The present invention is related to integrated electric double-layer ultracapacitor with carbon composite electrodes of high energy density having a cylindrical housing and to the battery composed from ultracapacitors.
From the prior art is known various construction of the double-layer capacitors. In document EE05629, 16.04.2012, OU Skeleton Technologies the inventors of the present invention are describing a prismatic double-layer capacitor. Until now the main problem with cylindrical double-layer capacitors is the contact between the electrode and current terminal.
From documents WO03/041097, 15.05.2003, Maxwell Technologies, Inc. is described double-layer capacitor comprising a first terminal and second terminal, a rolled electrode structure placed into capacitor can. Thereafter the capacitor can is closed with contact edge and first stud/collector. The second disk/terminal post is placed to the other end of the capacitor can. The main problem of cylindrical capacitors is contact between the “jellyroll” electrode and current terminal.
US2009/0180238, 16.07.2009, Maxwell Technologies, Inc., describes a double-layer energy storage device comprising a first current collector and a second current collector having opposite sides, a first and second electrode structure is disposed adjacent to opposing sides of corresponding current collectors.
The present invention describes carbon/carbon Electrical Double-Layer Capacitor (EDLC) of high specific capacity and energy density, which includes a negatively charged micro/mesoporous carbon composite electrode and a positively charged micro/mesoporous carbon composite electrode, separated from each other by a separator having porosity all through.
The invention describes also the structure of cylindrical-shape carbon/carbon EDLC of high specific capacity and energy density, which partially guarantees the efficient packing density and low internal resistance of the electrochemical system.
The invention describes in addition speciality of the cylindrical EDLC which enables without additional supporting elements to integrate individual elements of the EDLC into high-voltage EDLC battery.
The objective of the invention is to provide design of the cylindrical ultracapacitor of high power density having low internal resistance. Said objective has been achieved by integrating a first current terminal and end cap of the capacitor whereas the first current terminal comprising a stellate-like structure or star-like structure with feet or prongs or members extending radially from the centre of the current terminal and reinforcing ribs formed to one of the edges of the radially extending members. The current terminals are laser welded to the capacitor electrode along the bottom of the radially extending members. The capacitor comprises a housing having closed bottom with an opening through which protrudes out from the housing a terminal end of the second current terminal. Said design enables to have more compact and high power density ultracapacitor compared with the other ultracapacitors in prior art.
The embodiments of the present invention are described in the following detailed description with references to figures in which:
An electric double layer capacitor according to the present invention comprises a cylindrical housing 1 closed at one end, the other end is closed by an end cap or lid 2, which is integrated with the first current terminal 3 (
The end cap 2 for closing the capacitor housing has an opening/hole 9 for guiding out a terminal end of the first current terminal 3 protruding from said capacitor, whereas the end cap 2 and the terminal end of the first current terminal 3 are welded together along the perimeter of the opening 9 (
The terminal end of the second current terminal 4 is threaded, whereas the dimensions of the thread corresponds to the dimensions of the thread of the threaded hole 15 in the connecting sleeve 14 such that the individual electric double layer capacitors can be connected in series with a block of capacitors, i.e. the high-voltage battery is assembled (
The first current terminal 3 (
The bottom side of the star-like structure radially extending members 10 of the current terminal 3 is laser-spot welded respectively to the flattened positive or negative ends of the jelly-roll of wound carbon electrodes 7 placed into the cylindrical housing 1 during assembling the double-layer capacitor. The rectangular radially extending members 10 with reinforcing ribs 11 are formed and arranged radially into upper side of the star-like structure of the current terminals 3. From the trough hole 6 of the first current terminal 3 are extending channels 17 between the radially extending members 10 of the star-like structure of the first current terminal 3. These channels 17 are directing during the manufacturing process of the capacitor the electrolyte to the jelly-roll 7 when the current terminal 3 is welded to electrode.
The second current terminal 4 comprising similarly a star-like structure with rectangular extending members 20 protruding radially from the centre of current terminal 4 where to the upper side of the prongs 20 of the star-like structure are formed the reinforcing ribs 21 that are placed into contact with the bottom of the cylindrical housing 1. The bottom side of the star-like structure radially extending members 10 of the second current terminal 4 is laser-spot welded respectively to the flattened negative or positive ends of the jelly-roll of wound carbon electrodes 7 placed into the cylindrical housing 1 during assembling the double-layer capacitor.
