High Temperature, Damage Tolerant Superalloy, an Article of Manufacture Made from the Alloy, and Process for Making the Alloy

Information

  • Patent Application
  • 20180100222
  • Publication Number
    20180100222
  • Date Filed
    October 12, 2016
    9 years ago
  • Date Published
    April 12, 2018
    7 years ago
Abstract
A nickel-base alloy is disclosed that has the following weight percent composition. C about 0.005 to about 0.06Cr about 13 to about 17Fe about 4 to about 20Mo about 3 to about 9W up to about 8Co up to about 12Al about 1 to about 3Ti about 0.6 to about 3Nb up to about 5.5B about 0.001 to about 0.012Mg about 0.0010 to about 0.0020Zr about 0.01 to about 0.08Si up to about 0.7P up to about 0.05 and the balance is nickel, usual impurities, and minor amounts of other elements as residuals from alloying additions during melting,. The alloy provides a combination of high strength, good creep resistance, and good resistance to crack growth. A method of heat treating a nickel base superalloy to improve the tensile ductility of the alloy is also disclosed. An article of manufacture made from the nickel base superalloy described herein is also disclosed.
Description
BACKGROUND OF THE INVENTION
Field of the Invention

This invention relates generally to nickel-base superalloys and in particular to a nickel base superalloy that provides a novel combination of high strength, good creep strength, and good resistance to crack growth under stress.


Description of Related Art

Structural alloys that are designed to operate at high temperatures (e.g., ≥1100° F.) typically require high strength and creep resistance. However, as the strength and creep resistance properties are increased in such alloys, the alloys can become more susceptible to environmental effects, namely, oxygen in the atmosphere. This susceptibility can manifest itself as notch brittleness and/or an increase in crack growth rate. With regard to crack growth rate, nickel-base superalloys may be tolerant of this type of damage when fatigue cycled at a relatively fast rate, but an increased sensitivity to damage can occur when the alloy is stressed under low frequency with a dwell hold in each stressing/unstressing cycle. One theory for such sensitivity is that the increased dwell time during the stressing part of the cycle provides time for oxygen to diffuse down grain boundaries to form an oxide layer within the crack. That oxide layer then may act as a wedge when the load is released, advancing the crack tip movement at a faster overall rate.


In nickel-base superalloys, the compositional and structural factors that influence strength and creep resistance properties can also affect crack growth rate. Such factors include the effects of solid solution strengthening, precipitation strengthening (such as with the gamma prime (γ′) precipitate); anti-phase boundary energy; the volume, sizes, and coherency of the precipitates in the matrix; grain size; grain boundary structure; grain boundary precipitation (composition and morphology); as well as low levels of certain potent elements in the grain boundaries. An alloy that creeps to some extent allows creep relaxation to occur at the crack tip (blunting). The general oxidation resistance of the alloy also influences crack growth rate.


In view of the state of the art as outlined above, it has become desirable to have a nickel-base superalloy that provides not only good high temperature strength and creep resistance, but also improved resistance to crack growth during stress cycling in oxidizing environments.


The known heat treatments for precipitation hardenable (PH) Ni-base superalloys typically include a high temperature annealing treatment to solution discrete phases that precipitate in the alloy matrix material. This solution annealing treatment also relieves stresses in the material and modifies the grain size and structure of the alloy. Annealing temperatures may be termed supersolvus and subsolvus depending on whether the annealing temperature used is above or below the solvus temperature of the γ′ precipitate which forms in PH Ni-base superalloys. The solution annealing treatment is followed by a lower temperature aging heat treatment where γ′ and γ″ phases precipitate. The γ′ and γ″ phases are the primary strengthening phases in PH Ni-base superalloys. The aging heat treatment may consist of one or two heating steps that are performed at different temperatures that are selected to cause precipitation of γ′ and in some cases γ″, and to modify the size, morphology, and volume fraction of the γ′ and γ″ precipitates in the alloy.


BRIEF SUMMARY OF THE INVENTION

The disadvantages of the known alloys described above are overcome to a large degree by a nickel-base superalloy having the following broad, intermediate, and preferred ranges in weight percent.

















Broad
Intermediate
Preferred



















C
0.005-0.1 
0.01-0.05
0.02-0.04


Cr
13-17
14-16
14.5-15.5


Fe
 4-20
 8-17
 9-16


Mo
3-9
3.5-8  
3.8-4.5


W
0-8
0-4
0-3


Co
 0-12
0-8
0-5


Al
1-3
1.5-2.5
1.8-2.2


Ti
0.6-3  
  1-2.5
1.5-2.1


Nb + Ta
  0-5.5
1-5
  2-4.5


B
0.001-0.012
0.003-0.010
0.004-0.008


Mg
0.0001-0.0020
0.0003-0.0020
0.0004-0.0016


Zr
0.01-0.08
0.015-0.06 
0.02-0.04


Si
  0-0.7%
  0-0.7%
  0-0.7%


P
  0-0.05%
  0-0.05%
  0-0.05%










The balance of the alloy is essentially nickel, usual impurities, such as phosphorus and sulfur, found in precipitation hardenable nickel-base superalloys intended for similar service, and minor amounts of additional elements, such as manganese, which may be present in amounts that do not adversely affect the basic and novel properties provided by this alloy as described hereinbelow.


In accordance with another aspect of this invention there is provided a process of improving the tensile ductility of a nickel-base superalloy article. The process includes the step of providing an intermediate product form, such as bar or rod, that is made from a precipitation hardenable nickel-base superalloy having a composition including elements that can combine to form a gamma prime (γ′) precipitate in the alloy. In a first step, the intermediate product form is heated at a temperature above the solvus temperature of the γ′ precipitate (the supersolvus temperature) for a time sufficient to take γ′ precipitate into solid solution in the alloy. In a second step the intermediate product form is heated at a temperature that is about 10-150 F.° below the γ′ solvus temperature (the subsolvus temperature) for a time sufficient to cause precipitation and coarsening of γ′. The alloy is then cooled to room temperature from the subsolvus temperature. In a third step the intermediate product form is heated at an aging temperature and for a time sufficient to cause precipitation of fine γ′ precipitates. In a preferred embodiment, the third step may comprise a double-age in which the intermediate product form is heated at a first aging temperature, rapidly cooled from the first aging temperature, heated at a second aging temperature lower than said first aging temperature, and then cooling the alloy at a slower rate to room temperature.


