The present invention relates to a joint component manufacturing method for joining a first member and a second member by fitting of a shaft portion of the second member in a hole of the first member.
Typically, there has been a joint component manufacturing method for joining a first member and a second member by fitting of a shaft portion of the second member in a hole of the first member. For example, in a press-fit bonding structure disclosed in Patent Literature 1 below, a burr housing portion configured to house burrs generated upon press-fitting is formed in the vicinity of an end portion of a bonding interface at which a hole of a first member and a shaft portion of a second member are fitted to each other.
PATENT LITERATURE 1: JP-A-2005-14064
However, in the press-fit bonding structure described in Patent Literature I above, the burr housing portion is formed continuously to the bonding interface at which the hole of the first member and the shaft portion of the second member are fitted to each other. Thus, there are problems that bonding force between the first member and the second member is weakened and such bonding force is further decreased due to a clearance in the burr housing portion in a case where the amount of burrs entering the burr housing portion is small.
The present invention has been made for coping with the above-described problems. An object of the present invention is to provide the following joint component manufacturing method. In the manufacturing method, occurrence of burrs upon bonding between a first member having a hole and a second member having a shaft portion can be reduced while both members can be firmly bonded to each other.
In order to achieve the above-described object, an aspect of the present invention is a joint component manufacturing method for joining a first member and a second member by fitting of a shaft portion of the second member in a hole of the first member, the first member and the second member each including weak press-fit portions with a first weak press-fit interference at tip end portions first fitted to each other upon fitting between the hole and the shaft portion, and the first member or the second member including a strong press-fit portion protruding with respect to the weak press-fit portions and having a thicker first strong press-fit interference than the first weak press-fit interference on a far side of the weak press-fit portions. The method includes: a first weak press-fit step of press-fitting the weak press-fit portions of the first member and the second member to each other; and a first strong press-fit step of press-fitting one of the weak press-fit portions of the first member and the second member and the strong press-fit portion to each other in a state in which electric resistance heat is generated between the first member and the second member by applying a current.
Further, in order to achieve the above-described object, another aspect of the present invention is a joint component manufacturing method for joining a first member and a second member by fitting of a shaft portion of the second member in a hole of the first member, the first member and the second member each including, at tip end portions first fitted to each other upon fitting between the hole and the shaft portion, weak press-fit portions not contacting each other at the tip end portions and having a second weak press-fit interference with respect to each strong press-fit portion formed to protrude to a far side of each tip end portion and each strong press-fit portion having a thicker second strong press-fit interference than the second weak press-fit interference. The method includes: a second weak press-fit step of press-fitting each weak press-fit portion and each strong press-fit portion of the first member and the second member to each other; and a second strong press-fit step of press-fitting the strong press-fit portions of the first member and the second member to each other in a state in which electric resistance heat is generated between the first member and the second member by applying a current.
According to each aspect of the present invention configured as described above, in the joint component manufacturing method, the hole of the first member and the shaft portion of the second member are bonded to each other by press-fitting with the first strong press-fit interference and the second strong press-fit interference through press-fitting with the first weak press-fit interference and the second weak press-fit interference. In this case, the first weak press-fit interference and the second weak press-fit interference are, with respect to the first strong press-fit interference and the second strong press-fit interference, formed such that an overlapping thickness (i.e., the press-fit interference) between both members is decreased. Thus, according to the joint component manufacturing method of the present invention, occurrence of burrs upon bonding between the first member having the hole and the second member having the shaft portion can be reduced while close contact between both members without any clearances and firm bonding between both members can be realized.
According to other aspect of the present invention, in the joint component manufacturing method, the first weak press-fit interference and the second weak press-fit interference are formed to such an overlapping thickness that no burrs are generated between the first member and the second member fitted to each other.