In
The integrated current terminal 103 has a through hole 106 for filling for example double layer capacitor during the manufacturing process with the electrolyte. For distributing electrolyte evenly there are provided channels 117 in the bottom side of the current terminal, said channels are extending from the through hole 106 to contact point between the extending members 110 of the star-like structure 100.
These channels 117 are directing during the manufacturing process of the ultracapacitor the electrolyte to the jelly-roll when the current terminal is welded to electrode.
The bottom side of current terminal radially extending members 114 is welded to the flattened ends of the current collector foils bending over the plane of the cylindrical jelly-roll of wound electrodes. The laser welding or laser spot welding can be used for welding process.
The bottom side of the round base of the first and second current terminal have laser-spot welded respectively to positive and negative ends of the packed cylindrical carbon electrode 7 placed into the cylindrical housing 1 during assembling the double-layer capacitor. The reinforcing ribs 11, 21 are formed and arranged radially into upper side of the current terminals.
Advantages, which are provided by the “star-like current terminals” according to this invention, which is laser welded respectively to the flattened positive and negative ends of the current collector foils bending over the jelly-roll of packed carbon electrodes are following:
To isolate electrically the end cap 2 and packed carbon electrode 7 from the capacitor cylindrical housing 1 is used the seal 5 The seal 5 is ring with L-shaped cross-section where the shorter prong of the L-letter is supported to the step 12 in the outer edge of the end cap 2, and the longer prong of the L-letter is wrapped around cylindrically packed carbon electrode. The electrode is centered into housing and isolated from the housing in this way.
The electric double layer capacitor is prepared as follows: first of all, the second current terminal is placed into the cylindrical housing so that the reinforcement ribs in the upper side of the lamellar round base of the second current terminal are supported to the bottom of cylindrical housing and the terminal end of the second current terminal extends out from the housing. The terminal end of the second current terminal is welded on the outside to the bottom of the housing. The cylindrically packed carbon electrodes are placed into the housing and the cylindrical housing is closed with the end cap with seal so that the seal surrounds upper part of the carbon electrode (the electrode is isolated from the housing. Thereafter the upper edge of the cylindrical housing is rolled so that the capacitor is closed and sealed hermetically. The capacitor is filled through the hole 6 in the first current terminal with the electrolyte during the manufacturing process and thereafter the hole is closed with closing cap 16. The connecting sleeve 14 is welded to the terminal end of the first current terminal before or after filling the capacitor with electrolyte.
Example of the Manufacture of Glued Electrodes
For preparing a capacitor rechargeable positive electrode (anode) the 0.85 grams of titanium carbide (H.C. Starck) derived microporous synthetic primary carbon with irregular, non-graphite structure and 0.15 grams of silicon carbide (Sika-Tech) derived synthetic secondary carbon consisting of microporous graphene layers is mixed in 3 ml of ethanol. To the resulting mixture was added 8% of a polymeric binder (PTFE, Aldrich, 60% dispersion in water). After mixing, the resulting mixture was dried at 90° C. for approximately 1 hour at atmospheric pressure. Then the mixture was pressed into a 2-3 mm thick sheet and was formed using a rotary compactor gradually approximately 90 μm (micrometres) thick and approximately 50 mm wide carbon active layer film. Similarly was prepared a rechargeable negative electrode, wherein the primary carbon used was preferably with higher specific surface area. A carbon films were dried at 150° C. under vacuum. The dried carbon films were glued by using adhesion layer to the aluminium foil with 165 mm width (for example, C209, KDK Corporation, 20 mm). The used adhesion layer was previously prepared solution of 50% carbon black and 10% of PVDF (Aldrich) in NMP (N-methyl-2-pyrrolidone). Then the electrodes coated from one side with the active carbon layer where dried at 100° C., and the carbon films were glued to the opposite side of the aluminium strip of the opposite side of the carbon layer. Thereafter, the resulting double-side coated electrodes were dried at 130° C. for 48 h in vacuum.
