Abstract
Disclosed is an ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound.
Description


BACKGROUND OF THE INVENTION

[0001] The present invention is directed to aqueous ink compositions. More specifically, the present invention is directed to ink compositions exhibiting improved lightfastness. One embodiment of the present invention is directed to an ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound.


[0002] Ink jet printing systems generally are of two types: continuous stream and drop-on-demand. In continuous stream ink jet systems, ink is emitted in a continuous stream under pressure through at least one orifice or nozzle. The stream is perturbed, causing it to break up into droplets at a fixed distance from the orifice. At the break-up point, the droplets are charged in accordance with digital data signals and passed through an electrostatic field which adjusts the trajectory of each droplet in order to direct it to a gutter for recirculation or a specific location on a recording medium. In drop-on-demand systems, a droplet is expelled from an orifice directly to a position on a recording medium in accordance with digital data signals. A droplet is not formed or expelled unless it is to be placed on the recording medium.


[0003] Since drop-on-demand systems require no ink recovery, charging, or deflection, the system is much simpler than the continuous stream type. There are two types of drop-on-demand ink jet systems. One type of drop-on-demand system has as its major components an ink filled channel or passageway having a nozzle on one end and a piezoelectric transducer near the other end to produce pressure pulses. The relatively large size of the transducer prevents close spacing of the nozzles, and physical limitations of the transducer result in low ink drop velocity. Low drop velocity seriously diminishes tolerances for drop velocity variation and directionality, thus impacting the system's ability to produce high quality copies. Drop-on-demand systems which use piezoelectric devices to expel the droplets also suffer the disadvantage of a slow printing speed.


[0004] Another type of drop-on-demand system is known as thermal ink jet, or bubble jet, and produces high velocity droplets and allows very close spacing of nozzles. The major components of this type of drop-on-demand system are an ink filled channel having a nozzle on one end and a heat generating resistor near the nozzle. Printing signals representing digital information originate an electric current pulse in a resistive layer within each ink passageway near the orifice or nozzle, causing the ink in the immediate vicinity to evaporate almost instantaneously and create a bubble. The ink at the orifice is forced out as a propelled droplet as the bubble expands. When the hydrodynamic motion of the ink stops, the process is ready to start all over again. With the introduction of a droplet ejection system based upon thermally generated bubbles, commonly referred to as the “bubble jet” system, the drop-on-demand ink jet printers provide simpler, lower cost devices than their continuous stream counterparts, and yet have substantially the same high speed printing capability.


[0005] The operating sequence of the bubble jet system begins with a current pulse through the resistive layer in the ink filled channel, the resistive layer being in close proximity to the orifice or nozzle for that channel. Heat is transferred from the resistor to the ink. The ink becomes superheated far above its normal boiling point, and for water based ink, finally reaches the critical temperature for bubble formation or nucleation of around 280° C. Once nucleated, the bubble or water vapor thermally isolates the ink from the heater and no further heat can be applied to the ink. This bubble expands until all the heat stored in the ink in excess of the normal boiling point diffuses away or is used to convert liquid to vapor, which removes heat due to heat of vaporization. The expansion of the bubble forces a droplet of ink out of the nozzle, and once the excess heat is removed, the bubble collapses on the resistor. At this point, the resistor is no longer being heated because the current pulse has passed and, concurrently with the bubble collapse, the droplet is propelled at a high rate of speed in a direction towards a recording medium. The resistive layer encounters a severe cavitational force by the collapse of the bubble, which tends to erode it. Subsequently, the ink channel refills by capillary action. This entire bubble formation and collapse sequence occurs in about 10 microseconds. The channel can be refired after 100 to 500 microseconds minimum dwell time to enable the channel to be refilled and to enable the dynamic refilling factors to become somewhat dampened. Thermal ink jet processes are well known and are described in, for example, U.S. Pat. No. 4,601,777, U.S. Pat. No. 4,251,824, U.S. Pat. No. 4,410,899, U.S. Pat. No. 4,412,224, and U.S. Pat. No. 4,532,530, the disclosures of each of which are totally incorporated herein by reference.


[0006] Acoustic ink jet printing processes are also known. As is known, an acoustic beam exerts a radiation pressure against objects upon which it impinges. Thus, when an acoustic beam impinges on a free surface (i.e., liquid/air interface) of a pool of liquid from beneath, the radiation pressure which it exerts against the surface of the pool may reach a sufficiently high level to release individual droplets of liquid from the pool, despite the restraining force of surface tension. Focusing the beam on or near the surface of the pool intensifies the radiation pressure it exerts for a given amount of input power. These principles have been applied to prior ink jet and acoustic printing proposals. For example, K. A. Krause, “Focusing Ink Jet Head,” IBM Technical Disclosure Bulletin, Vol. 16, No. 4, September 1973, pp. 1168-1170, the disclosure of which is totally incorporated herein by reference, describes an ink jet in which an acoustic beam emanating from a concave surface and confined by a conical aperture was used to propel ink droplets out through a small ejection orifice. Acoustic ink printers typically comprise one or more acoustic radiators for illuminating the free surface of a pool of liquid ink with respective acoustic beams. Each of these beams usually is brought to focus at or near the surface of the reservoir (i.e., the liquid/air interface). Furthermore, printing conventionally is performed by independently modulating the excitation of the acoustic radiators in accordance with the input data samples for the image that is to be printed. This modulation enables the radiation pressure which each of the beams exerts against the free ink surface to make brief, controlled excursions to a sufficiently high pressure level for overcoming the restraining force of surface tension. That, in turn, causes individual droplets of ink to be ejected from the free ink surface on demand at an adequate velocity to cause them to deposit in an image configuration on a nearby recording medium. The acoustic beam may be intensity modulated or focused/defocused to control the ejection timing, or an external source may be used to extract droplets from the acoustically excited liquid on the surface of the pool on demand. Regardless of the timing mechanism employed, the size of the ejected droplets is determined by the waist diameter of the focused acoustic beam. Acoustic ink printing is attractive because it does not require the nozzles or the small ejection orifices which have caused many of the reliability and pixel placement accuracy problems that conventional drop-on-demand and continuous stream ink jet printers have suffered. The size of the ejection orifice is a critical design parameter of an ink jet because it determines the size of the droplets of ink that the jet ejects. As a result, the size of the ejection orifice cannot be increased, without sacrificing resolution. Acoustic printing has increased intrinsic reliability because there are no nozzles to clog. As will be appreciated, the elimination of the clogged nozzle failure mode is especially relevant to the reliability of large arrays of ink ejectors, such as page width arrays comprising several thousand separate ejectors. Furthermore, small ejection orifices are avoided, so acoustic printing can be performed with a greater variety of inks than conventional ink jet printing, including inks having higher viscosities and inks containing pigments and other particulate components. It has been found that acoustic ink printers embodying printheads comprising acoustically illuminated spherical focusing lenses can print precisely positioned pixels (i.e., picture elements) at resolutions which are sufficient for high quality printing of relatively complex images. It has also has been discovered that the size of the individual pixels printed by such a printer can be varied over a significant range during operation, thereby accommodating, for example, the printing of variably shaded images. Furthermore, the known droplet ejector technology can be adapted to a variety of printhead configurations, including (1) single ejector embodiments for raster scan printing, (2) matrix configured ejector arrays for matrix printing, and (3) several different types of pagewidth ejector arrays, ranging from single row, sparse arrays for hybrid forms of parallel/serial printing to multiple row staggered arrays with individual ejectors for each of the pixel positions or addresses within a pagewidth image field (i.e., single ejector/pixel/line) for ordinary line printing. Inks suitable for acoustic ink jet printing typically are liquid at ambient temperatures (i.e., about 25° C.), but in other embodiments the ink is in a solid state at ambient temperatures and provision is made for liquefying the ink by heating or any other suitable method prior to introduction of the ink into the printhead. Images of two or more colors can be generated by several methods, including by processes wherein a single printhead launches acoustic waves into pools of different colored inks. Further information regarding acoustic ink jet printing apparatus and processes is disclosed in, for example, U.S. Pat. No. 4,308,547, U.S. Pat. No. 4,697,195, U.S. Pat. No. 5,028,937, U.S. Pat. No. 5,041,849, U.S. Pat. No. 4,751,529, U.S. Pat. No. 4,751,530, U.S. Pat. No. 4,751,534, U.S. Pat. No. 4,801,953, and U.S. Pat. No. 4,797,693, the disclosures of each of which are totally incorporated herein by reference. The use of focused acoustic beams to eject droplets of controlled diameter and velocity from a free-liquid surface is also described in J. Appl. Phys., vol. 65, no. 9 (May 1, 1989) and references therein, the disclosure of which is totally incorporated herein by reference.