The foregoing tabulation is provided as a convenient summary and is not intended thereby to restrict the lower and upper values of the ranges of the individual elements of the alloy of this invention for use in combination with each other, or to restrict the ranges of the elements for use solely in combination with each other. Thus, one or more of the element ranges of the broad composition can be used with one or more of the other ranges for the remaining elements in the preferred composition. In addition, a minimum or maximum for an element of one preferred embodiment can be used with the maximum or minimum for that element from another preferred embodiment. It is further noted that the weight percent compositions described above define the constituents of the alloy that are essential to obtain the combination of properties that characterize the alloy according to this invention. Thus, it is contemplated that the alloy according to the present invention comprises or consists essentially of the elements described above, throughout the following specification, and in the appended claims. Here and throughout this application, unless otherwise indicated, the term percent or the symbol “%” means percent by weight percent or mass percent.


The basic and novel properties provided by the alloy according to this invention and in useful articles made therefrom include high strength, good creep resistance, and good crack growth resistance. Here and throughout this Specification the term “solvus temperature” means the solvus temperature of the γ′ precipitate. The term “high strength” as used in the present application means a room temperature yield strength of at least about 120 ksi and a yield strength of at least about 115 ksi when tested at a temperature of 1300° F. The term “good creep resistance” means a stress rupture life of at least about 23 hours when the alloy is tested at 1350° F. with an applied stress of 80 ksi. The term “good crack growth resistance” means a sub-critical dwell crack growth rate of not more than about 10−3 in./cycle when tested at a stress intensity factor range (ΔK) of 40 ksi√in, 5×10−5 in./cycle at a ΔK of 20 ksi√in, and crack growth rates between ΔK of 20 ksi√in and ΔK of 40 ksi√in that are not greater than those determined by the equation:






da/dN=1.2×10−10×ΔK4.3.





BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS

The foregoing summary and the following detailed description of the present invention may be further understood when read in conjunction with the appended drawings, in which:



FIG. 1 is a graph of crack growth rate (da/dN) as a function of stress intensity range for a first series of examples that were solution annealed at 1800° F. for 1 hour and then aged;



FIG. 2 is a graph of crack growth rate (da/dN) as a function of stress intensity range for the first series of examples that were solution annealed at 2075° F. for 1 hour and then aged; and



FIG. 3 is a graph of crack growth rate (da/dN) as a function of stress intensity range for a second series of examples that were solution annealed at 1850° F. for 1 hour and then aged.





DETAILED DESCRIPTION OF THE INVENTION

The concentrations of the elements that constitute the alloy of this invention and their respective contributions to the properties provided by the alloy will now be described.


Carbon: Carbon is present in this alloy because it forms grain boundary carbides that benefit the ductility provided by the alloy. Therefore, the alloy contains at least about 0.005% carbon, better yet at least about 0.01% carbon, and preferably at least about 0.02% carbon. For best results the alloy contains about 0.03% carbon. Up to about 0.1% carbon can be present in this alloy. However, too much carbon can produce carbonitride particles that may adversely affect fatigue behavior. Therefore, carbon is preferably limited to not more than about 0.06%, better yet to not more than about 0.05%, and most preferably to not more than about 0.04% in this alloy.


Chromium: Chromium is beneficial to the oxidation resistance and crack growth resistance provided by this alloy. In order to obtain those benefits the alloy contains at least about 13% chromium, better yet at least about 14% chromium, and preferably at least about 14.5% chromium. For best results, the alloy contains about 15% chromium. Too much chromium results in alloy phase instability as by the formation of a topologically close packed phase during high temperature exposure. The presence of such phase adversely affects the ductility provided by the alloy. Therefore, the alloy contains not more than about 17% chromium, better yet not more than about 16% chromium, and preferably not more than about 15.5% chromium.


Molybdenum: Molybdenum contributes to the solid solution strength and good toughness provided by this alloy. Molybdenum benefits the crack growth resistance when the alloy contains very little or no tungsten. For those reasons, the alloy contains at least about 3% molybdenum, better yet at least about 3.5% molybdenum, and preferably at least about 3.8% molybdenum. Too much molybdenum in the presence of chromium can adversely affect the phase balance of this alloy because, like chromium, it can cause the formation of a topologically close packed phase that adversely affects the ductility of the alloy. For that reason, contains not more than about 9%, better yet not more than about 8%, and preferably not more than about 4.5% molybdenum.


Iron: The alloy according to this invention contains at least about 4% iron in substitution for some of the nickel and for some of the cobalt when cobalt is present in the alloy. The presence of iron in substitution for some of the nickel results in a lowering of the solvus temperature for the γ′ and γ″ precipitates such that the solution annealing of the alloy can be performed at a lower temperature than when the alloy contains no iron. It is believed that a lower solvus temperature may be beneficial to the thermomechanical processability of this alloy. Therefore, the alloy preferably contains at least about 8% iron, and better yet at least about 9% iron. When the alloy contains too much iron the crack growth resistance provided by the alloy is adversely affected especially when tungsten is present in the alloy. Accordingly, the alloy contains not more than about 20% iron, better yet not more than about 17% iron, and preferably not more than about 16% iron.


Cobalt: Cobalt is optionally present in this alloy because it benefits the creep resistance provided by the alloy. However, the inventors have discovered that too much cobalt in the alloy has an adverse effect on the crack growth resistance property. Therefore, when cobalt is present in this alloy it is restricted to not more than about 12%, better yet to not more than about 8%, and preferably to not more than about 5%.


Aluminum: Aluminum combines with nickel and iron to foim the γ′ precipitates that benefit the high strength provided by the alloy in the solution annealed and aged condition. Aluminum has also been found to work synergistically with chromium to provide improved oxidation resistance compared to the known alloys. Aluminum is also beneficial for stabilizing the γ′ precipitates so that the γ′ does not transform to the eta phase or to the delta phase when the alloy is overaged. For those reasons the alloy contains at least about 1% aluminum, better yet at least about 1.5% aluminum, and preferably at least about 1.8% aluminum. Too much aluminum can result in segregation that adversely affects the processability of the alloy, for example, the hot workability of the alloy. Therefore, aluminum is limited to not more than about 3%, better yet to not more than about 2.5%, and preferably to not more than about 2.2% in this alloy.


Titanium: Titanium, like aluminum, contributes to the strength provided by the alloy through the formation of the γ′ strengthening precipitate. Accordingly, the alloy contains at least about 0.6% titanium, better yet at least about 1% titanium, and preferably at least about 1.5% titanium. Too much titanium adversely affects the crack growth resistance property of the alloy. Titanium causes rapid age hardening and can adversely affect theimo-mechanical processing and welding of the alloy. Therefore, the alloy contains not more than about 3% titanium, better yet not more than about 2.5% titanium, and preferably not more than about 2.1% titanium.