The double sided electrodes with active carbon layer were cut to size so that the width of the carbon strip was 50 mm and the width of the foil protruding from the one edge was 60 mm.
To the working surface was placed 60 mm wide separator and a positively charged capacitor electrode was placed on separator so that the edges of the separator would exceed the active layer carbon film from each side equally. In the same way was placed to said electrode the second separator and onto top of that negatively charged electrode whose foil edge was on the opposite edge with previous electrode. To the one end of the electrode and separator tape was attached tube with 5 mm diameter and electrode and separator tape was wrapped around said tube. Said formed roll with external diameter 29 mm was fixed with tape and the 5 mm tube was removed. The protruding foil of the electrodes were formed flat and the terminal of the positive package was spot welded to the positive current terminal of the capacitor. Thereafter the cylindrical package was placed into capacitor housing and negative terminal of the package was spot welded to the negative current terminal of the capacitor. The first current terminal was pushed into housing and was sealed by corresponding seal and the housing was closed and rolled hermetically.
The electrical resistance of closed capacitor was checked with Ohm meter and gas-tightness by gas He approximately with 5 atm pressure (506,625 kPa). After control the capacitor was connected to the vacuum system (approximately 7 mm/Hg), and left at 120° C. for 72 hours.
After removing all air the capacitor was filled with the previously prepared solution of anhydrous electrolyte consisting of acetonitrile (Aldrich) and 30% triethylmethyl ammonium tetrafluoroborate (Stella Chemical).
The following table shows the examples of the nanoporous electrode pairs used in present invention, which obviously will not restrict use of the present invention having different configuration of the carbon.
According to the present invention, a layer of activated carbon is connected to both surfaces of the current terminal, wherein the connecting methods may be: pressure contact of a carbon film to the surface of the current collector; gluing a carbon film to surface of the collector; compacting a dry mixture or paste of carbon and the binder to the current collector. The current collectors may be any electro-chemically resistant material with a very good electrical conductivity—typically a thin metal foil, for instance Al-foil 5-100 mkm thickness, which in turn may be coated with a thin (e.g. thickness 1-2 mkm) ceramic or any other electrically conductive layer for improving the electrical contact between the active carbon and current collector. Alternatively, a method for improving electrical contact may be coating an activated carbon film with a thin layer of metal using a vacuum deposition method such as thermal or plasma vacuum deposition PVD method (Physical Vapour Deposition) or a metal spraying method.
Possible method for connecting current collectors and terminal are spot welding; TIG welding; laser welding; diffusion welding; Al sputtering.
Aprotic electrolyte may comprise an organic solvent and aprotic salt being donor for ion pairs. The electrolyte salts may be quaternary ammonium salts, quaternary phosphonium salts, and, for example, tetraethyl ammonium tetrafluoroborate; triethylmethylammonium tetrafluoroborate, etc.
The electrolyte salt of the cation may be (R1R2)4N+ or R1R2P+ where R1 and R2 are alkyl groups of up to —CH3 to —C5H11 or cyclic phenyl ring —C6H 5, and anion BF4−; PF6—; AsF6−; Ph4B−; CF3SO3— or others.
Solvents used is selected from the following solvents and their mixtures: acetonitrile, benzonitrile, sulfolane, propylene carbonate, ethylene carbonate, ethylmethylcarbonate, dimethyl carbonate, diethyl carbonate, methyl acetate, γ-butyrolactone, tetrahydrofuran, N, N-dimethylformamide, dimethyl sulfoxide, pyridine, sulfolane, dimethyl ketone, and the like. Electrolytes, ionic liquids can be used as an imidazole moiety, for example, EMIBF6, EMICF3SO3 et al. concentrated or with solvents.
Number | Date | Country | Kind |
---|---|---|---|
1609299.1 | May 2016 | GB | national |
Filing Document | Filing Date | Country | Kind |
---|---|---|---|
PCT/EP2017/062787 | 5/26/2017 | WO | 00 |
Number | Date | Country | |
---|---|---|---|
62341657 | May 2016 | US |