[0007] Other known droplet ejectors include those of the type disclosed in, for example, U.S. Pat. No. 6,127,198, the disclosure of which is totally incorporated herein by reference.


[0008] U.S. Pat. No. 6,001,899 (Gundlach et al.), the disclosure of which is totally incorporated herein by reference, discloses an ink composition which comprises water, an anionic dye, and a polyquaternary amine compound selected from the group consisting of polydiallyl ammonium compounds, polyquaternized polyvinylamines, polyquaternized polyallylamines, and mixtures thereof. Also disclosed are methods for using the aforementioned ink composition in ink jet printing processes.


[0009] U.S. Pat. No. 6,054,505 (Gundlach et al.), the disclosure of which is totally incorporated herein by reference, discloses an ink composition which comprises (1) water; (2) a nonpolymeric salt comprising at least one cation and at least one anion; and (3) a colorant comprising an anionic dye complexed with a polyquaternary amine compound. Also disclosed is an ink composition which comprises (1) water; (2) a nonpolymeric salt comprising at least one cation and at least one anion; (3) an anionic dye; and (4) a polyquaternary amine compound. In one embodiment, the polyquaternary amine compound is selected from the group consisting of polydiallyl ammonium compounds, polyquaternized polyvinylamines, polyquaternized polyallylamines, epichlorohydrin/amine copolymers, cationic amido amine copolymers, copolymers of vinyl pyrrolidinone and a vinyl imidazolium salt, and mixtures thereof.


[0010] U.S. Pat. No. 6,005,022 (Schwarz), the disclosure of which is totally incorporated herein by reference, discloses an ink composition which comprises (1) water; (2) a dye; and (3) a cationic amido amine copolymer. Also disclosed are methods for using the aforementioned ink composition in ink jet printing processes.


[0011] U.S. Pat. No. 5,990,198 (Schwarz), the disclosure of which is totally incorporated herein by reference, discloses an ink composition which comprises (1) water; (2) an anionic dye; and (3) a copolymer of vinyl pyrrolidinone and a vinyl imidazolium salt. Also disclosed are methods for using the aforementioned ink compositions in ink jet printing processes.


[0012] U.S. Pat. No. 6,258,873 (Gundlach et al.), the disclosure of which is totally incorporated herein by reference, discloses an ink composition which comprises water, an acid dye, a monovalent salt, a polyquaternary amine compound, and an optional nonionic or cationic surfactant, said ink being substantially free of organic solvents. The ink is particularly suitable for applications such as ink jet printing and marking pens. The disclosed inks in some embodiments are substantially indelible. Also disclosed is a composition for removing the ink compositions from substrates to which they have been applied which comprises water and a dianionic surfactant, optionally further containing a salt, urea, and/or a viscosity building agent such as a gum.


[0013] U.S. Pat. No. 6,274,645 (Gundlach et al.), the disclosure of which is totally incorporated herein by reference, discloses a washing composition which comprises a linear alkyl diphenyl oxide disulfonate compound, a chloride, bromide, iodide, nitrate, acetylacetonate, polyphosphate, squarate, or sulfonate salt or mixtures thereof, and a cosolvent which is propylene glycol, dipropylene glycol, tripropylene glycol, diethylene glycol, glycerine, trimethylolethane, trimethylolpropane, or mixtures thereof.


[0014] U.S. Pat. No. 6,174,355 (Mayo et al.), the disclosure of which is totally incorporated herein by reference, discloses an ink composition comprising a colorant and poly(diallyl diethyl ammonium) bromide. Also disclosed are ink jet printing processes, including thermal ink jet and acoustic ink jet printing processes, for using the inks.


[0015] U.S. Pat. No. 5,855,657 (Bergthaller et al.), the disclosure of which is totally incorporated herein by reference, discloses an ink jet ink that results in improved colorfastness if the ink contains a water soluble inorganic thiosulphate, trithionate, or tetrathionate or an organic thiosulphate, in an amount of 0.2 to 8 percent by weight with respect to the ink base.


[0016] U.S. Pat. No. 4,256,493 (Yokoyama et al.), the disclosure of which is totally incorporated herein by reference, discloses a jet ink composition which comprises an aqueous jet ink containing a water soluble dye, a wetting agent, and water as main components and, incorporated therein, a water soluble ultraviolet absorbing agent as well as a metal salt, when necessary.


[0017] While known compositions and processes are suitable for their intended purposes, a need remains for improved aqueous inks. In addition, a need remains for aqueous inks particularly suitable for use in ink jet printing processes. Further, a need remains for ink compositions with improved waterfastness. Additionally, a need remains for ink compositions with improved wet smear resistance. There is also a need for ink compositions with reduced intercolor bleed when two or more colors are printed adjacent to each other. In addition, there is a need for ink compositions for ink jet printing which contain acid dyes, which enable advantages such as bright colors, low cost, and high waterfastness when complexed with cationic polymers. Further, there is a need for ink compositions with improved shelf stability. Additionally, there is a need for ink compositions with improved jetting characteristics. A need also remains for ink compositions which exhibit excellent smear resistance. In addition, a need remains for ink compositions which are heat stable. Further, a need remains for ink compositions which exhibit freeze/thaw stability. Additionally, a need remains for ink compositions suitable for use in ink jet printing processes and having relatively low viscosities. There is also a need for ink compositions with one or more of the above advantages and also with improved lightfastness.



SUMMARY OF THE INVENTION

[0018] The present invention is directed to an ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound.



DETAILED DESCRIPTION OF THE INVENTION

[0019] Inks of the present invention contain an aqueous liquid vehicle and a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound. The liquid vehicle can consist solely of water, or it can comprise a mixture of water and a water soluble or water miscible organic component, such as ethylene glycol, propylene glycol, diethylene glycols, glycerine, dipropylene glycols, polyethylene glycols, polypropylene glycols, amides, ethers, urea, substituted ureas, ethers, carboxylic acids and their salts, esters, alcohols, organosulfides, organosulfoxides, sulfones (such as sulfolane), alcohol derivatives, carbitol, butyl carbitol, cellusolve, tripropylene glycol monomethyl ether, ether derivatives, amino alcohols, ketones, N-methylpyrrolidinone, 2-pyrrolidinone, cyclohexylpyrrolidone, hydroxyethers, amides, sulfoxides, lactones, polyelectrolytes, methyl sulfonylethanol, imidazole, betaine, and other water soluble or water miscible materials, as well as mixtures thereof. When mixtures of water and water soluble or miscible organic liquids are selected as the liquid vehicle, the water to organic ratio typically ranges from about 100:0 to about 30:70, and preferably from about 97:3 to about 40:60. The non-water component of the liquid vehicle generally serves as a humectant or cosolvent which has a boiling point higher than that of water (100° C.). In the ink compositions of the present invention, the liquid vehicle is typically present in an amount of from about 80 to about 99.9 percent by weight of the ink, and preferably from about 90 to about 99 percent by weight of the ink, although the amount can be outside these ranges.