Niobium: Niobium is another element that combines with nickel, iron, and/or cobalt to for γ′. Although niobium is optionally present in this alloy, the alloy preferably contains at least about 1% niobium and better yet at least about 2% niobium to benefit the very high strength provided by the alloy in the solution annealed and aged condition. When the alloy contains less than about 1% aluminum, the niobium-enriched strengthening phase is more likely to transform to undesired delta phase when the alloy is overaged. That phenomenon is more pronounced when iron is present in this alloy. The presence of delta phase can limit the service temperature of the alloy to about 1200° F. which is insufficient for many gas turbine applications. As described above the alloy contains enough Al to prevent delta phase formation if the alloy is overaged at a temperature higher than 1200° F. When present, niobium is limited to not more than about 5.5%, better yet to not more than about 5%, and preferably to not more than about 4.5% in this alloy. Tantalum may be substituted for some or all of the niobium, when niobium is intentionally present in this alloy.


Tungsten: Tungsten is optionally present in the alloy of this invention to benefit the strength and creep resistance provided by this alloy. High levels of tungsten adversely affect the dwell crack growth resistance provided by the alloy. The alloy is more crack growth tolerant of tungsten when tungsten is present in place of some of the niobium. Accordingly, when present, tungsten is limited to not more than about 8% tungsten, better yet to not more than about 4% tungsten, and preferably to not more than about 3% in this alloy.


Boron, Magnesium, Zirconium, Silicon, and Phosphorus: Up to about 0.015% boron can be present in this alloy to benefit the high temperature ductility of the alloy thereby making the alloy better suited for hot working. Preferably, the alloy contains about 0.001-0.012% boron, better yet about 0.003-0.010% boron, and most preferably about 0.004-0.008% boron. Magnesium is present as a deoxidizing and desulfurizing agent. Magnesium also appears to benefit the crack growth resistance provided by the alloy by tying up sulfur. For those reasons the alloy contains about 0.0001-0.005% magnesium, better yet about 0.0003-0.002% magnesium, and preferably about 0.0004-0.0016% magnesium. It was found that for this alloy a small position addition of zirconium is beneficial for good hot working ductility to prevent cracking during hot forging of ingots made from the alloy. In that regard, the alloy contains at least about 0.001% zirconium. Preferably, the alloy contains about 0.01-0.08% zirconium, better yet about 0.015-0.06% zirconium, and most preferably about 0.02-0.04% zirconium. For best results, the alloy contains about 0.03% zirconium. Silicon is believed to benefit the notch ductility of this alloy at elevated temperatures. Therefore, up to about 0.7% silicon can be present in the alloy for such purpose. Although phosphorus is typically considered to be an impurity element, a small amount of phosphorus, up to about 0.05%, can be included to benefit the stress rupture properties provided by this alloy when niobium is present.


The balance of the alloy composition is nickel and the usual impurities found in commercial grades of nickel-base superalloys intended for similar service or use. Also included in the balance are residual amounts of other elements such as manganese that are not intentionally added, but which are introduced through charge materials used to melt the alloy. Preferably the alloy contains at least about 58% nickel for a good overall combination of properties (strength, creep resistance, and crack growth resistance). It was discovered that the alloy has a lower gamma prime solvus temperature when the alloy contains nickel in the lower portion of the nickel range. Therefore, for a selected amount of aluminum, titanium, and niobium in this alloy, the annealing temperature to obtain a particular grain size and combination of properties is based somewhat on nickel content.


In order to provide the basic and novel properties that are characteristic of the alloy, the elements are preferably balanced by controlling the weight percent concentrations of the elements molybdenum, niobium, tungsten, and cobalt. More particularly, when the alloy contains less than 0.1% niobium, the combined amounts of molybdenum and tungsten are greater than about 7%, and the alloy is to be annealed at a temperature greater than the γ′ solvus temperature, then cobalt is restricted to less than 9%. When the alloy contains at least 0.1% niobium, then the alloy is preferably balanced such that the γ′ solvus temperature is not greater than about 1860° F. and the alloy is preferably processed to provide a grain size that is as coarse as practicable.


The alloy of this invention is preferably produced by vacuum induction melting (VIM). When desired, the alloy may be refined by a double melting process in which the VIM ingot is remelted by electroslag remelting (ESR) or by vacuum arc remelting (VAR). For the most critical applications, a triple-melt process consisting of VIM followed by ESR and then VAR can be used. After melting, the alloy is cast as one or more ingots that are cooled to room temperature to fully solidify the alloy. Alternatively, the alloy can be atomized to form metal powder after the primary melting (VIM). The alloy powder is consolidated to form intermediate product forms such as billets and bars that can be used to manufacture finished products. The alloy powder is preferably consolidated by loading the alloy powder into a metal canister and then hot isostatically pressing (HIP) the metal powder under conditions of temperature, pressure, and time sufficient to fully or substantially fully consolidate the alloy powder into a canister ingot.


The solidified ingot, whether cast or HIP'd, is preferably homogenized by heating at about 2150° F. for about 24 hours depending on the cross-sectional area of the ingot. The alloy ingot can be hot worked to an intermediate product form by forging or pressing. Hot working is preferably carried out by heating the ingot to an elevated starting temperature of about 1900-2100° F., preferably about 2050-2075° F. If additional, reduction in cross-sectional area is needed, the alloy must be reheated to the starting temperature before additional hot working is performed.


The tensile and creep strength properties that are characteristic of the alloy according to this invention are developed by heat treating the alloy. In this regard, the as-worked alloy is preferably solution annealed at the supersolvus temperature as defined above. Therefore, in general, the alloy is preferably heated at a supersolvus temperature of about 1850-2100° F. for a time sufficient to dissolve substantially all intermetallic precipitates in the matrix alloy material. Alternatively, when the alloy contains more than 0.1% niobium, the alloy can be annealed at a temperature below the γ′ solvus temperature. When the γ′ solvus temperature of the alloy is greater than about 1880° F., then tungsten is preferably restricted to not more than about 1% when the alloy is to be annealed at the subsolvus temperature. The time at temperature depends on the size of the alloy product faun and is preferably about 1 hour per inch of thickness. The alloy is cooled to room temperature at a rate that is sufficiently fast to retain the dissolved precipitates in solution.


After the solution annealing heat treatment, the alloy is subjected to an aging treatment that causes the precipitation of the strengthening phases in the alloy. Preferably, the aging treatment includes a two-step process. In a first or stabilizing step the alloy is heated at a temperature of about 1500-1550° F. for about 4 hours and then cooled to room temperature by water quenching or air cooling depending on the section size of the alloy part. In a second or precipitation step the alloy is heated at a temperature of about 1350-1400° F. for about 16 hours and then cooled in air to room temperature. Although the two-step aging treatment is preferred, the aging treatment can be conducted in a single step in which the alloy is heated at a temperature of about 1400° F. for about 16 hours and then cooled in air to room temperature.


In the solution-treated and aged condition, the alloy provides a room temperature yield strength of at least about 120 ksi and an elevated temperature yield strength (1300° F.) of at least about 115 ksi. The foregoing tensile yield strengths are provided in combination with good creep resistance as defined by a stress rupture strength of at least about 23 hours when tested at 1350° F. and an applied stress of 80 ksi.