According to the other aspect of the present invention configured as described above, in the joint component manufacturing method, the first weak press-fit interference and the second weak press-fit interference are formed to such a thickness that no burrs are generated between the first member and the second member fitted to each other. Thus, occurrence of burrs upon bonding between the first member having the hole and the second member having the shaft portion can be more effectively reduced. In this case, the first weak press-fit interference and the second weak press-fit interference are set for each of the materials, shapes, and press-fit conditions of the first member and the second member, and therefore, are obtained by experiment in advance. Note that a burr is one generated when part of the material forming the hole and/or the shaft portion is carved or extruded to the periphery of an opening of the hole upon fitting between the hole and the shaft portion in a press-fit stale,
According to other aspect of the present invention, in the joint component manufacturing method, a guide portion having an inclined surface or a curved surface is formed at at least one corner portion of the tip end portions first fitted to each other upon fitting between the hole and the shaft portion.
According to the other aspect of the present invention configured as described above, the guide portion having the inclined surface or the curved surface is formed at at least one corner portion of the tip end portions first fitted to each other upon fitting between the hole and the shaft portion. Thus, the shaft portion of the second member is smoothly guided to the hole of the first member, and is easily fitted in the hole. Thus, occurrence of burrs can be more effectively reduced.
According to other aspect of the present invention, in the joint component manufacturing method, the weak press-fit portion has a gradually-changing portion of which the shape gradually changes with respect to the strong press-fit portion.
According to the other aspect of the present invention configured as described above, in the joint component manufacturing method, the weak press-fit portion has the gradually-changing portion of which the shape gradually changes with respect to the strong press-fit portion. Thus, the shaft portion of the second member is smoothly guided to the hole of the first member, and is easily fitted in the hole. Thus, occurrence of buns can be more effectively reduced.
According to other aspect of the present invention, in the joint component manufacturing method, at least one of the first member and the second member is, at the first weak press-fit step and the second weak press-fit step, supported in a displaceable state in a direction perpendicular to a fitting direction.
According to the other aspect of the present invention configured as described above, in the joint component manufacturing method, at least one of the first member and the second member is. at the first weak press-fit step and the second weak press-fit step, supported in the displaceable state in the direction perpendicular to the fitting direction. Thus, even in a case where misalignment between the hole of the first member and the shaft portion of the second member has occurred, the first member and/or the second member are, at the first weak press-fit step and the second weak press-fit step, moved to perform fitting with the centers of both members being coincident with each other. With this configuration, according to the joint component manufacturing method of the present invention, the first member and the second member can be bonded to each other with the cores of the first member and the second member being coincident with each other even in a case where the cores are shifted from each other upon bonding between both members.
Hereinafter, a first embodiment of a joint component manufacturing method according to the present invention will be described with reference to the drawings.
First, the joint component 100 formed by the joint component manufacturing method according to the present invention will be briefly described. The joint component 100 mainly includes a first member 110 obtained in such a manner that a steel member is formed in a flat plate ring shape, and a second member 120 obtained in such a manner that a steel member is formed in a cylindrical shape. A though-hole-shaped hole 111 to which the second member 120 is bonded with the second member 120 being fitted in the hole 111 is formed at a center portion of a flat plate ring body of the first member 110. Moreover, a cylindrical shaft portion 121 bonded with the shaft portion 121 being fitted in the hole 111 of the first member 110 is formed on one end side (the lower side as viewed in the figure) of a cylindrical body of the second member 120. The first member 110 and the second member 120 are, at the hole 111 and the shaft portion 121, bonded to each other by electric resistance welding to integrally form the joint component 100.
The joint component 100 includes, for example, a component forming a power transmission device such as a clutch or a transmission in a self-propelled vehicle, the component including, for example, a pulley in a centrifugal clutch, an interlock sleeve in a manual transmission, or a manual plate in an automatic transmission.
First, a worker manufacturing the joint component 100 prepares, as a first step, each of the first member 110 and the second member 120 as materials of the joint component 100, as illustrated in
As illustrated in
More specifically, the first weak press-fit interference Lw1 is set to such a size that the amount of burrs generated when the shaft-side weak press-fit portion 122 of the shaft portion 121 is press-fitted in the hole-side weak press-fit portion 112 of the hole 111 is less than the amount of burrs generated when at least a later-described shaft-side strong press-fit portion 124 is press-fitted in the hole-side weak press-fit portion 112. The first weak press-fit interference Lw1 is set for each of the materials, shapes, and press-fit conditions of the first member 110 and the second member 120, and therefore, is experimentally obtained in advance.