[0020] The polyquaternary amine compound, which generally is complexed with the anionic dye in the ink, is a polymer containing quaternary groups in the repeat units thereof. The polymer typically has a weight average molecular weight of from about 1,000 to about 10,000,000, preferably from about 3,000 to about 1,000,000, and more preferably from about 5,000 to about 400,000, although the value can be outside of these ranges. The polymer typically has a number average molecular weight of from about 800 to about 11,000,000, preferably from about 3,300 to about 1,100,000, and more preferably from about 5,600 to about 450,000, although the value can be outside of these ranges. The polymer typically has from about 5 to about 70,000 repeat monomer units therein, preferably from about 21 to about 7,000 repeat monomer units, and more preferably from about 35 to about 2,800 repeat monomer units, although the number of repeat monomer units can be outside of this range. Suitable polyquaternary amine compounds typically are of the general formulae
1


[0021] wherein n is an integer representing the number of repeat monomer units, R1 and R7 each, independently of the other, is an alkylene group, including saturated, unsaturated, cyclic, and substituted alkylene groups (wherein hetero atoms, such as oxygen, sulfur, nitrogen, silicon, phosphorus, and the like can be present in the alkylene group, and the alkylene groups including polymethylene oxide groups, polyethylene oxide groups, polypropylene oxide groups, and the like), typically with from 1 to about 30 carbon atoms and preferably with from 1 to about 6 carbon atoms, an arylene group, including substituted arylene groups, typically with from 6 to about 50 carbon atoms and preferably with from 6 to about 18 carbon atoms, an arylalkylene group, including substituted arylalkylene groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, or an alkylarylene group, including substituted alkylarylene groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, and R2, R3, R4, R5, and R6 each, independently of the others, are hydrogen atoms, alkyl groups, including saturated, unsaturated, cyclic, and substituted alkyl groups (wherein hetero atoms, such as oxygen, sulfur, nitrogen, silicon, phosphorus, and the like can be present in the alkyl group), typically with from 1 to about 30 carbon atoms and preferably with from 1 to about 6 carbon atoms, aryl groups, including substituted aryl groups, typically with from 6 to about 50 carbon atoms and preferably with from 6 to about 18 carbon atoms, arylalkyl groups, including substituted arylalkyl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, or alkylaryl groups, including substituted alkylaryl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, wherein the substituents on the substituted alkyl, alkylene, aryl, arylene, arylalkyl, arylalkylene, alkylaryl, and alkylarylene groups can be (but are not limited to) hydroxy groups, amine groups, carbonyl groups, sulfide groups, halogen atoms, mixtures thereof, and the like, wherein two or more substituents can be joined together to form a ring.


[0022] Examples of suitable polyquaternary amine compounds include polydiallyl ammonium compounds, of the general formula
2


[0023] wherein n is an integer representing the number of repeat monomer units, R1 and R2 each, independently of the other, are hydrogen atoms, alkyl groups, including saturated, unsaturated, cyclic, and substituted alkyl groups (wherein hetero atoms, such as oxygen, sulfur, nitrogen, silicon, phosphorus, and the like can be present in the alkyl group), typically with from 1 to about 30 carbon atoms and preferably with from 1 to about 6 carbon atoms, aryl groups, including substituted aryl groups, typically with from 6 to about 50 carbon atoms and preferably with from about 6 to about 18 carbon atoms, arylalkyl groups, including substituted arylalkyl groups, typically with from about 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, or alkylaryl groups, including substituted alkylaryl groups, typically with from about 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, wherein the substituents on the substituted alkyl aryl, arylalkyl, and alkylaryl groups can be (but are not limited to) hydroxy groups, amine groups, carbonyl groups, sulfide groups, halogen atoms, mixtures thereof, and the like, wherein two or more substituents can be joined together to form a ring, and A is an anion, such as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO3, NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like, such as polydiallyl dimethyl ammonium compounds, including polydiallyl dimethyl ammonium chloride, of the formula
3


[0024] wherein n is an integer representing the number of repeat monomer units, commercially available with a molecular weight of about 400,000 (wherein n is an integer of about 2,500) from Calgon Corp. as 261-RV, and with a molecular weight of about 5,000 (wherein n is an integer of about 31) from Calgon Corp. as VARIKEM 110 or E2253.


[0025] Also suitable are polyquaternized polyvinylamines, of the general formula
4


[0026] wherein n is an integer representing the number of repeat monomer units, R1, R2, and R3 each, independently of the others, are hydrogen atoms, alkyl groups, including saturated, unsaturated, cyclic, and substituted alkyl groups (wherein hetero atoms, such as oxygen, sulfur, nitrogen, silicon, phosphorus, and the like can be present in the alkyl group), typically with from 1 to about 30 carbon atoms and preferably with from 1 to about 6 carbon atoms, aryl groups, including substituted aryl groups, typically with from 6 to about 50 carbon atoms and preferably with from about 6 to about 18 carbon atoms, arylalkyl groups, including substituted arylalkyl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, or alkylaryl groups, including substituted alkylaryl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, wherein the substituents on the substituted alkyl, aryl, arylalkyl, and alkylaryl groups can be (but are not limited to) hydroxy groups, amine groups, carbonyl groups, sulfide groups, halogen atoms, mixtures thereof, and the like, wherein two or more substituents can be joined together to form a ring, and A is an anion, such as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO3, NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like.


[0027] Also suitable are polyquaternized polyallylamines, of the general formula
5


[0028] wherein n is an integer representing the number of repeat monomer units, R1, R2, and R3 each, independently of the others, are hydrogen atoms, alkyl groups, including saturated, unsaturated, cyclic, and substituted alkyl groups (wherein hetero atoms, such as oxygen, sulfur, nitrogen, silicon, phosphorus, and the like can be present in the alkyl group), typically with from 1 to about 30 carbon atoms and preferably with from 1 to about 6 carbon atoms, aryl groups, including substituted aryl groups, typically with from 6 to about 50 carbon atoms and preferably with from about 6 to about 18 carbon atoms, arylalkyl groups, including substituted arylalkyl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, or alkylaryl groups, including substituted alkylaryl groups, typically with from 7 to about 60 carbon atoms and preferably with from 7 to about 20 carbon atoms, wherein the substituents on the substituted alkyl, aryl, arylalkyl, and alkylaryl groups can be (but are not limited to) hydroxy groups, amine groups, carbonyl groups, sulfide groups, halogen atoms, mixtures thereof, and the like, wherein two or more substituents can be joined together to form a ring, and A is an anion, such as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO331 , NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like.


[0029] Also suitable are epichlorohydrin/amine copolymers, including those of the general formula
6


[0030] wherein n is an integer of from about 3 to about 3,000, and preferably from about 5 to about 100, although the value can be outside of these ranges, and A is any suitable or desired anion, such as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO3, NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like. Polymers of this formula are commercially available from Hercules, Wilmington, Del. as RETEN 200 or RETEN 201 (molecular weight generally less than 10,000), and from Cytex, Inc., West Patterson, N.J., as CYPRO 514, 515, and 516 (wherein the polymers have a molecular weight range of from about 75,000 to about 250,000 and n is from about 870 to about 3,000), and as SUPERFLOC C567 (wherein the polymer has a molecular weight of about 10,000 and n is from about 110 to about 120, typically about 116).


