bexton Nov 1996 A
5871551 Rodriguez-Leon Feb 1999 A
Foreign Referenced Citations (4)
Number Date Country
787713 Sep 1935 FR
435772 Sep 1935 GB
2 068 918 Aug 1981 GB
WO 9965823 Dec 1999 WO