The invention relates to laminated glazings consisting of a thick transparent polymer material sheet and a thin mineral glass sheet, which are bonded to one another by an adhesive interlayer.
The specific problem posed by this type of structure is that of the differential thermal expansion between the polymer material and the mineral glass at the temperatures for assembling the laminates, referred to as a bimaterial strip effect. The polymer material sheet is bonded to the glass sheet by means of a thermoplastic adhesive. The bonding requires heating from ambient temperature to 100-120° C. depending on the nature of the polymer material, and preferably to a temperature slightly above 80° C., then cooling to ambient temperature. During cooling, the polymer material shrinks much more than the thin glass which then has a tendency to deform by forming ripples: this is also referred to as hillocking. The optical quality of the laminate is of course seriously affected thereby.
The inventors have realised that the choice of the nature and of the thickness of the adhesive interlayer made it possible, in very rare cases, to eliminate hillocking.
This objective was therefore able to be achieved by the invention, one subject of which is consequently a glazing essentially consisting of a transparent polymer material sheet having a thickness of from 5 to 25 mm and a glass sheet having a thickness of between 0.5 and 1.5 mm, which are bonded to one another by an adhesive interlayer, the hardness of which at a temperature at least equal to −5° C. is at most equal to 70 Shore A and the thickness of which is a decreasing function of the thickness of the glass sheet, an adhesive interlayer thickness of 2.5 mm being sufficient for a glass sheet thickness of 0.55 mm and an adhesive interlayer thickness of 1.25 mm being sufficient for a glass sheet thickness of 1.25 mm.
Within the meaning of the invention, glass is understood to mean any type of mineral glass such as soda-lime float glass which is optionally chemically strengthened, aluminosilicate glass which is optionally chemically strengthened, with or without alkali metals, borosilicate glass, aluminoborosilicate glass, etc.
Owing to the low hardness level and the considerable thickness of the adhesive layer according to the invention, a perfectly even, ripple-free surface of glass sheets as thin as 0.5 mm thick, laminated with the thick sheet of polymer material, is benefited from.
Without difficulty, it is also possible to obtain the customary qualities required for glazings in demanding applications such as aeronautics, in particular resistance to ambient usage temperatures as low as −40° C., bird strike resistance, indentation—gravel impact resistance, scratch resistance, etc.
The threshold of −5° C. for determining the hardness corresponds substantially to the minimum temperature reached by the adhesive interlayer in the presence of glazing with a heating layer.
According to preferred features of the glazing of the invention:
One subject of the invention is moreover the application of a glazing as described above for a terrestrial, airborne or water-borne transport vehicle, the surface of which in contact with the external atmosphere consists of one said glass sheet. This glass sheet offers an excellent mechanical resistance, with respect to scratches and indentations, and protects the surface of the underlying transparent polymer material. It guarantees the preservation of the original visual appearance of the surface of the glazing, which is essentially free of marks, and the maintaining of excellent optical and transparency quality.
The invention will be better understood in light of the following example.
A 9 mm thick sheet of poly(methyl methacrylate) is bonded to a 0.55 mm or 1.25 mm thick sheet of soda-lime-silica float glass chemically strengthened by an adhesive interlayer having a thickness of 1.25 mm or 2.5 mm consisting of polyvinyl butyral which is compatible with the PMMA, sold by Saflex under the registered trademark Saflex® PVB DB, or of thermoplastic polyurethane sold by Huntsman under the registered trademark Krystalflex® PE 499.
At 20° C., the hardness of Saflex® PVB DB is 95 Shore A and that of the Krystalflex® PE 499 TPU is 65 Shore A.
Six laminated glazings are assembled, having the features recorded in the table below.
These six laminates are subjected to the polarized light test (plane polariscope) which makes it possible to visualize the stresses in the laminate.
This test consists in exposing the sample to a source of polarized light and in observing the sample through a polarized filter.
The stress levels in the material are shown by the observation of color fringes known as isochromatics.
A zero stress level gives a black color; when the stress levels increase, the cold colors (blue, green) decrease in order to give way to hot colors (yellow, red).
An absence of stresses is only observed for the laminated glazings 4 and 6. It guarantees that the bimaterial strip effect described above does not occur, and that rippling of the thin glass sheets should not be expected for the laminated glazings 4 and 6. This is in accordance furthermore with direct visual observation through these glazings or using a shadow technique: specifically, no rippling is seen on the laminated glazings 4 and 6, unlike the other laminated glazings.