In the present embodiment, the first weak press-fit interference Lw1 is set to such a size that no burrs due to radial compression and deformation of at least one of the hole-side weak press-fit portion 112 or the shaft-side weak press-fit portion 122 are generated when the shaft-side weak press-fit portion 122 is press-fitted in the hole-side weak press-fit portion 112. Note that according to experiment by the present inventor et al., the first weak press-fit interference Lw1 preferably has a diameter of greater than 0 mm and equal to or less than 0.1 mm in a case where the diameter of each of the hole 111 and the shaft portion 121 formed of the steel members is within a range of 10 mm to 100 mm in terms of diameter.
The first weak press-fit interference Lw1 is defined by the minus tolerance of the hole ill. with respect to a reference inner diameter dimension of the hole-side weak press-fit portion 112 and the plus tolerance of the shaft portion 121 with respect to a reference outer diameter dimension of the shaft-side weak press-fit portion 122. That is, the first weak press-fit interference Lw1 is defined by interference fit between the hole 111 and the shaft portion 121. The formation length Lwh of the shaft-side weak press-fit portion 122 on a side provided with the shaft-side strong press-fit portion 124 among the hole-side weak press-fit portion 112 and the shaft-side weak press-fit portion 122 is set in a relationship with the formation length Lsh of the shaft-side strong press-fit portion 124. That is, the formation length Lwh of the shaft-side weak press-fit portion 122 is a portion for reducing the burr generation amount due to fitting between the hole 111 and the shaft portion 121. On the other hand, the formation length Lsh of the shaft-side strong press-fit portion 124 is a portion defining bonding force between the hole 111 and the shaft portion 121.
Thus, the formation length Lwh of the shaft-side weak press-fit portion 122 is set according to the bonding force between the hole 111 and the shaft portion 121, the bonding force being necessary for the joint component 100. According to the experiment by the present inventor et al., the formation length Lwh of the shaft-side weak press-fit portion 122 may be preferably equal to or less than the half of the formation length Lsh of the shaft-side strong press-fit portion 124, and more preferably equal to or less than ⅓ of the formation length Lsh of the shaft-side strong press-fit portion 124. In the present embodiment, the formation length Lwh of the shaft-side weak press-fit portion 122 is formed equal to or less than ⅓ of the formation length Lsh of the shaft-side strong press-fit portion 124.
The lower limit of the formation length Lwh of the shaft-side weak press-fit portion 122 is set to such a length that the hole-side weak press-fit portion 112 and the shaft-side weak press-fit portion 122 evenly contact each other in a cylindrical surface shape and smooth electrical conduction between both portions is allowed. According to the experiment by the present inventor et al., the lower limit of the formation length Lwh of the shaft-side weak press-fit portion 122 may be equal to or greater than ⅕ of the thickness ST of a bonding portion between the hole 111 and the shaft portion 121, and more preferably equal to or less than ¼ of such a bonding portion.
On the other hand, the formation length Lwh of the hole-side weak press-fit portion 112 not provided with the shaft-side strong press-fit portion 124 in the hole 111 is formed with a thickness of equal to or greater than the thickness ST in bonding between the hole 111 and the shaft portion 121. In the present embodiment, the thickness ST in bonding between the hole 111 and the shaft portion 121 is the same as the thickness of the first member 110, and therefore, the formation length Lwh of the hole-side weak press-fit portion 112 is formed with the same length as the thickness of the first member 110, i.e., is formed across the entirety of the hole 111.
A gradually-changing portion 123 is formed at a far-side back end portion (the lower side as viewed in the figure) of the shaft-side weak press-fit portion 122. The gradually-changing portion 123 is a portion of which the shape gradually changes between the shaft-side weak press-fit portion 122 and the shaft-side strong press-fit portion 124. In the present embodiment, the gradually-changing portion 123 is formed such that the shaft-side weak press-fit portion 122 and the shaft-side strong press-fit portion 124 are connected by an arc-shaped curved surface. The shaft-side strong press-fit portion 124 is formed on a far side (the lower side as viewed in the figure) of the gradually-changing portion 123.