[0031] Also suitable are cationic amido amine copolymers. Examples of suitable cationic amido amine copolymers include those of the general formula


(A—B)n2n+·2nX


[0032] wherein X is an anion, such as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO3, NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like, n is an integer representing the number of repeating monomer units, and typically is from about 2 to about 1,000, preferably from about 3 to about 200, more preferably from about 3 to about 100, and even more preferably from about 3 to about 10, although the value can be outside of these ranges, “A” is
7


[0033] and “B” is selected from the group consisting of (a) monomers of the formula
8


[0034] wherein p is an integer representing the number of repeat monomer units, and typically is from 1 to about 12, preferably from 1 to about 7, and more preferably from 1 to about 4, although the value can be outside of these ranges, such as (i) azeleic acid diamido, wherein p is 7, of the formula
9


[0035] or (ii) adipic acid diamido, wherein p is 4, of the formula
10


[0036] and (b) ureido, of the formula
11


[0037] Mixtures of two or more “B” monomers can also be used within the polymer. In a preferred embodiment, these specific polymers typically are condensation polymers, with alternating “A” and “B” monomer units. The weight average molecular weight of the polymer typically is from about 1,000 to about 100,000, preferably from about 1,000 to about 30,000, and more preferably from about 2,000 to about 5,000, although the value can be outside of these ranges. Copolymers of an amine and an amide are commercially available from, for example, Rhone-Poulenc, Cranbury, N.J., as, for example, MIRAPOL AZ-1, of the above formula wherein the “B” monomer is azeleic acid diamido, n has an average value of about 100, and the molecular weight is about 50,000, MIRAPOL AD-1, of the above formula wherein the “B” monomer is adipic acid diamido, n has an average value of about 100, and the molecular weight is about 50,000, and MIRAPOL A-15, of the above formula wherein the “B” monomer is ureido, n has an average value of about 6, and the molecular weight is about 2,260.


[0038] Also suitable are copolymers of vinyl pyrrolidinone and a vinyl imidazolium salt. In one embodiment, the copolymer is of a vinyl imidazolium salt of the formula
12


[0039] wherein X is an anion and R is a hydrogen atom or an alkyl group, typically with from 1 to about 8 carbon atoms and preferably with from 1 to about 3 carbon atoms, and vinyl pyrrolidinone, of the formula
13


[0040] wherein the copolymer is of the general formula
14


[0041] where X is any suitable or desired anion, as Cl, Br, I, HSO4, HSO3, SO42−, SO32−, CH3SO3, CH3C6H4SO3, NO3, HCOO, CH3COO, H2PO4, HPO42−, SCN, BF4, ClO4, SSO3, PF6, SbCl6, or the like, R is a hydrogen atom or an alkyl group, typically with from 1 to about 8 carbon atoms, and preferably with from 1 to about 3 carbon atoms, m is an integer representing the number of repeat vinyl imidazolium units, and n is an integer representing the number of repeat vinyl pyrrolidinone units. When R is a hydrogen atom, the pH of the ink can be adjusted to provide optimal ink-paper interaction; for example, the hydrogen atom can be extracted upon contact with the paper, or the cationic character of the polymer can be adjusted with ink pH. Random copolymers of the above formula generally are preferred, although alternating and block copolymers are also suitable. The weight average molecular weight of the polymer typically is from about 1,000 to about 1,000,000, preferably from about 1,000 to about 100,000, and more preferably from about 2,000 to about 5,000, although the value can be outside of these ranges. The ratio of vinyl imidazolium monomers to vinyl pyrrolidinone monomers typically is from about 99:1 to about 5:95, preferably from about 95:5 to about 20:80, more preferably from about 95:5 to about 30:70, and even more preferably from about 95:5 to about 50:50, although the value can be outside of these ranges. Vinyl pyrrolidinone/vinyl imidazolium salt copolymers are commercially available; for example, BASF, Parsippany, N.J., provides vinyl imidazolium chloride/vinyl pyrrolidinone copolymers (of the above formula wherein R is CH3) with a molecular weight of about 100,000 in three monomer ratios: LUVIQUAT® FC905 has a vinyl imidazolium chloride:vinyl pyrrolidinone ratio of 95:5 with 6.7 milliequivalents per gram of cationic groups, LUVIQUAT® FC550 has a vinyl imidazolium chloride:vinyl pyrrolidinone ratio of 50:50 with 3.0 milliequivalents per gram of cationic groups, and LUVIQUAT® FC370 has a vinyl imidazolium chloride:vinyl pyrrolidinone ratio of 30:70 with 1.8 milliequivalents per gram of cationic groups. Also available from BASF is LUVIQUAT® HM552, with a molecular weight of about 800,000 and a vinyl imidazolium chloride:vinyl pyrrolidinone ratio of 50:50.


[0042] Mixtures of two or more polyquaternary amine compounds can also be used.


[0043] Any suitable anionic dye or mixture of anionic dyes can be used. Examples of suitable dyes include Food dyes such as Food Black No. 1, Food Black No. 2, Food Red No. 40, Food Blue No. 1, Food Yellow No. 7, and the like, FD & C dyes, Acid Black dyes (No. 1, 7, 9, 24, 26, 48, 52, 58, 60, 61, 63, 92, 107, 109, 118, 119, 131, 140, 155, 156, 172, 194, and the like), Acid Red dyes (No. 1, 8, 32, 35, 37, 52, 57, 92, 115, 119, 154, 249, 254, 256, and the like), Acid Blue dyes (No. 1, 7, 9, 25, 40, 45, 62, 78, 80, 92, 102, 104, 113, 117, 127, 158, 175, 183, 193, 209, and the like), Acid Yellow dyes (No. 3, 7, 17, 19, 23, 25, 29, 38, 42, 49, 59, 61, 72, 73, 114, 128, 151, and the like), Direct Black dyes (No. 4, 14, 17, 22, 27, 38, 51, 112, 117, 154, 168, and the like), Direct Blue dyes (No. 1, 6, 8, 14, 15, 25, 71, 76, 78, 80, 86, 90, 106, 108, 123, 163, 165, 199, 226, and the like), Direct Red dyes (No. 1, 2, 16, 23, 24, 28, 39, 62, 72, 236, and the like), Direct Yellow dyes (No. 4, 11, 12, 27, 28, 33, 34, 39, 50, 58, 86, 100, 106, 107, 118, 127, 132, 142, 157, and the like), anthraquinone dyes, monoazo dyes, disazo dyes, phthalocyanine derivatives, including various phthalocyanine sulfonate salts, aza(18)annulenes, formazan copper complexes, triphenodioxazines, Bernacid Red 2BMN; Pontamine Brilliant Bond Blue A; Pontamine; Caro direct Turquoise FBL Supra Conc. (Direct Blue 199), available from Carolina Color and Chemical; Special Fast Turquoise 8GL Liquid (Direct Blue 86), available from Mobay Chemical; Intrabond Liquid Turquoise GLL (Direct Blue 86), available from Crompton and Knowles; Cibracron Brilliant Red 38-A (Reactive Red 4), available from Aldrich Chemical; Drimarene Brilliant Red X-2B (Reactive Red 56), available from Pylam, Inc.; Levafix Brilliant Red E-4B, available from Mobay Chemical; Levafix Brilliant Red E-6BA, available from Mobay Chemical; Procion Red H8B (Reactive Red 31), available from ICI America; Pylam Certified D&C Red #28 (Acid Red 92), available from Pylam; Direct Brilliant Pink B Ground Crude, available from Crompton & Knowles; Cartasol Yellow GTF Presscake, available from Sandoz, Inc.; Tartrazine Extra Conc. (FD&C Yellow #5, Acid Yellow 23), available from Sandoz; Carodirect Yellow RL (Direct Yellow 86), available from Carolina Color and Chemical; Cartasol Yellow GTF Liquid Special 110, available from Sandoz, Inc.; D&C Yellow #10 (Acid Yellow 3), available from Tricon; Yellow Shade 16948, available from Tricon, Basacid Black X34, available from BASF, Carta Black 2GT, available from Sandoz, Inc.; Neozapon Red 492 (BASF); Savinyl Blue GLS (Sandoz); Luxol Blue MBSN (Morton-Thiokol); Basacid Blue 750 (BASF); Bernacid Red, available from Berncolors, Poughkeepsie, N.Y.; Pontamine Brilliant Bond Blue; Berncolor A.Y. 34; Telon Fast Yellow 4GL-175; BASF Basacid Black SE 0228; the Pro-Jet® series of dyes available from ICI, including Pro-Jet® Yellow I (Direct Yellow 86), Pro-Jet® Magenta I (Acid Red 249), Pro-Jet® Cyan I (Direct Blue 199), Pro-Jet® Black I (Direct Black 168), Pro-Jet® Yellow 1-G (Direct Yellow 132), Aminyl Brilliant Red F-B, available from Sumitomo Chemical Company (Japan), the Duasyn® line of “salt-free” dyes available from Hoechst, such as Duasyn® Direct Black HEF-SF (Direct Black 168), Duasyn® Black RL-SF (Reactive Black 31), Duasyn® Direct Yellow 6G-SF VP216 (Direct Yellow 157), Duasyn® Brilliant Yellow GL-SF VP220 (Reactive Yellow 37), Duasyn® Acid Yellow XX-SF LP413 (Acid Yellow 23), Duasyn® Brilliant Red F3B-SF VP218 (Reactive Red 180), Duasyn® Rhodamine B-SF VP353 (Acid Red 52), Duasyn® Direct Turquoise Blue FRL-SF VP368 (Direct Blue 199), Duasyn® Acid Blue AE-SF VP344 (Acid Blue 9), various Reactive dyes, including Reactive Black dyes, Reactive Blue dyes, Reactive Red dyes, Reactive Yellow dyes, and the like, as well as mixtures thereof.