The alloy according to this invention when heat treated as described above has a relatively coarse-grained microstructure that benefits the stress rupture property (creep strength). In connection with the invention described herein, the term “coarse-grained” means an ASTM grain size number of 4 or coarser as determined in accordance with ASTM Standard Test Method E-112. However, the inventors discovered that the coarse-grained microstructure may result in an undesirable reduction in the tensile ductility provided by the alloy in the single-solution-treated and aged condition. Therefore, in connection with the development of the alloy, the inventors developed a modified heat treatment to overcome the loss in tensile ductility that otherwise results when the alloy is heat treated as described above.


The modified heat treatment according to the present invention includes a two-step annealing procedure. In the first step, the alloy is solution annealed by heating at a supersolvus temperature of about 1850-2100° F. as described above. The time at temperature is preferably about 0.5-4 hours depending on the size and cross-sectional area of the alloy product. The alloy is cooled from the supersolvus temperature to room temperature as described above. In the second step, the alloy is heated at a subsolvus temperature that is about 10 F.° to about 150 F.° below the γ′ solvus temperature of the alloy. The alloy is preferably held at the subsolvus temperature for about 1-8 hours, again depending on the size and cross-sectional area of the alloy product. The alloy is then cooled to room temperature before the aging heat treatment is performed as described above. The inventors believe that the subsolvus annealing step causes the precipitation of γ′ that coarsens into sizes that are large relative to the finer-sized γ′ that is precipitated during the aging treatment. The combination of the coarsened and fine-sized γ′ is believed to benefit the tensile ductility provided by the alloy because the coarser γ′ precipitates are more stable during the elevated temperatures experienced by the alloy when used in elevated temperature service. The coarsened γ′ also consumes a portion of the aluminum, titanium, and niobium in the alloy, thereby limiting the total amount of the finer-sized γ′ that precipitates during the aging treatment and when the alloy is in elevated temperature service. The resulting restriction on the overall amount of the γ′ precipitate in the alloy limits the peak strength and stress rupture life provided by the alloy to an acceptable degree, but also reduces precipitation and coarsening of undesirable brittle phases that otherwise would adversely affect the tensile ductility provided by the alloy.


WORKING EXAMPLES

The following examples are presented in order to demonstrate the combination of properties that characterize the alloy according to this invention.


Example I

In order to demonstrate the novel combination of properties provided by the alloy according to this invention, several small heats were vacuum induction melted and cast as 40 lb., 4-in. square ingots. The weight percent compositions of the ingots are set forth in Table 1 below. The balance of each heat was nickel and a residual amount of zirconium resulting from an addition of 0.03% Zr during melting.


All of the ingots were homogenized at 2150° F. for 24 hours. The “S” heats were forged from a starting temperature of 2150° F. to 1.75-in. square bar, cut in half, reheated to 2150° F., and then forged to 0.8 in.×1.4 in. rectangular cross section bars. The “G” heats were forged from a starting temperature of 2050-2075° F. to 1.75-in. square bar, cut in half, reheated to 2150° F., and then forged to 0.8 in.×1.4 in. rectangular cross section bars.