The shaft-side strong press-tit portion 124 is a portion formed with the first strong press-fit interference Ls1 as a predetermined press-fit interference from the hole-side weak press-fit portion 112. The first strong press-fit interference Ls1 is the thickness of an overlapping portion upon fitting between the shaft-side strong press-fit portion 124 and the hole-side weak press-fit portion 112. The first strong press-fit interference Ls1 is formed greater (thicker) than the first weak press-fit interference Lw1. More specifically, the first strong press-fit interference Ls1 is set such that the minimum necessary press-fit interference for electric resistance welding is ensured upon electric resistance welding between the hole 111 and the shaft portion 121.
The first strong press-fit interference Ls1 is set for each of the materials, shapes, and press-fit conditions of the first member 110 and the second member 120, and therefore, is experimentally obtained in advance. According to the experiment by the present inventor et al., the first strong press-fit interference Ls1 preferably has a diameter of 0.5±0.05 in a case where the diameter of each of the hole 111 and the shaft portion 121 formed of the steel members is within a range of 10 mm to 100 mm in terms of diameter.
The first strong press-fit interference Ls1 is defined by the minus tolerance of the hole 111 with respect to the reference inner diameter dimension of the hole-side weak press-fit portion 112 and the plus tolerance of the shaft portion 121 with respect to the reference outer diameter dimension of the shaft-side strong press-fit portion 124. That is, the first strong press-fit interference Ls1 is defined by interference fit between the hole 111 and the shaft portion 121. Moreover, the formation length Lsh of the shaft-side strong press-fit portion 124 is set according to the bonding force between the hole 111 and the shaft portion 121, the bonding force being necessary for the joint component 100.
Next, the worker sets, as a second step, the first member 110 and the second member 120 on a processing machine 200 configured to perform electric resistance welding. The processing machine 200 described herein is a welding device configured to generate electric resistance heat by applying a current between two members fitted to each other to press-fit these two members, thereby generating plastic flow of an interface between these members to perform solid phase bonding of the members. As illustrated in
The first die 201 and the second die 202 are components configured to press the hole 111 of the first member 110 and the shaft portion 121 of the second member 120 in a current application state to press-fit these portions. Each of the first die 201 and the second die 202 is made of a material (e.g., chromium copper) exhibiting electric conductivity. Of these components, the first die 201 is a movable die configured to press the first member 110 arranged on the second member 120 toward the second member 120, and is formed in a cylindrical shape.
On the other hand, the second die 202 is a fixed die configured to support the second member 120, and is formed in a flat plate shape. In this case, a recessed portion 202a recessed in a ring shape is formed at a portion of a surface of the second die 202 corresponding to an outer peripheral portion of the shaft portion 121 of the second member 120. That is, the first die 201 and the second die 202 press both of the first member 110 and the second member 120 in a state in which each of the first member 110 and the second member 120 is not restricted in a direction perpendicular to a pressing direction, i.e., a radial direction of each of the first member 110 and the second member 120, and is displaceable in such a direction.
At the second step, the worker arranges the second member 120 on the second die 202. Thereafter, the worker arranges the first member 110 on the shaft portion 121 of the second member 120. In this case, for the first weak press-fit interference Lw1, the inner diameter of the hole 111 is smaller than the outer diameter of the shaft portion 121 of the second member 120. Thus, the first member 110 is placed on the shaft portion 121 of the second member 120.
Next, the worker press-fits, as a third step, the hole-side weak press-fit portion 112 of the first member 110 and the shaft-side weak press-fit portion 122 of the second member 120 to each other. Specifically, the worker operates the processing machine 200 to move (move downward in a direction indicated by a dashed arrow in each of
Moreover, at the third step, the first die 201 and the second die 202 each press the first member 110 and the second member 120 with these members being displaceable in the radial direction. Thus, in a case where the positions of the center axes of the hole-side weak press-fit portion 112 and the shaft-side weak press-fit portion 122 are shifted from each other upon fitting therebetween, at least one of the first member 110 or the second member 120 is displaced in the radial direction such that the positions of the center axes of these portions are coincident with each other. In this manner, the first member 110 and the second member 120 are fitted to each other with the center axes being coincident with each other. The third step corresponds to a first weak press-fit step according to the present invention. That is, each of the hole-side weak press-fit portion 112 and the shaft-side weak press-fit portion 122 corresponds to a weak press-fit portion according to the present invention.