[0044] Any desired or suitable anionic lightfastness-imparting agent can be used. For example, one class of suitable lightfastness-imparting agents is that of ultraviolet absorbers. These materials improve lightfastness by absorbing short wavelength radiation and dissipating it thermally or by mechanisms such as fluorescence or the like, thereby preventing the short wavelength radiation from harming the chromophore. Examples of suitable lightfastness-imparting agents in this class include (hydroxyphenyl)benzotriazoles, of the general formulae
15


[0045] hydroxybenzophenones, of the general formulae
16


[0046] hydroxybenzoic acids, of the general formulae
17


[0047] alkoxybenzoic acids, of the general formulae
18


[0048] wherein R is an alkyl group, typically with from 1 to about 12 carbon atoms, although the number of carbon atoms can be outside of this range, esters of substituted benzoic acids, of the general formula
19


[0049] wherein R′ is an alkyl group, typically with from 1 to about 12 carbon atoms, although the number of carbon atoms can be outside of this range, (hydroxyphenyl)1,3,5 triazines, of the general formulae
20


[0050] and the like, wherein in all of the above generic formulae, A is a substituent containing an anionic moiety. A can be either an anionic moiety by itself, such as a carboxylate group, sulfonate group, phosphonate group, or the like, or can be an aliphatic or aromatic group (including aliphatic and aromatic groups containing hetero atoms, such as oxygen, nitrogen, sulfur, silicon, phosphorus, or the like) to which an anionic group is attached. It is to be understood that other substituents can also be present on materials of these formulae. Many compounds in these classes and having ionizable ionic substitutents are commercially available, such as 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid; 2,2′-dihydroxy-4,4′dimethoxybenzophenone-5-sulfonic acid; 2,3-dimethoxybenzoic acid; 3,4-dimethoxybenzoic acid; 3,5-dimethoxybenzoic acid; 2,5-dimethoxybenzoic acid; 2,6-dimethoxybenzoic acid 3,4-dimethoxybenzenesulfonic acid; 3,4,5-trimethoxybenzoic acid; 2,4,5-trimethoxybenzoic acid; 4,5-dimethoxyphthalic acid; 2,3-bis-isopropylidenedioxybenzoic acid; 2,3-bis-(carboxymethyloxy)-benzoic acid; 2,5-dihydroxyphenylacetic acid; and the like, commercially available from sources such as Aldrich Chemical Co., Milwaukee, Wis., and Chem Service Inc., Westchester, Pa. Also suitable are compounds and salts thereof such as those of the following formulae, disclosed in, for example, U.S. Pat. No. 5,686,633, the disclosure of which is totally incorporated herein by reference:
21


[0051] and the like, as well as mixtures thereof. Materials of these formulae can be prepared as disclosed in, for example, U.S. Pat. No. 5,686,633, the disclosure of which is totally incorporated herein by reference. Mixtures of two or more of these lightfastness-imparting agents can also be employed.


[0052] Another class of suitable lightfastness-imparting agents is that of reducing agents. These materials improve lightfastness by interacting with free radicals that might be formed by incident radiation, thereby preventing such radicals from harming the chromophore. Examples of suitable lightfastness-imparting agents in this class include sulfite salts, thiosulfate salts, trithionate salts, tetrathionate salts, and the like, as well as mixtures thereof. These salts are generally easily commercially available as sodium salts; other salts, however, such as any water soluble alkali metal or alkaline earth metal salts of these reducing anions, are also suitable.


[0053] The polyquaternary amine compound, anionic dye, and anionic lightfastness-imparting agent can be present in any desired or effective relative amounts. Typically, the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the dye molecule is at least about 1.5, preferably at least about 2, and more preferably at least about 3, and typically no more than about 10, preferably no more than about 7, and more preferably no more than about 5, although the relative amounts of anionic dye and polyquaternary amine can be outside of these ranges. Typically, the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the lightfastness-imparting agent molecule is at least about 1, preferably at least about 1.5, and more preferably at least about 2, and typically no more than about 5, preferably no more than about 3, and more preferably no more than about 2.5, although the relative amounts of anionic lightfastness-imparting agent and polyquaternary amine can be outside of these ranges. Typically the molar ratio of dye molecules to lightfastness-imparting agent molecules is at least about 2:1, preferably at least about 3:1, and more preferably at least about 4:1, and typically no more than about 20:1, preferably no more than about 10:1, and more preferably no more than about 5:1, although the relative amounts of anionic lightfastness-imparting agent and anionic dye can be outside of these ranges.


[0054] The ratio of cationic sites on the polymer and anionic sites on the dye and the lightfastness agent in specific embodiments are nearly stoichiometric, with a slight excess of quaternary ammonium sites. Further, in specific embodiments, the molar concentration of the dye is about 10 times that of the lightfastness agent. The concentration of dye present in the ink depends on the color and optical density desired; in ink jet inks the dye concentration typically is from about 1 to about 5 percent by weight of the ink, although the amount can be outside of this range.


[0055] The complex of the anionic dye, anionic lightfastness-imparting agent, and polyquaternary amine compound can be prepared by any desired or suitable method. For example, these ingredients can all be admixed with the other ink ingredients so that the complex forms within the ink. In one instance, a process wherein a reducing agent lightfastness-imparting agent was first dissolved in water, followed by addition of the polyquaternary amine compound to the solution, followed by addition of the ink cosolvents or humectants to the solution, followed by addition of the anionic dye to the solution, was found to work well. Alternatively, inks of the present invention can be made by first preparing a preformed complex of the dye and/or the lightfastness-imparting agent, by the method disclosed in Copending application U.S. Ser. No. (not yet assigned; Attorney Docket No. D/A1422), filed concurrently herewith.


[0056] While not being limited to any particular theory, it is believed that in the inks according to the present invention, the lightfastness-imparting agent and the anionic dye are both complexed to the polyquaternary amine compound, and are thus in close proximity to each other; accordingly, the lightfastness-imparting agent is always in a location wherein it can function most efficaciously in protecting the chromophore from degradation caused by short wave radiation such as ultraviolet radiation. This protection is particularly important in ink compositions that employ an anionic dye in combination with cationic fixing agents. The use of anionic dyes (Acid, Direct, and Reactive classes) and cationic compounds in combination is known in dyeing processes and ink jet printing, wherein cationic compounds serve as dye fixing agents to improve waterfastness. It is known that the cationic agent sometimes reduces the lightfastness of dyes (see T. S. Wu and K. M. Chen, J.S.D.C., 108 (1992) 388, the disclosure of which is totally incorporated herein by reference). Oka and Kimura (J.S.D.C., 111 (1995) 311-315, the disclosure of which is totally incorporated herein by reference) studied the photofading of the combination of the anionic dye Acid Red 249 and Polyfix 601, of the formula
22


[0057] They found that while aqueous solutions of Acid Red 249 showed high lightfastness, the presence of a polycation caused a dramatic reduction in the lightfastness of Acid Red 249. They also found that the reduction in lightfastness was related to the degree of dye aggregation. Experiments under aerated and oxygen-free conditions demonstrated that the rapid photofading of Acid Red 249 in the presence of a polycation proceeded predominantly by a photo-oxidative process. Oka and Kimua concluded that electron transfer from a photoexcited anionic radical of Acid Red 249 to oxygen retarded the non-degradative charge recombination process that occurs in the absence of oxygen. Dye aggregation in the presence of a polycation facilitated charge separation and photofading.


