Leather impregnated with temperature stabilizing material and method for producing such leather

Abstract
The present invention is directed towards a tanned leather product that is impregnated with a plurality of microspheres containing a temperature stabilizing material. The present invention is also directed to a tanning process for embedding the microspheres into the leather. The thermal stabilizing material is a phase change material that allows the leather to have enhanced thermal properties when exposed to heat or cold.
Description




TECHNICAL FIELD




The present invention relates generally to leather and leather products, and more particularly to leather impregnated with microspheres containing a temperature stabilizing material, and a method for tanning the microspheres into leather.




BACKGROUND OF THE INVENTION




Tanning is a very old art, which is a treatment for preventing the decomposition of raw hides or skins. The tanned raw hides, typically referred to as leather, are also flexible and very strong. Originally, tanning was accomplished by using vegetable tanning agents such as bark, leaf, or bean extracts. Bark extracts used include for example those that can be obtained from oak, hemlock or avaram trees. Leaf extracts used include those that can be obtained from for example sumac. Bean extracts can be obtained for example from the acacia tree.




Mineral tanning agents or tannins have gradually replaced vegetable tanning agents, because mineral tanning agents produce stronger and more flexible leathers from the raw skins. Of the mineral tannages, the most prominent used today is chromium sulfate. Zirconium and aluminum are other minerals widely used in tanning. Other natural tannages include aldehyde, which is toxic because it uses formaldehyde, and oil tannage. Oil tannage is primarily used for “chamois” leather. Syntans or synthetic organic tanning agents are also used. Of all these tannages, it is widely believed that “chrome” tannage produces the strongest leather.




For many years various attempts have been made to improve the function and appearance of leathers by changing the methods of tanning and by putting various additives into the tanning mixture during processing. When leather is used for various garments, such as for shoes and gloves, it is desirable that the leather have additional properties that would improve the comfort to the wearer and durability of the leather. For example, leathers have been stain-proofed and waterproofed using various additives. However, there remains a need for improved leather and improved processes for treating leather that provides a thermally enhanced leather, while maintaining the softness, stretchability, resilience, and appearance of the leather.




SUMMARY OF THE INVENTION




One object of the present invention is to provide an improved leather impregnated with a temperature stabilizing material, such as microspheres containing a phase change material.




Yet a further object of the invention is to provide an improved process for tanning leather for use in garments with microencapsulated phase change material, which provides improved thermal properties to the leather.




The invention is generally directed to a tanned leather including an internal fiber matrix and a plurality of microspheres containing a temperature stabilizing material. The microspheres are embedded within the fiber matrix in a sufficient amount that the microspheres enhance the thermal stability of the leather when subject to heat or cold. The present invention is also directed to leather products formed of such leather, such as garments, shoes, and gloves. This allows such leather products to thermally regulate the temperature of the user.




The present invention is also directed to a method of impregnating a material having an internal fiber matrix. The method comprises the steps of placing the material in a container, adding a tanning agent to the container, combining a plurality of microspheres containing a temperature stabilizing material with a liquid to form a suspension, adding the suspension to the container, and agitating the contents of the container until microspheres are embedded within the fiber matrix. A sufficient amount of the microspheres are embedded so that, the microspheres enhance the thermal stability of the material when subject to heat or cold. In the method, the material to be treated, can be either raw skins or tanned leather.











BRIEF DESCRIPTION OF THE DRAWINGS





FIG. 1

is a flow chart diagram of a re-tanning process for embedding a temperature stabilizing material into an internal fiber matrix, in accordance with one embodiment of the invention;





FIG. 2

is a perspective view of a rotating drum for embedding the temperature stabilizing material into the matrix, in accordance with the invention;





FIG. 3

is a flow chart diagram of a tanning process for embedding the temperature stabilizing material into the matrix, in accordance with an alternative embodiment of the invention;





FIG. 4

is a perspective view of a golf shoe formed of the leather of the present invention; and





FIG. 5

is a front view of a golf glove formed of the leather of the present invention.











DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS




Leather tanning is an ancient art that has been practiced on a wide variety of materials. The process described and claimed herein can be applied to many raw materials, for example, including but not limited to sheep skin, goat skin, cowhide, deer skin and calf skin. The raw material selected depends upon the application for the final leather produced.




However, all of the raw material includes an internal fiber matrix, which is the dermis skin layer. The dermis consists of bundles of connective fibers which form a three-dimensional “mesh” of connective tissue. The fibers are made of protein.




In the first embodiment of the method of the present invention, as shown in

FIG. 1

, in step


201


the raw material is first brought to a fully chrome-tanned state, which imparts permanency to the fiber structure. A typical chrome tanning process described in the Leather Technician's Handbook by J. H. Sharphouse, B.S.c Leather Producer's Association, Kings Park Road, Moulton Park, Northampton, U.K. includes a series of fourteen separate steps, as discussed below.




1. First the skins are soaked in drums running at four revolutions per minute with 300% water at 27° Celsius and adjusted to a pH of 9.0 with 0.1% non-ionic surfactant. The skins are drummed intermittently for a period of six to 12 hours.




2. The skins are then drained.




3. The flesh sides of the skins are painted with 15% sodium hydrogen sulphide (33% strength), 50% hydrated lime and 35% water. The skins are allowed to pile overnight and then the wool is removed.




4. Next, 600% water and 12% lime are placed in a vat with agitating paddles run five minutes every four hours for 24 hours. Then ½% sodium sulphide is added to the vat and the agitating is continued for an additional 12 hours.




5. Next, the flesh is removed from the back side of the skin with a rotary fleshing machine.




6. Next, the skin is washed in soft, running water in a paddle vat for 30 minutes.




7. The skins are delimed in paddle vats containing 500% water at 37° Celsius with 1.5% ammonium chloride where the paddles are run for 60 minutes or until the skins re free of lime.




8. The bating process includes the addition of 1% bacterial bate with the addles run for two to three hours.




9. Next the skins are pickled in a drum with the pickling liquor being formed of 200% water at 20° Celsius, 20% salt and 2% sulfuric acid. The drum is run for 60 minutes, with the final pickle liquor strength being a 0.5% solution of sulfuric acid. The drum is then drained and the skins are stored for aging for several days.




10. The Chrome tanning solution is put in the drum. The tanning solution includes 100% water, 5% salt, 1% chromic oxide (as 10% of chrome liquor of 11% chromic oxide and 33% basicity, SO


2


reduced) and then 1% chromic oxide (as 10% of the above chrome liquor). The skins are then drummed for from two to six hours in this mixture until penetrated.




11. The skins are then basified. To complete the tannage ½-1% sodium bicarbonate should be added carefully over four hours and then a shrinkage temperature test should be taken. At the completion of tannage, the pH should be approximately 4.4 and the shrinkage temperature 98° Celsius.




12. The skins are then piled and drained for 24 hours.




13. Then the skins are neutralized thoroughly in the drum with 150% water and 1½% ammonium bicarbonate. The drum is run for 60 minutes to give a pH throughout the skin of 5.5-6.0.




14. Finally, the skins are washed well, at which point the leather is fully chrome tanned and ready for the re-tanning by the impregnation process of the present invention.




The chrome tanning process described above is well known in the art. It is merely provided as a representative description of the primary tanning process performed on the raw skins prior to the re-tanning process for impregnation of the thermal stabilizing material of the present invention. Other chrome tanning processes or even other basic mineral or vegetable tanning processes can be utilized as the preliminary tanning preparatory to the use of the impregnation process. Chromium sulfate, zirconium and aluminum mineral primary tannages may also be utilized with the present invention.




The re-tanning impregnation will now be discussed, with reference to

FIGS. 1 and 2

. In step


202


, the chrome tanned skins are placed in a rotating re-tanning drum


100


.