Next, the worker press-fits, as a fourth step, the hole-side weak press-fit portion 112 of the first member 110 and the shaft-side strong press-fit portion 124 of the second member 120 to each other. Specifically, the worker operates the processing machine 200 to move (move downward in a direction indicated by a dashed arrow in
In this case, a bonding portion SP between the hole ill and the shaft portion is formed inclined from the shaft-side weak press-fit portion 122 toward the shaft-side strong press-fit portion 124. Further, a burr B clue to solid phase bonding between the hole-side weak press-fit portion 112 and the shaft-side strong press-fit portion 124 might be generated at a tip end portion of the bonding portion SP. That is, the burr B is or is not generated according to the formation length Lwh of the shaft-side weak press-fit portion 122.
At the bonding portion SP, a press-fit portion between the shaft-side weak press-fit portion 122 and part (the upper side as viewed in
By the fourth step, the first member 110 and the second member 120 are bonded to each other to form the joint component 100. The fourth step corresponds to a first strong press step according to the present invention. That is, the shaft-side strong press-fit portion 124 corresponds to a strong press-fit portion according to the present invention.
Note that the bonding portion SP does not clearly appear, and
Next, the worker takes, as a fifth step, the joint component 100 out of the processing machine 200. Specifically, the worker confirms, after the fourth step, that the first die 201 has been separated (has moved upward as viewed in the figure) from the second die 202 and the processing machine 200 has returned to an original position, and then, takes the joint component 100 out of the second die 202. Thereafter, the worker performs necessary processing for the joint component 100, thereby bringing the joint component 100 to completion. This post-processing for the joint component 100 does not directly relate to the present invention, and therefore, description thereof will be omitted.
As seen from operation description above, in the method for manufacturing the joint component 100, the hole 111 of the first member 110 and the shaft portion 121 of the second member 120 are, according to the first embodiment, bonded to each other by press-fitting with the first strong press-fit interference Ls1 through press-fitting with the first weak press-fit interference Lw1. In the this case, the first weak press-fit interference Lw1 is, with respect to the first strong press-fit interference Ls1, formed such that an overlapping thickness (i.e., the press-fit interference) between both members is decreased. Thus, according to the method for manufacturing the joint component 100 according to the present invention, occurrence of the burrs B in bonding between the first member 110 having the hole 111 and the second member 120 having the shaft portion 121 is reduced while close contact between both members without any clearances and firm bonding between both members can be realized.
Further, implementation of the present invention is not limited to the above-described embodiment, and various changes can be made without departing from the object of the present invention.
For example, in the above-described embodiment, the shaft-side strong press-fit portion 124 as the strong press-fit portion according to the present invention is provided at the shaft portion 121 of the second member 120. However, the strong press-fit portion may be formed at either one of the first member 110 or the second member 120. Thus, the strong press-fit portion can be formed as a hole-side strong press-fit portion at the hole 111 of the first member 110 on a far side (the upper side as viewed in
Next, a second embodiment of a joint component manufacturing method according to the present invention will be described with reference to
A joint component 300 configured in a manner similar to that of the joint component 100 mainly includes a first member 310 and a second member 320. In the first member 310, each of a hole-side weak press-fit portion 312, a gradually-changing portion 313, and a hole-side strong press-fit portion 314 is formed at a through-hole-shaped hole 311. Moreover, the second member 320 is configured such that each of a shaft-side weak press-fit portion 322, a gradually-changing portion 323, and a shaft-side strong press-fit portion 324 is formed at a cylindrical shaft portion 321.