[0058] While not being limited to any particular theory or mechanism of action, it is believed that incorporation of anionic lightfastness agents in accordance with the teachings of this invention promote the lightfastness of ternary mixtures of an anionic lightfastness-imparting agent and anionic dye in association with a polyquaternary amine compound by separating the dye molecules associated with the anionic polymer with anionic reagents that can actively interact with photoexcited dye molecules to promote non-destructive recombination of photoexcited anionic radicals and intercept destructive free-radical intermediates.


[0059] The inks of the present invention can optionally further contain a nonpolymeric salt comprising at least one cation and at least one anion. Examples of suitable cations include alkali metal cations, such as Li+, Na+, and K+, alkaline earth metal cations, such as Mg2+and Ca2+, Al3+, transition metals, nonpolymeric or monomeric ammonium and quaternary amine cations, including those of the general formula
23


[0060] wherein each of R1, R2, R3, and R4, independently of the others, is a hydrogen atom, an alkyl group (including saturated, unsaturated, cyclic, and substituted alkyl groups, wherein substituted alkyl groups can include alkoxy or polyalkoxy groups such as ethylene oxide, polyethylene oxide, or the like), preferably with from 1 to about 10 carbon atoms and more preferably with from 1 to about 4 carbon atoms, although the number of carbon atoms can be outside of this range, aryl groups, including substituted aryl groups, preferably with from 6 to about 18 carbon atoms and more preferably with from 6 to about 12 carbon atoms, although the number of carbon atoms can be outside of this range, arylalkyl groups, preferably with from 7 to about 20 carbon atoms and more preferably with from 7 to about 13 carbon atoms, or alkylaryl groups, preferably with from 7 to about 20 carbon atoms and more preferably with from 7 to about 13 carbon atoms, wherein the substituents on the substituted alkyl, aryl, arylalkyl, and alkylaryl groups can be (but are not limited to) hydroxy groups, carbonyl groups, sulfide groups, mixtures thereof, and the like, wherein two or more substituents can be joined together to form a ring, with specific examples of ammonium and quaternary amine cations including NH4+, N(CH3)4+, H3NCH2CH2NH32+, (H3C)3NCH2CH2N(CH3)32+, imidazolium, quaternized 1,4-diazabicyclo(2.2.2)octane, choline, of the formula
24


[0061] alkyl amine quaternary salts such as ETHOQUAD C/12, of the formula
25


[0062] wherein R is a long chain alkyl group with 12 carbon atoms, x and y are integers of 0, 1, or 2 representing the number of ethoxy groups, wherein x+y=2, and A is an anion, such as chloride, commercially available from Akzo Chemie, Chicago, Ill., and the like, as well as mixtures thereof. Any desired anion can be employed. Examples of suitable anions include NO3, ClO4, SO42−, PF6, BF4, organic strong acid anions, such as tosylate, mesylate, triflate, trifluoroacetate, sulfamate, and the like, organic weak acid anions, such as formate, acetate, propionate, and the like, acetylacetonate, of the formula
26


[0063] squarate, of the formula
27


[0064] halides, including chloride, bromide, and iodide, and the like, as well as mixtures thereof. Specific examples of suitable salts include lithium chloride, lithium bromide, lithium iodide, lithium nitrate, lithium formate, lithium acetate, lithium propionate, sodium chloride, sodium bromide, sodium iodide, sodium nitrate, sodium perchlorate, sodium formate, sodium acetate, sodium propionate, potassium chloride, potassium bromide, potassium iodide, potassium formate, potassium acetate, potassium propionate, calcium chloride, calcium nitrate, calcium formate, calcium acetate, calcium propionate, magnesium chloride, magnesium sulfate, magnesium formate, magnesium acetate, magnesium propionate, ammonium chloride, ammonium bromide, ammonium iodide, ammonium acetate, ammonium formate, ammonium nitrate, ammonium sulfate, ammonium propionate, tetramethylammonium chloride, tetramethylammonium formate, tetramethylammonium acetate, tetramethylammonium propionate, ethylene diamine dihydrochloride, 1,4-diazabicyclo(2.2.2)octane salts, such as hexamethonium bromide, of the formula
28


[0065] imidazole salts, such as imidazolium chloride, acetylacetonate salts, such as lithium acetylacetonate, squarate salts, such as tetramethylammonium squarate, choline salts, such as choline chloride, ETHOQUAD C/12, and the like. Salts with oxidizing anions, such as NO3, ClO4, and the like, should not be used in ink compositions that employ reducing salts (bisulfite, thiosulfate, trithionate tetrathionate, or the like) as lightfastness-enhancing agents.


[0066] The salt is present in the ink in any desired or effective amount, typically at least about 0.1 percent by weight of the ink, preferably at least about 1 percent by weight of the ink, and more preferably at least about 5 percent by weight of the ink, and typically no more than about 40 percent by weight of the ink, preferably no more than about 30 percent by weight of the ink, more preferably no more than about 20 percent by weight of the ink, and even more preferably no more than about 15 percent by weight of the ink, although the amount can be outside of these ranges. The preferred relative amounts of salt and anionic dye in the ink can also be expressed as a stoichiometric ratio, with the molar ratio of anions in the added salt to anionic dye groups typically being from about 0:1 to about 100:1 for anionic dyes and from about 0:1 to about 500:1 for direct dyes. For all anionic dyes (acid dyes, direct dyes, reactive dyes, and the like), the preferred molar ratio of anions in the added salt to anionic dye groups from about 5:1 to about 100:1, more preferably from about 10:1 to about 80:1. The molar ratio of anions in the added salt to anionic dye groups can, however, be outside of these ranges.


[0067] While not being limited to any particular theory, it is believed that the presence of the salt suppresses the extent to which the complex is associated in solution, and thereby solubilizes the dye/quaternary polymer complex in the inks of the present invention. Again, while not being limited to any particular theory, it is believed that within the ink, the polyquaternary amine tends to be associated with the anionic dye and the lightfastness-imparting agent, with the dye and the lightfastness-imparting agent playing the roles of counterions. The complex is rendered soluble in the ink vehicle by virtue of the presence of water soluble ionic salts, the anions of which limit the extent of association of anionic dyes with the quaternary polymer in solution. The presence of the salt in the ink can also reduce jitter when the ink is jetted and increase ink surface tension.


[0068] Other optional additives to the inks include biocides such as Dowicil 150, 200, and 75, benzoate salts, sorbate salts, and the like, present in an amount of from about 0.0001 to about 4 percent by weight of the ink, and preferably from about 0.01 to about 2.0 percent by weight of the ink, pH controlling agents such as acids or, bases, phosphate salts, carboxylates salts, sulfite salts, amine salts, and the like, present in an amount of from 0 to about 1 percent by weight of the ink and preferably from about 0.01 to about 1 percent by weight of the ink, or the like.