TABLE 1







Heat
C
Cr
Ni
Mo
W
Co
Al
Ti
Nb
B
Fe
Mg





























Inv.1
S31
0.025
14.97
58.06
8.01
0.01
0.01
1.00
3.00
<0.01
0.0053
14.90
0.0015



S32
0.021
15.02
57.97
8.01
<0.01
<0.01
2.96
0.60
<0.01
0.0050
15.38
0.0016



S66
0.038
15.00
57.86
4.02
3.98
<0.01
1.99
1.80
<0.01
0.0053
15.34
<0.001



G16
0.032
14.95
62.87
4.01
2.94
0.10
1.98
1.79
1.03
0.0047
10.25
0.0004



G17
0.032
15.06
62.85
3.98
1.98
0.01
1.98
1.73
1.98
0.0051
10.35
0.0007



G18
0.032
14.96
62.93
4.00
1.00
<0.01
2.00
1.73
2.97
0.0046
10.33
0.0011



G19
0.033
14.97
62.98
4.00
0.01
<0.01
1.97
1.72
3.97
0.0049
10.30
0.0014



G20
0.030
14.90
58.08
3.86
3.09
9.95
1.95
1.84
1.02
0.0053
5.25
0.0005



G24
0.034
15.03
57.89
4.01
2.93
0.13
1.97
1.79
1.04
0.0049
15.13
0.0004



G25
0.034
15.02
57.83
3.99
1.99
0.01
1.97
1.79
2.01
0.0058
15.31
0.0006



G26
0.030
14.99
57.91
4.00
1.00
<0.01
1.96
1.78
2.99
0.0053
15.28
0.0009



G27
0.032
15.06
58.07
4.00
0.02
<0.01
2.01
1.76
3.68
0.0051
15.33
0.0015


Comp.2
S25
0.022
9.99
62.81
7.99
<0.01
<0.01
0.95
2.96
<0.01
0.0046
15.23
0.0012



S26
0.024
10.03
62.85
8.00
0.01
<0.01
2.94
0.61
<0.01
0.0046
15.51
0.0015



S27
0.028
9.96
63.12
7.99
<0.01
9.95
1.00
2.97
<0.01
0.0047
4.97
0.0015



S28
0.024
10.02
62.87
4.02
3.96
<0.01
1.97
1.80
<0.01
0.0048
15.31
0.0006



S29
0.025
10.03
62.77
0.00
7.98
<0.01
1.00
3.07
<0.01
0.0045
15.12
0.0011



S30
0.026
10.00
63.00
4.01
3.98
10.04
1.97
1.80
<0.01
0.0049
5.17
0.0014



S33
0.025
14.90
58.25
8.00
<0.01
9.98
0.98
2.98
<0.01
0.0049
4.87
0.0014



S34
0.023
14.94
58.18
7.98
<0.01
9.97
2.97
0.60
<0.01
0.0055
5.34
0.0014



S37
0.024
10.06
62.78
<0.01
7.97
0.01
2.98
0.60
<0.01
0.0052
15.57
0.0013



S38
0.026
10.01
63.04
<0.01
7.96
10.06
1.02
3.06
<0.01
0.0045
4.82
0.0014



S39
0.026
10.02
63.10
<0.01
7.98
10.07
2.98
0.59
<0.01
0.0045
5.23
0.0015



S40
0.025
9.99
63.15
8.01
0.01
10.02
2.96
0.60
<0.01
0.0046
5.26
0.0015



S67
0.035
14.95
58.12
4.03
3.99
9.93
1.97
1.80
<0.01
0.0045
5.22
<0.001



S68
0.030
14.89
58.07
0.03
7.98
10.01
1.00
3.04
<0.01
0.0038
4.99
0.0010



S69
0.029
15.05
57.82
<0.01
8.00
0.06
2.98
0.63
<0.01
0.0042
15.46
0.0010



S70
0.030
15.02
58.52
<0.01
8.00
10.01
2.98
0.07
<0.01
0.0042
5.40
0.0010



S44
0.030
14.96
58.06
<0.01
8.01
10.03
0.98
3.04
<0.01
0.0051
4.88
0.0013



G12
0.034
14.90
63.00
3.95
3.03
10.01
1.94
1.78
0.99
0.0048
0.32
0.0004



G13
0.032
14.92
63.07
4.00
1.99
9.99
1.96
1.78
1.99
0.0047
0.22
0.0007



G14
0.033
14.92
63.07
4.00
1.00
10.00
1.97
1.78
2.98
0.0047
0.22
0.0009



G15
0.033
14.89
63.11
3.99
0.02
9.99
1.97
1.78
3.97
0.0042
0.22
0.0012



G21
0.032
14.89
58.06
4.00
1.99
9.99
1.96
1.79
2.01
0.0052
5.24
0.0007



G22
0.033
14.93
58.04
3.98
1.00
10.00
1.97
1.78
3.00
0.0046
5.23
0.0010



G23
0.034
14.71
58.72
3.93
0.01
9.80
1.92
1.75
3.94
0.0051
5.15
0.0013






1Invention




2Comparative







Standard tensile test specimens and standard test specimens in accordance with ASTM Standard Specification E399 for dwell crack growth testing were prepared from the as-forged bars. The specimens were heat treated as set forth in Table 2 below.











TABLE 2





Alloy
Solution Treatment
Aging Treatment







“G” (H1)
1800 F./1 h/OQ
1550 F./4 h/AC + 1350 F./16 h/AC


“G” (H2)
2075 F./1 h/OQ
1550 F./4 h/AC + 1350 F./16 h/AC


“S”
1850 F./1 h/OQ
1550 F./4 h/AC + 1350 F./16 h/AC









The results of room temperature tensile testing are set forth in Table 3A below including the 0.2% offset yield strength (YS), the ultimate tensile strength (UTS), the percent elongation (% El), and the percent reduction in cross-sectional area (% RA). The results set forth in Table 3A include tests performed after heat treatment and tests perfoiined after the samples were heated at 1300° F. for 1000 hrs.











TABLE 3A









1300 F./1000 hrs

















HEAT
YS
UTS
% El
% RA
YS
UTS
% El
% RA




















Inv.
S31
143.03
204.67
16.63
15.50
148.97
204.63
8.00
 9.19


(H1)
S32
121.34
179.18
23.50
33.79
131.26
188.88
16.30
28.15














S66
136.61
193.54
26.14
34.85
Not Tested

















G16
170.64
208.65
18.22
44.67
171.06
210.64
19.40
48.41



G17
178.60
216.21
10.59
42.88
174.07
211.34
16.70
42.70



G18
184.64
221.64
16.24
46.47
186.31
222.39
16.87
34.03



G19
124.51
213.85
18.71
26.18
111.99
210.20
9.60
10.52



G20
161.70
205.55
24.36
41.86
156.86
200.99
19.10
37.24



G24
161.73
203.76
21.19
44.63
146.93
190.25
7.80
32.75



G25
162.90
203.60
8.71
36.13
162.43
209.91
11.60
34.05



G26
168.66
212.62
9.11
31.55
164.94
216.82
14.16
34.85



G27
173.25
219.87
11.29
17.16
155.88
210.03
12.30
16.17


Comp.
S25
115.46
188.02
29.11
46.36
119.73
189.12
22.30
30.50



S26
111.45
172.65
27.33
49.42
117.64
174.93
25.00
46.35



S27
119.16
190.87
30.50
47.14
129.01
194.18
28.80
47.30



S28
125.30
187.66
26.10
53.10
126.43
186.66
23.90
41.92



S29
124.82
194.69
23.76
46.39
131.03
195.64
23.10
48.65



S30
132.32
193.56
25.40
50.79
134.06
192.72
26.50
46.72



S33
126.61
200.41
27.62
34.10
133.19
195.12
12.60
15.90



S34
130.90
187.56
17.80
45.68
133.44
190.52
26.30
49.59



S37
131.66
190.03
23.96
43.62
137.39
190.55
22.48
46.39



S38
132.72
198.25
26.14
53.02
139.14
199.38
24.75
49.51



S39
128.98
198.41
24.60
45.76
133.99
191.38
23.50
41.44



S40
125.91
186.81
25.60
34.49
128.45
187.29
27.60
50.87














S67
132.07
192.34
29.11
48.21
Not Tested



S68
134.10
198.92
27.13
44.80
Not Tested



S69
138.88
183.89
21.88
48.37
Not Tested



S70
131.08
186.15
25.74
54.31
Not Tested

















S44
143.55
208.28
20.10
39.93
144.14
205.03
22.08
37.59



G12
175.48
212.95
21.98
52.21
180.00
220.92
22.57
42.97














G13
160.91
212.84
25.45
47.72
Not Tested

















G14
173.66
218.37
11.49
34.31
162.92
216.70
19.80
32.75














G15
147.40
208.31
17.82
20.03
Not Tested

















G21
166.80
210.04
19.60
41.58
175.26
220.48
21.40
48.00



G22
177.52
222.62
13.10
45.17
168.89
217.99
16.60
37.14



G23
163.62
215.16
17.10
23.30
155.25
220.27
16.40
22.54










The results of additional room temperature tensile testing of the G-heat samples that were heat treated with H2 are set forth in Table 3B below including the 0.2% offset yield strength (YS), the ultimate tensile strength (UTS), the percent elongation (% El), and the percent reduction in cross-sectional area (% RA).











TABLE 3B









1300 F./1000 hrs

















HEAT
YS
UTS
% El
% RA
YS
UTS
% El
% RA




















Inv.
G16
170.64
208.65
18.22
44.67
118.13
167.97
 9.80
12.18


(H2)
G17
178.60
216.21
10.59
42.88
123.51
174.80
10.00
12.13



G18
184.64
221.64
16.24
46.47
135.58
192.50
13.80
12.41



G19
124.51
213.85
18.71
26.18
141.19
203.83
16.00
17.09



G20
161.70
205.55
24.36
41.86
121.87
175.10
14.40
13.48



G24
161.73
203.76
21.19
44.63
116.37
175.91
12.38
11.95



G25
162.90
203.60
8.71
36.13
127.14
188.91
15.50
14.70



G26
168.66
212.62
9.11
31.55
138.25
194.38
13.60
13.36



G27
173.25
219.87
11.29
17.16
142.74
203.15
14.60
14.57


Comp.
G12
175.48
212.95
21.98
52.21
119.81
180.83
24.16
20.15














G13
160.91
212.84
25.45
47.72
Not Tested

















G14
173.66
218.37
11.49
34.31
139.79
186.23
11.49
12.09














G15
147.40
208.31
17.82
20.03
Not Tested

















G21
166.80
210.04
19.60
41.58
131.12
183.44
12.70
14.36



G22
177.52
222.62
13.10
45.17
139.34
189.79
13.00
13.97



G23
163.62
215.16
17.10
23.30
143.33
201.98
16.20
16.03










The results of elevated temperature tensile testing are set forth in Table 4A below including the 0.2% offset yield strength (YS), the ultimate tensile strength (UTS), the percent elongation (% El), and the percent reduction in cross-sectional area (% RA). In these tests a first set of tensile specimens was tested at a temperature of 1000° F. and a second set of tensile specimens was tested at a temperature of 1300° F.