As illustrated in
More specifically, as in the first weak press-fit interference Lw1, the second weak press-fit interference Lw2 is set to such a size that the amount of burrs generated when the shaft-side strong press-fit portion 324 is press-fitted in the hole-side weak press-fit portion 312 and when the shaft-side weak press-fit portion 322 is press-fitted in the hole-side strong press-fit portion 314 is less than the amount of burrs generated when at least the later-described shaft-side strong press-fit portion 324 is press-fitted in the hole-side strong press-fit portion 314. The second weak press-fit interference Lw2 is set for each of the materials, shapes, and press-fit conditions of the first member 310 and the second member 320, and therefore, is experimentally obtained in advance. Moreover, the same second weak press-fit interference Lw2 forming the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is applied.
In the present embodiment, the second weak press-fit interference Lw2 is, as in the first weak press-fit interference Lw1, set to such a size that no burrs are generated due to compression deformation of each portion in a radial direction when the shaft-side strong press-fit portion 324 is press-fitted in the hole-side weak press-fit portion 312 and when the shaft-side weak press-fit portion 322 is press-fitted in the hole-side strong press-fit portion 314. Note that according to experiment by the present inventor et al., the second weak press-fit interference Lw2 preferably has a diameter of greater than 0 mm and equal to or less than 0.1 mm in a case where the diameter of each of the hole 311 and the shaft portion 321 formed of steel members is within a range of 1.0 mm to 100 mm in terms of diameter.
As in the first weak press-fit interference Lw1, the second weak press-fit interference Lw2 is defined by interference fitting between the hole 311 and the shaft portion 321. Moreover, as in the formation length Lwh of the shaft-side weak press-fit portion 122, the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is set in a relationship with the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324. That is, the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is a portion for reducing the amount of burrs generated due to fitting between the hole 311 and the shaft portion 321. On the other hand, the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 is a portion defining bonding force between the hole 311 and the shaft portion 321.
Thus, the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is set according to the bonding force between the hole 311 and the shaft portion 321, the bonding force being necessary for the joint component 300. According to the experiment by the present inventor et al., the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 may be preferably equal to or less than the half of the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324, and more preferably equal to or less than ⅓ of the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324, in the present embodiment, the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is formed equal to or less than ⅓ of the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324.
The lower limit of the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 is set to such a length that the hole-side weak press-fit portion 312 and the shaft-side strong press-fit portion 324 evenly contact each other in a cylindrical surface shape, the hole-side strong press-fit portion 314 and the shaft-side weak press-fit portion 322 evenly contact each other in a cylindrical surface shape, and smooth electrical conduction between both portions is allowed. According to the experiment by the present inventor et al., the lower limit of the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 may be equal to or greater than ⅕ of the thickness ST of a bonding portion between the hole 311 and the shaft portion 321, and more preferably equal to or greater than ¼ of such a bonding portion.
The hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 are portions formed with the second strong press-fit interference Ls2 as a predetermined press-fit interference between these portions. The second strong press-fit interference Ls2 is the thickness of an overlapping portion upon fitting between the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324. The second strong press-fit interference Ls2 is formed greater (thicker) than the second weak press-fit interference Lw2. More specifically, the second strong press-fit interference Ls2 is set such that the minimum necessary press-fit interference for electric resistance welding is ensured upon electric resistance welding between the hole 311 and the shaft portion 321.
The second strong press-fit interference Ls2 is set for each of the materials, shapes, and press-fit conditions of the first member 310 and the second member 320, and therefore, is experimentally obtained in advance. According to the experiment by the present inventor et al., the second strong press-fit interference Ls2 preferably has a diameter of 0.5±0.05 in a case where the diameter of each of the hole 311 and the shaft portion 321 formed of the steel members is within a range of 10 mm to 100 mm in terms of diameter.
The second strong press-fit interference Ls2 is defined by interference fitting between the hole 311 and the shaft portion 321. Moreover, the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 is set according to the bonding force between the hole 311 and the shaft portion 321, the bonding force being necessary for the joint component 300. Moreover, the same second strong press-fit interference Ls2 forming the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 is applied.