The rotating drum


100


is a container for use in leather treatment processes and can be replaced with other conventional containers such as a pit. The drum


100


includes a wooden drum portion


101


, supported on legs


102


for rotation about a horizontal axis as shown by arrow


110


. A motor


120


is used with linkage


121


to drive the rotation of drum portion


101


. Motor


120


and linkage


121


are conventional elements. Drum portion


101


also includes a flap


103


adapted to open when the skins are to be added or removed from drum


101


and to seal tightly when the re-tanning process is underway. Drum portion


101


also includes interior baffles


104


used to mix the skins with the various liquids used in the re-tanning process and to prevent skins sticking to each other. The wooden drum is well known in the tanning and re-tanning arts and can be used for a primary tanning process as well.




Turning again to

FIG. 1

, in step


203


, water at a predetermined temperature, an appropriate syntan, and a temperature stabilizing material, which is microencapsulated phase change material (PCM), are premixed. Syntans such as gluteraldehyde solution, formaldehyde, phenols and napthalenes for example may be utilized. The amounts of each of these components, the temperature, and mixing procedures are readily determinable by one of ordinary skill in the art. The premixing of the syntan and microencapsulated phase change material has the purpose of suspending the microencapsulated phase change material in a liquid suspension, which will carry the phase change material into a deep penetration of the internal fiber matrix of the skins.




The amount of microencapsulated phase change material utilized varies depending upon the physical characteristics of the skins being re-tanned, the primary tanning process utilized, and the thermal properties desired. The amount of the thermal material present after this process is complete should be sufficient to allow the microspheres to enhance the thermal stability of the leather when subject to heat or cold. The recommended amount of this material is about 3% or greater by weight of the leather, and more preferably between about 3% to about 15%.




Where a sufficient amount of the microencapsulated phase change material is utilized, the full benefits of the thermal capabilities and characteristics of the microencapsulated phase change material are achieved without the material leaving the leather's internal matrix.




The temperature stabilizing material is within a microcapsule. The microcapsules can range in size from about one to about several 100 microns in diameter and are formed according to the methods described in any one of the following texts to which the reader is referred for an explanation on how to fabricate microcapsules:




Books on Microencapsulation:




1. Vandergaer, J. E., Ed: Microcncapsulation: Processes and Applications. Plenum Press, New York, 1974.




2. Gutcho, M. H.: Microcapsules and Microencapsulation Techniques. Noyes Data Corp., Park Ridge, N.J., 1976.




3. Ranney, M. W.: Microencapsulation Technology, Noyes Development Corp., Park Ridge, N.J., 1969.




4. Kondo, A.: Microcapsule Processing and Technology. Marcel Dekker, Inc., New York, 1979.




5. Nixon, J. R.: Microencapsulation. Marcel Dekker, Inc., New York, 1976.




Articles on Microencapsulation:




1. Sparks, R. E.: “Microencapsulation”, Kirk-Othmer Encyclopedia of Chemical Technology, Vol. 15, 3rd Edition, John Wiley and Sons, Inc., 1981.




2. Thies, C.: “Physicochemical Aspects of Microencapsulation,” Polym. Plast. Technol. Eng., Vol. 5, 7 (1975).




3. Thies, C.: “Microencapsulation”, McGraw-Hill Yearbook of Science and Technology, 1979, pp. 13-21.




4. Herbig, J. A.: “Microencapsulation”, Encyclopedia of Polymer Science and Technology, Vol. 8, 719 (1968).




The temperature stabilizing material within the microcapsules is a phase change material, such as cicosane, or plastic crystals. Plastic crystals, such as 2,2-dimethyl-1,3-propanediol (DMP) and 2-hydroxymethyl-2-methyl-1,3-propanediol (HMP) and the like may be used. When plastic crystals absorb thermal energy, the molecular structure is temporarily modified without changing the phase of the material. In another aspect of the invention, the composition of the phase change material may be modified to obtain optimum thermal properties for a given temperature range.