TABLE 4A









1000 F.
1300 F.

















HEAT
YS
UTS
% El
% RA
YS
UTS
% El
% RA




















Inv.
S31
130.44
190.96
10.27
11.85
106.72
137.86
26.93
50.47


(H1)
S32
114.70
166.24
15.28
32.44
100.58
127.70
22.28
35.72



S66
129.16
181.89
20.69
35.00
115.54
139.83
17.33
22.27



G16
155.32
195.65
12.71
30.28
97.82
137.01
34.76
79.44














G17
155.57
204.57
13.49
35.71
Not Tested

















G18
169.59
209.96
12.29
31.29
100.20
141.05
32.83
85.12



G19
130.20
198.47
16.02
26.11
77.05
129.80
41.39
86.01



G20
134.85
174.71
16.45
28.39
117.35
153.44
19.82
20.18



G24
143.02
191.03
12.11
29.99
106.71
141.07
32.11
40.31



G25
154.2 
201.46
10.72
25.95
105.44
146.90
32.11
73.71



G26
142.58
192.21
7.05
15.05
105.56
143.52
36.51
98.52



G27
138.93
195.32
7.53
14.22
96.97
148.34
27.47
73.20


Comp.
S25
107.99
173.16
18.78
32.89
95.46
132.92
6.34
12.16



S26
106.90
160.41
19.20
44.27
95.40
125.53
6.76
14.24



S27
113.90
172.94
20.42
41.11
101.06
130.44
3.50
4.63



S28
115.33
174.99
18.90
43.09
104.69
132.51
5.25
10.97



S29
120.48
179.02
14.25
37.52
110.84
136.20
3.26
5.65



S30
120.92
176.39
19.63
40.92
115.34
133.06
2.90
6.42



S33
117.68
179.88
17.63
32.10
113.22
144.58
4.16
11.60



S34
120.71
174.98
19.93
35.36
112.75
136.36
6.80
10.99



S37
125.76
177.28
14.55
38.40
107.53
133.19
4.16
8.68



S38
122.39
177.13
17.33
48.37
111.34
133.53
3.30
9.84



S39
121.79
174.00
19.38
39.83
113.24
139.63
5.50
7.04



S40
114.65
170.23
20.53
42.94
110.02
129.18
3.80
6.92














S67
120.48
172.09
26.04
38.79
Not Tested

















S68
124.10
180.78
27.82
44.26
120.42
149.63
8.02
16.37



S69
129.52
176.71
19.31
43.06
115.08
137.95
11.98
11.48



S70
121.89
169.43
20.79
47.72
107.08
133.27
8.32
16.43



S44
129.84
188.18
18.54
36.89
118.25
149.96
4.10
3.94



G12
156.85
204.55
13.43
22.68
124.20
157.88
39.70
77.27











G13
Not Tested
Not Tested

















G14
145.13
206.96
14.10
25.59
128.36
166.26
15.00
38.07














G15
Not Tested
121.81
165.78
4.34
6.72

















G21
156.85
204.02
11.14
26.65
118.88
156.18
32.65
65.37



G22
155.61
206.17
8.8
15.58
120.20
161.13
27.17
71.19



G23
140.94
212.23
12.77
18.77
121.13
161.90
15.36
20.55










The results of additional elevated temperature tensile testing of the G-heat samples that were heat treated with H2 are set forth in Table 4B below including the 0.2% offset yield strength (YS), the ultimate tensile strength (UTS), the percent elongation (% El), and the percent reduction in cross-sectional area (% RA).












TABLE 4B









1000 F.
1300 F.

















HEAT
YS
UTS
% El
% RA
YS
UTS
% El
% RA




















Inv.
G16
105.87
160.99
19.58
24.29
101.25
146.95
21.69
24.30


(H2)
G17
113.48
165.72
16.81
21.23
106.85
151.73
20.66
24.11



G18
118.07
171.82
14.1
22.15
116.10
159.27
19.70
25.55



G19
122.65
177.89
11.33
19.90
120.21
163.04
10.12
11.67



G20
103.84
154.42
26.39
35.34
108.61
155.82
15.60
19.84














G24
Not Tested
108.17
146.82
17.11
20.67

















G25
113.42
166.93
13.13
18.90
114.31
151.82
24.04
28.66



G26
121.27
174.17
11.39
15.12
117.58
157.23
18.19
18.40



G27
126.18
176.51
8.19
14.36
130.71
162.25
10.48
12.02


Comp.
G12
101.71
151.2
27.59
37.15
97.68
143.01
15.18
18.53











G13
Not Tested
Not Tested

















G14
118.69
164.83
22.29
30.09
112.42
139.57
3.80
10.45











G15
Not Tested
Not Tested

















G21
156.85
204.02
11.14
26.65
118.88
156.18
32.65
65.37



G22
119.56
168.35
18.98
26.83
114.75
152.72
4.94
13.36



G23
122.83
174.97
18.07
27.52
99.42
143.18
13.61
23.51










The results of stress rupture testing performed at 1350° F. and an applied stress of 80 ksi are presented in Table 5A below including the time to rupture (Life) in hours, the percent elongation (% El) and the percent reduction in cross-sectional area (% RA).