[0069] When used in ink jet printing applications, the ink compositions according to the present invention are generally of a viscosity suitable for use in said ink jet printing processes. For example, for thermal ink jet printing applications, at room temperature (i.e., about 25° C.), typically, the ink viscosity is typically at least about 1 centipoise and typically is up to about 10 centipoise, preferably up to about 5 centipoise, and more preferably up to about 4 centipoise, although the viscosity can be outside these ranges, particularly when the ink is used for applications such as acoustic ink jet printing. When used in marking pen applications, the ink compositions are generally of a viscosity suitable for use in said applications.


[0070] The ink compositions can be of any suitable or desired pH. For some embodiments, such as thermal ink jet printing processes, typical pH values are at least about 3, preferably at least about 5, and more preferably at least about 6, and typically up to about 11, preferably up to about 10, and more preferably up to about 9, although the pH can be outside of these ranges.


[0071] The ink compositions can be prepared by any suitable process. Typically, the inks are prepared by simple mixing of the ingredients. One process entails mixing all of the ink ingredients together and filtering the mixture to obtain an ink. Inks can be prepared by mixing the ingredients, heating if desired, and filtering, followed by adding any desired additional additives to the mixture and mixing at room temperature with moderate shaking until a homogeneous mixture is obtained, typically from about 5 to about 10 minutes. Alternatively, the optional ink additives can be mixed with the other ink ingredients during the ink preparation process, which takes place according to any desired procedure, such as by mixing all the ingredients, heating if desired, and filtering.


[0072] The ink compositions of the present invention can be used in a process which entails incorporating the ink composition into an ink jet printing apparatus and causing droplets of the ink composition to be ejected in an imagewise pattern onto a substrate. In a particularly preferred embodiment, the printing apparatus employs a thermal ink jet process wherein the ink in the nozzles is selectively heated in an imagewise pattern, thereby causing droplets of the ink to be ejected in imagewise pattern. In another embodiment, the printing apparatus employs an acoustic ink jet process wherein droplets of the ink are caused to be ejected in imagewise pattern by acoustic beams. In yet another embodiment, the printing apparatus employs a piezoelectric ink jet process, wherein droplets of the ink are caused to be ejected in imagewise pattern by oscillations of piezoelectric vibrating elements. Any suitable substrate can be employed, including plain papers such as Xerox® 4024 papers, Xerox® Image Series papers, Courtland 4024 DP paper, ruled notebook paper, bond paper, silica coated papers such as Sharp Company silica coated paper, JuJo paper, and the like, transparency materials, fabrics, textile products, plastics, polymeric films, inorganic substrates such as metals and wood, and the like. In a preferred embodiment, the process entails printing onto a porous or ink absorbent substrate, such as plain paper.


[0073] Specific embodiments of the invention will now be described in detail. These examples are intended to be illustrative, and the invention is not limited to the materials, conditions, or process parameters set forth in these embodiments. All parts and percentages are by weight unless otherwise indicated.







EXAMPLE I

[0074] An ink composition was prepared by admixing 10 parts by weight of sodium thiosulfate (obtained from Fisher Scientific, Fairlawn, N.J.) with 22.4 parts by weight of deionized water with stirring. To this mixture was then added with stirring 6 parts by weight of an aqueous solution containing about 30 percent by weight of poly(dimethyldiallyl ammonium chloride) (CALGON® CP-1030, obtained from Nalco Chemical, Naperville, Ill.). Subsequently, to this mixture was added with stirring 10 parts by weight of 2-pyrrolidinone (containing 95 percent by weight pure 2-pyrrolidinone and 5 percent by weight water; obtained from BASF, Mt. Olive, N.J.), 20 parts by weight of sulfolane (containing 95 percent by weight pure sulfolane and 5 percent by weight water) (obtained from Phillips Petroleum Co., Bartlesville, Okla.), and 1 part by weight of N-octyl-2-pyrrolidinone (obtained from Aldrich Chemical Co., Milwaukee, Wis.). Thereafter, to this mixture was added with stirring 5 parts by weight of PROJET® RED OAM dye (Acid Red 52; aqueous solution containing 8.5 percent by weight dye solids; obtained from Avecia, Inc., Wilmington, Del.) and 25 parts by weight of PROJET® MAGENTA 1-3BOA (aqueous solution containing 10 percent by weight dye solids; obtained from Avecia, Inc., Wilmington, Del.).



EXAMPLE II

[0075] An ink composition was prepared by admixing 2.0 parts by weight of sodium thiosulfate pentahydrate (obtained from Fisher Scientific, Fairlawn, N.J.) and 8 parts by weight of choline chloride with 22.4 parts by weight of deionized water with stirring. To this mixture was then added with stirring 6 parts by weight of an aqueous solution containing about 30 percent by weight of poly(dimethyldiallyl ammonium chloride) (CALGON® CP-1030, obtained from Nalco Chemical, Naperville, Ill.). Subsequently, to this mixture was added with stirring 10 parts by weight of 2-pyrrolidinone (containing 95 percent by weight pure 2-pyrrolidinone and 5 percent by weight water; obtained from BASF, Mt. Olive, N.J.), 20 parts by weight of sulfolane (containing 95 percent by weight pure sulfolane and 5 percent by weight water; obtained from Phillips Petroleum Co., Bartlesville, Okla.), and 1 part by weight of N-octyl-2-pyrrolidinone (obtained from Aldrich Chemical Co., Milwaukee, Wis.). Thereafter, to this mixture was added with stirring 5 parts by weight of PROJET® RED OAM dye (Acid Red 52; aqueous solution containing 8.5 percent by weight dye solids; obtained from Avecia Inc., Wilmington, Del.) and 25 parts by weight of PROJET® MAGENTA 1-3BOA (aqueous solution containing 10 percent by weight dye solids; obtained from Avecia, Wilmington, Del.).



EXAMPLE III


Comparative

[0076] For comparison purposes, an ink similar to that of Example I was made by the same process except that 10 parts by weight of choline chloride (obtained from Aldrich Chemical Co., Milwaukee, Wis.) was substituted for the 10 parts by weight of sodium thiosulfate and that 6.6 parts by weight of the poly(dimethyldiallyl ammonium chloride) solution were used instead of 6 parts by weight. with deionized water to generate approximately 5 percent by weight solids aqueous solutions. These solutions were mixed (adding the dye solution to a stirred solution of the quaternary polymer). A precipitate formed immediately in each case and was isolated by centrifugation.



EXAMPLE IV


Synthesis of Poly(dimethyldiallyammonium/Acid Yellow 23) Complex

[0077] In the preparation of the poly(dimethyldiallyammonium/Acid Yellow 23) complex, 1 mole of Acid Yellow 23 was mixed with 4 molar repeat residues (C8H6N+) of the poly(dimethyldiallyammonium chloride) to yield a precipitate that comprised 2.7 C8H6N+ residues per mole of Acid Yellow 23.



EXAMPLE V


Synthesis of Poly(dimethyldiallyammonium/Acid Red 52) Complex

[0078] In the preparation of the poly(dimethyldiallyammonium/Acid Red 52) complex, 1 mole of Acid Red 52 was mixed with 3 molar repeat residues (C8H6N+) of the poly(dimethyldiallyammonium chloride) to yield a precipitate that comprised 2.0 C8H6N+ residues per mole of Acid Red 52.



EXAMPLE VI


Synthesis of Poly(dimethyldiallyammonium/PROJET MAGENTA 3BOA) Complex

[0079] In the preparation of the poly(dimethyldiallyammonium/PROJET MAGENTA 3BOA) complex, 1 mole of triazine dye was mixed with 5 molar repeat residues (C8H6N+) of the poly(dimethyldiallyammonium chloride) to yield a precipitate that comprised 5.0 C8H6N+ residues per mole of triazine dye.



EXAMPLE VII


Synthesis of Poly(dimethyldiallyammonium/Acid Blue 9) Complex

[0080] In the preparation of the poly(dimethyldiallyammonium/Acid Blue 9) complex, 1 mole of cyan dye was mixed with 3 molar repeat residues (C8H6N+) of the poly(dimethyldiallyammonium chloride) to yield a precipitate that comprised 2.0 C8H6N+ residues per mole of cyan dye.