For example, the melting point of a homologous series of paraffinic hydrocarbons is directly related to the number of carbon atoms as shown in the following table:





















Number of




Melting Point







Compound Name




Carbon Atoms




Degrees Centigrade













n-Octacosane




28




61.4







n-Heptacosane




27




59.0







n-Hexacosane




26




56.4







n-Pentacosame




25




53.7







n-Tetracosane




24




50.9







n-Tricosane




23




47.6







n-Docosane




22




44.4







n-Heneicosane




21




40.5







n-Eicosane




20




36.8







n-Nonadecane




19




32.1







n-Octadecane




18




28.2







n-Heptadecane




17




22.0







n-Hexadecane




16




18.2







n-Pentadecane




15




10.0







n-Tetradecane




14




5.9







n-Tridecame




13




−5.5















Each of the above materials can be separately encapsulated and is most effective near the melting point indicated. It will be seen from the foregoing that the effective temperature range of the leather can, therefore, be tailored to a specific environment by selecting the phase change materials required for the corresponding temperature and adding microcapsules containing the material to the leather.




In addition, the leather can be designed to have enhanced thermal characteristics over a wide range of temperature or at discrete temperature ranges through proper selection of phase change material.




Referring again to

FIG. 1

, in step


204


, the microencapsulated phase change material suspension is added to the drum


100


containing the tanned skins. In step


205


, the rotating drum is run, which mixes and agitates the skins, until the microencapsulated phase change material suspension penetrates the internal fiber matrix of the tanned skins.




Next, in step


206


, an agent such as Calcium Formate is added to the drum, which is conventionally used in tannage processes. In step


207


, the drum is again rotated to allow good distribution of the Calcium Formate around the skins. The drum is run for a predetermined period of time.




Finally, in step


208


the drums are rinsed at a predetermined temperature for a predetermined time. At this point the suspended microencapsulated phase change material has fully penetrated the fiber matrix of the skins and is embedded within the matrix. In some cases the material can bond with the fibers.




The re-tanned leather has microencapsulated phase change material within the internal fiber matrix of the leather in an amount sufficient to produce the thermal properties desired in response to heat or cold.




Referring to

FIG. 3

, a second embodiment of the method of the present invention is diagramed. In this embodiment microencapsulated phase change material is impregnated into the leather during the primary tanning process. In step


301


, the raw skins are placed in a drum. In step


302


, the microencapsulated phase change material is mixed with a liquid to form a suspension. This mixture can include a tanning agent such as chrome or other mineral tannin, a vegetable tannin or a syntan or a combination of these. Once the suspension is formed, in step


303


the suspension is added to the drum. In step


304


, a tannage is added to the drum. The tannage can be added before or after the phase change material. If the suspension has sufficient tanning agent within it, this separate tannage step can be removed. Prior to steps


302


and


304


, the skins can be prepared in the customary manner as discussed above to remove the hair, flesh, and prepare the skins for tanning.




Steps


305


-


310


are similar to steps


205


-


210


, which allow the suspension to penetrate the fiber matrix of the skins until the microencapsulated phase change material is embedded therein. These steps also include rinsing, draining and treating the surface of the skins as known by one of ordinary skill in the art. As a result, the second embodiment allows the microencapsulated phase change material to be impregnated into the leather during the primary tanning process. This primary tanning can be followed up by a re-tanning that includes additional microencapsulated phase change material or without this additional phase change material depending on the concentration of phase change material achieved during primary tanning.




In accordance with the processes disclosed above, the microencapsulated phase change material is able to impregnate the entire leather product so that their unique thermal properties are within the leather, which are sustained permanently.




Leather with embedded microencapsulated phase change material is particularly suitable for use in a variety of leather products, including but not limited to clothing, wearing apparel, sporting goods, home furnishings, vehicles, bags, watch bands as well as other applications where an individual is exposed to different temperatures. The leather is also suitable for use in wearing apparel like dress or specialty/sports gloves, shoes, elbow guards, knee guards and other similar bracing materials, and watch bands, etc.




This material is particularly suited for making sports shoes, such as a golf shoe


400


shown in FIG.