TABLE 5A







HEAT
Life
% El
% RA






















Inv.
S31
2.65
23.10
62.20



(H1)
S32
1.52
28.30
43.70




S66
3.68
21.60
39.90




G16
1.16
22.50
69.40




G17
1.18
39.40
77.20




G18
0.99
26.60
75.00




G19
0.88
49.20
79.20




G20
14.70
28.10
51.90




G24
3.15
28.30
40.00




G25
5.95
36.40
60.70




G26
3.71
27.30
70.90




G27
10.70
26.00
43.00



Comp.
S25
0.40
6.60
9.80




S26
2.06
14.60
26.10




S27
3.52
4.30
6.60




S28
1.03
3.70
7.90




S29
0.92
1.40
2.30




S33
8.41
6.10
8.30




S34
3.32
13.90
18.90




S30
3.24
4.30
4.70




S37
2.72
8.00
10.20




S38
2.98
2.90
4.40




S39
4.68
4.30
8.70




S40
4.60
10.60
17.40




S67
18.60
18.20
22.00




S68
1.33
4.40
7.20




S69
4.70
15.30
28.20




S70
3.38
14.60
24.00




S44
10.50
4.00
7.70




G12
4.31
11.00
18.50




G13
12.00
13.00
14.50




G14
27.20
21.60
71.00




G15
1.14
30.40
70.00




G21
12.30
24.60
68.20




G22
14.70
33.40
67.40




G23
13.20
22.30
68.30










The results of additional stress rupture testing of the G-heat samples that were heat treated with H2 are presented in Table 5B including the time to rupture (Life) in hours, the percent elongation (% El) and the percent reduction in cross-sectional area (% RA).














TABLE 5B







HEAT
Life
% El
% RA






















Inv.
G16
37.50
16.30
17.60



(H2)
G17
51.00
18.00
25.90




G18
62.80
26.10
37.40




G19
73.00
26.40
30.00




G20
35.60
24.20
11.00




G24
30.80
7.50
8.90




G25
46.70
25.60
39.80




G26
54.20
25.30
42.90




G27
57.60
27.60
38.40



Comp.
G12
31.60
2.10
4.90




G13
51.90
1.10
3.20




G14
117.00
4.30
8.70




G15
96.30
0.36
2.80




G21
104.00
13.00
19.50




G22
121.00
5.60
7.50




G23
127.00
8.00
8.70










In addition to the tensile and stress rupture testing, selected samples of the G and S heats were tested for dwell crack growth resistance. The results of the crack growth resistance testing are shown in FIGS. 1-3. FIG. 1 includes a graph of the line that is defined by the equation da/dN=1.2×10−10×ΔK4.3 compared to the graphs for the examples that were tested.


Example II

Additional testing was performed to demonstrate the benefits of the modified heat treatment according to the present invention. The testing was performed on samples of alloy G27, the composition of which is set forth in Table 1 above. The onset of the γ′ solvus was 1845° F. as determined by differential scanning calorimetry with a heating rate of 36° F./min. The samples were heat treated using several different heat treatments including single and double annealing treatments as shown in Table 6 below. Heat treatments HT-1 to HT-6 included a single annealing treatment at a temperature above the solvus temperature. Heat treatments HT-7 to HT-9 included a single annealing treatment at a temperature below the solvus temperature. Heat treatments HT-10 to HT-17 included a double annealing treatment consisting of a supersolvus anneal followed by a subsolvus anneal. All heat treatments included a standard aging treatment as described above.


Table 6 below shows the results of elevated temperature tensile testing at 1300° F. including the yield strength (Y.S.) and tensile strength (U.T.S.) in ksi, the percent elongation (% El.), and the percent reduction in area (% R.A.) on the several heat treated samples. Also shown in Table 6 are the results of stress rupture testing including the stress rupture life in hours at 1350° F. under 80 ksi load (TTF). The values reported in Table 6 are the average of measurements taken on duplicate samples, except HT-1. A single sample was tested for HT-1.
















TABLE 6





HT I.D.
Heat Treatment
Anneal
Y.S.
T.S.
% El.
% R.A.
TTF






















1
2075 F./1 h/OQ + WQ Age
Supersolvus
130.7
162.3
10.5
12.0
57.6


2
2075 F./1 h/OQ + FC Age
Supersolvus
128.3
154.3
9.0
8.5



3
1850 F./1 h/OQ + FC Age
Supersolvus
138.5
158.3
6.2
8.5
17.5


4
1850 F./1 h/OQ + 1400 F./16 h/AC
Supersolvus
141.3
167.6
6.2
12.4
29.3


5
1850 F./1 h/OQ + WQ Age
Supersolvus
136.3
159.5
5.9
7.5



6
1850 F./1 h/SC + FC Age
Supersolvus
129.3
153.5
7.8
10.0



7
1825 F./1 h/OQ + FC Age
Subsolvus
117.5
149.8
51.3
74.0



8
1800 F./1 h/OQ + FC Age
Subsolvus
110.3
146.4
40.4
75.3
 5.21


9
1750 F./1 h/OQ + FC Age
Subsolvus
101.0
142.8
39.8
70.3
 4.91


10
2075 F./1 h/OQ + 1800 F./4 h/OQ + WQ Age
Double
123.0
153.0
14.8
18.0
30.0


11
2000 F./1 h/OQ + 1800 F./4 h/OQ + WQ Age
Double
122.8
153.8
19.0
15.8
26.8


12
2075 F./1 h/OQ + 1800 F./8 h/OQ + WQ Age
Double
124.3
153.8
12.5
13.5



13
2075 F./1 h/OQ + 1700 F./8 h/OQ + WQ Age
Double
103.0
144.0
18.3
19.3



14
2000 F./1 h/OQ + 1800 F./8 h/OQ + WQ Age
Double
124.0
153.0
10.8
12.5



15
2075 F./1 h/FC + 1800 F./4 h/OQ + WQ Age
Double
128.8
155.0
5.0
9.0



16
2075 F./1 h/OQ + 1800 F./4 h/FC + WQ Age
Double
98.8
142.3
19.0
24.8



17
1850 F./1 h/FC + 1800 F./4 h/OQ + FC Age
Double
132.0
154.3
14.3
12.3










None of the heat treatments that used a supersolvus annealing temperature met the tensile ductility objective for this alloy. HT-1 through HT-5 show variations in the annealing temperature and aging procedure, yet ductility at acceptable levels was not achieved. A slow cool (SC) from the supersolvus annealing temperature to room temperature (HT-6) was also not effective to provide the desired ductility. Subsolvus annealing heat treatments used in HT-7, HT-8, and HT-9 resulted in improved ductility, but the yield strength decreased to less than 120 ksi and the stress rupture life was not acceptable.


A comparison of the results for HT-1 to the results for HT-10 shows that the addition of a second annealing step below the solvus temperature resulted in significantly increased ductility. The percent elongation increased from 10.5% to 14.8% and the percent reduction in area increased from 12% to 18%. The ductility provided after HT-10 exceeds the minimum acceptable ductility provided by a known superalloy. Although the tensile strength and stress rupture life after HT-10 are lower than after HT-1, the stress rupture life provided still exceeds the stress rupture life provided by another known superalloy.