As in the first embodiment, the first member 310 and the second member 320 configured as described above are, as illustrated in
Then, a worker press-fits, as a third step, the hole-side weak press-fit portion 312 of the first member 310 and the shaft-side strong press-fit portion 324 of the second member 320 to each other. At the same time, the worker press-fits the hole-side strong press-fit portion 314 of the first member 310 and the shaft-side weak press-fit portion 322 of the second member 320 to each other. Specifically, the worker operates a processing machine 200 to move (move downward in a direction indicated by a dashed arrow in
At the third step, the first die 201 and the second die 202 each press the first member 310 and the second member 320 with these members being displaceable in the radial direction. Thus, in a case where the positions of the center axes of the hole-side weak press-fit portion 312 and the shaft-side strong press-fit portion 324 are shifted from each other upon fitting therebetween and the positions of the center axes of the shaft-side weak press-fit portion 322 and the hole-side strong press-fit portion 314 are shifted from each other upon fitting therebetween, at least one of the first member 310 or the second member 320 is displaced in the radial direction such that the positions of the center axes of these members are coincident with each other. In this manner, the first member 310 and the second member 320 are fitted to each other with the center axes being coincident with each other. The third step corresponds to a second weak press-fit step according to the present invention. That is, each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 corresponds to a weak press-fit portion according to the present invention. Each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 corresponds to a strong press-fit portion according to the present invention.
Next, the worker press-fits, as a fourth step, the hole-side strong press-fit portion 314 of the first member 310 and the shaft-side strong press-fit portion 324 of the second member 320 to each other. Specifically, the worker operates the processing machine 200 to move (move downward in a direction indicated by a dashed arrow in
In this case, burrs B due to solid phase bonding between the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 might be generated at both end portions of a bonding portion SP between the hole 311 and the shaft portion 321. That is, the burrs B are or are not generated according to the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322.
At the bonding portion SP, a press-fit portion between the hole-side weak press-fit portion 312 and the shaft-side strong press-fit portion 324 and a press-fit portion between the shaft-side weak press-fit portion 322 and the hole-side strong press-fit portion 314 are each bonding portions formed by press-fit bonding and/or solid phase bonding. A press-fit portion between the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 is a bonding portion by solid phase bonding. In this case, the press-fit portion between the hole-side weak press-fit portion 312 and the shaft-side strong press-fit portion 324 and the press-fit portion between the shaft-side weak press-fit portion 322 and the hole-side strong press-fit portion 314 includes, according to the materials, shapes, press-fit conditions, and current application conditions of the first member 310 and the second member 320, the case of bonding only by press-fitting, the case of bonding only by solid phase bonding, and the case of bonding by a combination of press-fit bonding and solid phase bonding.
Thus, according to the bonding component manufacturing method of the present invention, the formation length Lwh of each of the hole-side weak press-fit portion 312 and the shaft-side weak press-fit portion 322 and the formation length Lsh of each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 are adjusted as necessary so that the amount of generated burrs B and bonding strength between both members can be adjusted.
By the fourth step, the first member 310 and the second member 320 are bonded to each other to form the joint component 300. The fourth step corresponds to a second strong press-fit step according to the present invention. That is, each of the hole-side strong press-fit portion 314 and the shaft-side strong press-fit portion 324 corresponds to a strong press-fit portion according to the present invention.
Note that the bonding portion SP does not clearly appear, and
As seen from operation description above, in the joint component manufacturing method, the hole 311 of the first member 310 and the shaft portion 321 of the second member 320 are, according to the second embodiment, bonded to each other by press-fitting with the second strong press-fit interference Ls2 through press-fitting with the second weak press-fit interference Lw2. In the this case, the second weak press-fit interference Lw2 is, with respect to the second strong press-fit interference Ls2, formed such that an overlapping thickness (i.e., the press-fit interference) between both members is decreased. Thus, according to the joint component manufacturing method according to the present invention, occurrence of burrs in bonding between the first member 310 having the hole 311 and the second member 320 having the shaft portion 321 is reduced while close contact between both members without any clearances and firm bonding between both members can be realized.