[0081] The inks of Examples VIII through X are each prepared by adding the quaternary polymer/dye complex prepared in one of Examples I to IV to a mixture of the other ink ingredients (water, cosolvents, salt, etc.) and agitating the mixture gently until the quaternary polymer/dye complex is dissolved in the solution. This dissolution typically is accomplished within a period of 15 minutes to 2 hours. As a matter of practice, mixtures are commonly agitated overnight (16 hours). The inks are then syringe filtered through a Gelman Laboratory Acrodisc® 37 mm Syringe Filter with a 1 micron Glass Fiber Membrane.



EXAMPLE VIII

[0082]

1











Yellow Ink Containing Poly(dimethyldiallylammonium/Acid Yellow 23)


Comolex, Anionic UV Stabilizer, and Auxiliary Salt, CaCl2











Amount




(parts by


Ingredient
Supplier
weight)












deionized water

51.7


sulfolane*
Phillips 66
20.0


calcium chloride dihydrate
Aldrich Chemical Co.
5.03


2-pyrrolidinone
Aldrich Chemical Co.
10.0


2,2′-dihydroxy-4,4′-dimethoxy-
Chem Service
0.50


benzophenone-5-sulfonic acid,


sodium salt


poly(diallyldimethylammonium
Example IV
5.77


chloride)/Acid Yellow 23


Complex


1-octyl-2-pyrrolidinone
Aldrich Chemical Co.
1.0






*95 wt. % sulfolane, 5 wt. % water









EXAMPLE IX

[0083]

2











Magenta Ink Containing Poly(dimethyldiallylammonium/Red Dye)


Complexes, Anionic UV Stabilizer, and Auxiliary Salt, CaCl2











Amount




(parts by


Ingredient
Supplier
weight)












Deionized water

57.3


sulfolane*
Phillips 66
20.0


calcium chloride dihydrate
Aldrich Chemical Co.
5.03


2-pyrrolidinone
Aldrich Chemical Co.
10.0


2,2′-dihydroxy-4,4′-dimethoxy-
Chem Service
0.50


benzophenone-5-Sulfonic acid,


sodium salt


poly(diallyldimethylammonium
Example VI
5.56


chloride)/PROJET MAGENTA


3BOA Complex


poly(diallyldimethylammonium
Example V
0.61


chloride)/Acid Red 52 Complex


1-octyl-2-pyrrolidinone
Aldrich Chemical Co.
1.0






*95 wt. % sulfolane, 5 wt. % water









EXAMPLE X

[0084]

3











Cyan Ink Containing Poly(Dimethyldiallylammonium/Acid Blue 9)


Complex, Anionic UV Stabilizer, and Auxiliary Salt, CaCl2











Amount




(parts by


Ingredient
Supplier
weight)












Deionized water

57.7


sulfolane*
Phillips 66
20.0


calcium chloride dihydrate
Aldrich Chemical Co.
5.03


2-pyrrolidinone
Aldrich Chemical Co.
10.0


2,2′-dihydroxy-4,4'-dimethoxy-
Chem Service
0.50


benzophenone-5-sulfonic acid,


sodium salt


poly(diallyldimethylammonium
Example VII
3.6


chloride)/Acid Blue 9 Complex


1-octyl-2-pyrrolidinone
Aldrich Chemical Co.
1.0






*95 wt. % sulfolane, 5 wt. % water








[0085] Other embodiments and modifications of the present invention may occur to those of ordinary skill in the art subsequent to a review of the information presented herein; these embodiments and modifications, as well as equivalents thereof, are also included within the scope of this invention.


[0086] The recited order of processing elements or sequences, or the use of numbers, letters, or other designations therefor, is not intended to limit a claimed process to any order except as specified in the claim itself.


Claims
  • 1. An ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound.
  • 2. An ink according to claim 1 wherein the polyquaternary amine compound is of the formulae
  • 3. An ink according to claim 1 wherein the polyquaternary amine compound is selected from the group consisting of polydiallyl ammonium compounds, polyquaternized polyvinylamines, polyquaternized polyallylamines, epichlorohydrin/amine copolymers, cationic amido amine copolymers, copolymers of vinyl pyrrolidinone and a vinyl imidazolium salt, and mixtures thereof.
  • 4. An ink according to claim 1 wherein the polyquaternary amine compound is a polydiallyl dimethyl ammonium compound.
  • 5. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is an ultraviolet absorber.
  • 6. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is selected from the group consisting of (hydroxyphenyl)benzotriazoles, hydroxybenzophenones, hydroxybenzoic acids, alkoxybenzoic acids, esters of substituted benzoic acids, (hydroxyphenyl)1,3,5 triazines, and mixtures thereof.
  • 7. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is selected from the group consisting of 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid; 2,2′-dihydroxy-4,4′dimethoxybenzophenone-5-sulfonic acid; 2,3-dimethoxybenzoic acid; 3,4-dimethoxybenzoic acid, 3,5-dimethoxybenzoic acid; 2,5-dimethoxybenzoic acid; 2,6-dimethoxybenzoic acid 3,4-dimethoxybenzenesulfonic acid; 3,4,5-trimethoxybenzoic acid; 2,4,5-trimethoxybenzoic acid; 4,5-dimethoxyphthalic acid; 2,3-bis-isopropylidenedioxybenzoic acid; 2,3-bis-(carboxymethyloxy)-benzoic acid; 2,5-dihydroxyphenylacetic acid; and mixtures thereof.
  • 8. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is selected from the group consisting of
  • 9. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is a reducing agent.
  • 10. An ink according to claim 1 wherein the anionic lightfastness-imparting agent is selected from the group consisting of sulfite salts, thiosulfate salts, trithionate salts, tetrathionate salts, and mixtures thereof.
  • 11. An ink according to claim 1 wherein the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the dye molecule is at least about 1.5, and wherein the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the dye molecule is no more than about 10.
  • 12. An ink according to claim 1 wherein the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the lightfastness-imparting agent molecule is at least about 1, and wherein the number of cationic sites on the polyquaternary amine molecule for every one anionic site on the lightfastness-imparting agent molecule is no more than about 5.
  • 13. An ink according to claim 1 wherein the molar ratio of dye molecules to lightfastness-imparting agent molecules is at least about 2:1, and wherein the molar ratio of dye molecules to lightfastness-imparting agent molecules is no more than about 20:1.
  • 14. An ink according to claim 1 further containing a nonpolymeric salt.
  • 15. An ink according to claim 14 wherein the nonpolymeric salt is present in the ink in an amount of at least about 0.1 percent by weight of the ink, and wherein the nonpolymeric salt is present in the ink in an amount of no more than about 40 percent by weight of the ink.
  • 16. A process which comprises (a) incorporating into an ink jet printing apparatus an ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound, and (b) causing droplets of the ink composition to be ejected in an imagewise pattern onto a substrate.
  • 17. A process according to claim 16 wherein the printing apparatus employs a thermal ink jet process wherein the ink in the nozzles is selectively heated in an imagewise pattern, thereby causing droplets of the ink to be ejected in imagewise pattern.
  • 18. A process according to claim 16 wherein the printing apparatus employs an acoustic ink jet process wherein droplets of the ink are caused to be ejected in imagewise pattern by acoustic beams.
  • 19. A process according to claim 16 wherein the printing apparatus employs a piezoelectric ink jet process, wherein droplets of the ink are caused to be ejected in imagewise pattern by oscillations of piezoelectric vibrating elements.
  • 20. A process which comprises (a) incorporating into an ink jet printing apparatus an ink composition comprising (a) water and (b) a complex of (i) an anionic dye, (ii) an anionic lightfastness-imparting agent, and (iii) a polyquaternary amine compound, and (b) causing droplets of the ink composition to be ejected in an imagewise pattern onto a paper substrate.