The results for HT-11 show that the double anneal can be used with a lower temperature supersolvus temperature. The results for HT-12 and HT-14 demonstrate that extended times at the second annealing temperature may result in a lessening of the beneficial effect when close to the solvus temperature. The results for HT-13 show that conducting the second anneal at a temperature farther below the solvus temperature for the second anneal with extended time at temperature results in a further increase in ductility, but with a concomitant reduction in strength. The use of a 100° F./h furnace cool after the first annealing temperature eliminated any gains in ductility as shown by the results for HT-15. However, when the same furnace cool was used only after the second annealing temperature as in HT-16, a relatively high ductility was obtained, albeit with substantially lower strength. The results after HT-17 demonstrate that % elongation can be significantly increased when a second anneal of 1800° F. is used in combination with an first 1850° F. anneal, as compared to a single 1850° F. anneal (HT-3).


The terms and expressions which are employed in this specification are used as terms of description and not of limitation. There is no intention in the use of such terms and expressions of excluding any equivalents of the features shown and described or portions thereof. It is recognized that various modifications are possible within the invention described and claimed herein.

Claims
  • 1. A nickel-base superalloy that provides a combination of high strength, good creep resistance, and good resistance to crack growth, said alloy consisting essentially of, in weight percent: C about 0.005 to about 0.1Cr about 13 to about 17Fe about 4 to about 20Mo about 3 to about 9W up to about 8Co up to about 12Al about 1 to about 3Ti about 0.6 to about 3Nb up to about 5.5B about 0.001 to about 0.015Mg about 0.0001 to about 0.0050Zr about 0.001 to about 0.08Si up to about 0.7P up to about 0.05
  • 2. The alloy as claimed in claim 1 which contains at least about 0.01% carbon.
  • 3. The alloy as claimed in claim 1 which contains at least about 14% chromium.
  • 4. The alloy as claimed in claim 1 which contains at least about 3.5% molybdenum.
  • 5. The alloy as claimed in claim 1 which contains not more than about 17% iron.
  • 6. The alloy as claimed in claim 1 which contains up to about 8% cobalt.
  • 7. The alloy as claimed in claim 1 which contains at least about 1% niobium.
  • 8. The alloy as claimed in claim 1 which contains at least about 1% titanium.
  • 9. A nickel-base superalloy that provides a combination of high strength, good creep resistance, and good resistance to crack growth, said alloy consisting essentially of, in weight percent: C about 0.01 to about 0.05Cr about 14 to about 16Fe about 8 to about 17Mo about 3.5 to about 8W up to about 4Co up to about 8Al about 1.5 to about 2.5Ti about 1 to about 2.5Nb about 1 to about 5B about 0.003 to about 0.010Mg about 0.0001 to about 0.0020Zr about 0.015 to about 0.06Si up to about 0.7P up to about 0.05
  • 10. The alloy as claimed in claim 9 which contains at least about 0.02% carbon.
  • 11. The alloy as claimed in claim 9 which contains at least about 14.5% chromium.
  • 12. The alloy as claimed in claim 9 which contains at least about 3.8% molybdenum.
  • 13. The alloy as claimed in claim 9 which contains not more than about 16% iron.
  • 14. The alloy as claimed in claim 9 which contains up to about 5% cobalt.
  • 15. The alloy as claimed in claim 9 which contains at least about 2% niobium.
  • 16. The alloy as claimed in claim 9 which contains at least about 1.5% titanium.
  • 17. A nickel-base superalloy that provides a combination of high strength, good creep resistance, and good resistance to crack growth, said alloy consisting essentially of, in weight percent: C about 0.02 to about 0.04Cr about 14.5 to about 15.5Fe about 9 to about 16Mo about 3.8 to about 4.5W up to about 3Co up to about 5Al about 1.8 to about 2.2Ti about 1.5 to about 2.1Nb about 2 to about 4.5B about 0.004 to about 0.008Mg about 0.0001 to about 0.0016Zr about 0.02 to about 0.04Si up to about 0.7P up to about 0.05
  • 18. An article of manufacture having a combination of high strength, good creep resistance, and good resistance to crack growth, said article being made from a nickel-base superalloy that consists essentially of, in weight percent: C about 0.005 to about 0.06Cr about 13 to about 17Fe about 4 to about 20Mo about 3 to about 9W up to about 8Co up to about 12Al about 1 to about 3Ti about 0.6 to about 3Nb up to about 5.5B about 0.001 to about 0.012Mg about 0.0001 to about 0.0020Zr about 0.01 to about 0.08Si up to about 0.7P up to about 0.05
  • 19. An article of manufacture having a combination of high strength, good creep resistance, and good resistance to crack growth, said article being made from a nickel-base superalloy that consists essentially of, in weight percent: C about 0.01 to about 0.05Cr about 14 to about 16Fe about 8 to about 17Mo about 3.5 to about 8W up to about 4Co up to about 8Al about 1.5 to about 2.5Ti about 1 to about 2.5Nb about 1 to about 5B about 0.003 to about 0.010Mg about 0.0001 to about 0.0020Zr about 0.015 to about 0.06Si up to about 0.7P up to about 0.05
  • 20. An article of manufacture having a combination of high strength, good creep resistance, and good resistance to crack growth, said article being made from a nickel-base superalloy that consists essentially of, in weight percent: C about 0.01 to about 0.05Cr about 14 to about 16Fe about 8 to about 17Mo about 3.5 to about 8W up to about 4Co up to about 8Al about 1.5 to about 2.5Ti about 1 to about 2.5Nb about 1 to about 5B about 0.003 to about 0.010Mg about 0.0001 to about 0.0020Zr about 0.015 to about 0.06Si up to about 0.7P up to about 0.05
  • 21. A process for improving the tensile ductility of a precipitation hardenable nickel-base superalloy comprising the steps of: providing an intermediate product form made from a precipitation hardenable, nickel-base alloy;determining the solvus temperature of γ′ phase in the precipitation hardenable, nickel-base alloy;heating the intermediate product form at a supersolvus temperature for a time sufficient to solution the γ′ phase in the alloy; thenheating the intermediate product form at a subsolvus temperature for a time sufficient to cause precipitation and coarsening of γ′ precipitate in the alloy; and thenaging the intermediate product form at temperature and time conditions selected to precipitate γ′ phase in the alloy without further coarsening of the γ′ phase.
  • 22. The process according to claim 21 wherein the aging step comprises the steps of: heating the intermediate product form at a first aging temperature;cooling the intermediate product form to a temperature below the first aging temperature;heating the intermediate product faun at a second aging temperature lower than the first aging temperature; and thencooling the intermediate product form to room temperature.
  • 23. The process as claimed in claim 21 wherein the subsolvus temperature is 10 to 150 F.° below the solvus temperature.
  • 24. The process as claimed in claim 21 wherein the supersolvus temperature is about 1850-2100° F.
  • 25. The process as claimed in claim 21 comprising the step of cooling the intermediate product form at a rate of 100 F.° per hour after the intermediate product form is heated at the subsolvus temperature.