Further, implementation of the present invention is not limited to each of the above-described embodiments, and various changes can be made without departing from the object of the present invention. Note that the same reference numerals are used to represent the same components as those of each of the above-described embodiments in the figures referred in description of variations below, and description thereof will be omitted as necessary.
For example, in each of the above-described embodiments, a corner portion of a tip end portion (an opening) on an insertion side of the shaft portion 121, 321 at the hole 111, 311 of the first member 110, 310 and a corner portion of a tip end portion on an insertion side of the hole 111, 311 at the shaft portion 121, 321 of the second member 120, 320 are formed at right angle. However, a guide portion 400 having an inclined surface or a curved surface can be provided at at least one of the corner portion of the tip end portion (the opening) of the hole 111, 311 or the corner portion of the tip end portion of the shaft portion 121, 321. For example, as illustrated in
Alternatively, the guide portion 400 can be, for example, provided in a curved shape at a corner portion of a tip end portion of the hole 111 on a side to be first fitted, as illustrated in
In other words, this means that the first weak press-fit interference Lw1 and the second weak press-fit interference Lw2 can be increased. According to the experiment by the present inventor et al., it has been confirmed that the guide portion 400 is provided at the corner portion of the tip end portion (the opening) of the hole 111 and occurrence of buns can be accordingly avoided even in a case where the first weak press-fit interference Lw1 and the second weak press-fit interference Lw2 have a diameter of greater than 0 mm and equal to or less than 0.2 mm when the diameter of each of the hole 111 and the shaft portion 121 formed of the steel members is within a range of 10 mm to 100 mm in terms of diameter.
Moreover, in each of the above-described embodiments, the gradually-changing portions 123, 313, 323 are provided at the first member 310 and the second member 120, 320. However, the first member 310 and the second member 120, 320 can be configured such that the gradually-changing portions 123, 313, 323 are omitted. In this case, at the first member 310 and the second member 120, 320, the hole-side weak press-fit portion 312 and the hole-side strong press-fit portion 314 are in a shape of which inner or outer diameter promptly changes in a stepwise manner, and the shaft-side weak press-fit portion 122, 322 and the shaft-side strong press-fit portion 124, 324 are in a shape of which inner or outer diameter promptly changes in a stepwise manner.
Further, in each of the above-described embodiments, the first member 110, 310 and the second member 120, 320 are made of the same material. However, the first member 110. 310 and the second member 120, 320 can be made of different materials. In this case, at the first member 110, 310 and the second member 120, 320, a member (e.g., a shape having a relatively-small thickness) more-deformable shape at the first weak press-fit step and the second weak press-fit step is made of a material having lower hardness than that of a member (e.g., a shape having a relatively-great thickness) in a less-deformable shape. Thus, occurrence of the burrs B at the first weak press-fit step and the second weak press-fit step can be more effectively reduced.
In addition, in each of the above-described embodiments, the first die 201 and the second die 202 each press or support the first member 110, 310 and the second member 120, 320 in a deformable state in the direction perpendicular to the fitting direction. However, the first die 201 and the second die 202 can also each press or support the first member 110, 310 and the second member 120, 320 in a state in which displacement in the direction perpendicular to the fitting direction is restricted, i.e., a state in which the first member 110, 310 and the second member 120, 320 are held.
Moreover, in each of the above-described embodiments, the processing machine 200 is configured such that the first die 201 moves toward or away from the second die 202. However, the processing machine 200 can be configured such that the second die 202 moves toward or away from the first die 201. Alternatively, the processing machine 200 can be configured such that the tops and bottoms of the first die 201 and the second die 202 are inverted. That is, in the joint component manufacturing method, the first member 110. 310 may be displaced with respect to the second member 120, 320, or the second member 120, 320 may be displaced with respect to the first member 110, 310. Displacement of both members is relative displacement.
Number | Date | Country | Kind |
---|---|---|---|
2016-204275 | Oct 2016 | JP | national |
Filing Document | Filing Date | Country | Kind |
---|---|---|---|
PCT/JP2016/081076 | 10/20/2016 | WO | 00 |