4


. The golf shoe


400


includes an upper


402


joined in a conventional fashion to an outsole


404


. The upper and outsole form an opening


403


for receiving a user's foot. The upper


402


includes an external layer


406


and an internal layer or lining


408


. The lining can be formed of the leather of the present invention, which has a temperature stabilizing material embedded therein. By choosing an appropriate phase change material, the shoes can be adapted for cold or warm weather use. The heat from the user's foot can liquify the phase change material thus cooling the user's foot. If the user's foot is cold, the material can solidify to warm the users' foot. Thus, the user can remain comfortable regardless of the ambient temperature. By incorporating the temperature stabilizing material into the lining, the appearance and fit of the shoe are not affected. The closer this material is to the wearer's skin the better the performance. The preferred microspheres used for golf shoe application is a powder called THERMASORB® 83, which is available from Frisby Technologies of Freeport, New York. Other THERMASORB® formulations made by Frisby Technologies are recommended for activation at higher or lower temperatures.




Leather with microencapsulated phase change material can also form the external layer


406


. This leather can also be placed at various other locations of the shoe including the tongue. This leather can also be combined with thermally enhanced foam or fabric located in other areas of the shoe, such as the insole, tongue, and the collar surrounding the opening so that the surface area of wearers' foot in contact with thermally enhanced materials is maximized.




This material can be used to form various types of sports gloves, including golf, bicycle, baseball/softball, weight lifting gloves and the like. Turning to

FIG. 5

, a golf glove


410


is shown which is formed in a conventional manner to include a body


412


having two panels, which are front panel


412




a


and rear panel


412




b


. The body defines an opening


414


for receiving a user's hand and a plurality of finger casings


416


. The thumb casing can be formed integral with the body or as a separate component. The leather of the present invention can be used to form one or both panels


412




a


,


412




b


of the body to keep the wearer's hands at a comfortable temperature.




While it is apparent that the illustrative embodiments of the invention disclosed herein fulfill the objectives stated above, it is appreciated that numerous modifications and other embodiments may be devised by those of ordinary skill in the art. For example, the Calcium Formate can be removed from the processes or substituted with a similar agent. In addition, the processes can further include impregnating the leather with other additives, such as dyes, etc. as known by those of ordinary skill in the art. Therefore, it will be understood that the appended claims are intended to cover all such modifications and embodiments which would come within the spirit and scope of the present invention.



Claims
  • 1. A tanned leather comprising:an internal fiber matrix; a plurality of microspheres containing a temperature stabilizing material, said microspheres being disposed and embedded within the fiber matrix in a sufficient amount so that the microspheres enhance the thermal stability of the leather when subject to heat or cold.
  • 2. The leather of claim 1, wherein the temperature stabilizing material is a phase change material.
  • 3. The leather of claim 1, wherein the temperature stabilizing material is a plurality of plastic crystals.
  • 4. The leather of claim 1, wherein the amount is about 3% to about 15% by weight.
  • 5. The leather of claim 1, wherein the microspheres are bonded to the internal fiber matrix.
  • 6. The leather of claim 1, wherein it is incorporated in a product selected from clothing, gloves, or shoes.
  • 7. The leather of claim 1, wherein the leather is a leather product in a vehicle.
  • 8. The leather of claim 1, wherein the leather is incorporated into an article of furniture.
  • 9. The leather of claim 6, wherein the leather is incorporated into a shoe.
  • 10. The leather of claim 9, wherein the leather is incorporated into a tongue of a shoe.
  • 11. The leather of claim 9, wherein the leather is incorporated into an insole of a shoe.
  • 12. A method of impregnating a material selected from skins and hides, wherein the method comprises the steps of:placing the material in a container; adding a tanning agent to the container; combining a plurality of microspheres containing a temperature stabilizing material with a liquid to form a suspension; adding the suspension to the container; and agitating the contents of the container until a portion of the micorspheres are disposed and embedded within the fiber matrix so that the microspheres enhance the thermal stability of the material when subjected to head or cold.
  • 13. The method of claim 12, wherein the material is raw skins.
  • 14. The method of claim 12, wherein the material is tanned skins.
  • 15. The method of claim 12, wherein the container is a rotating drum.
  • 16. The method of claim 12, wherein the temperature stabilizing material is a phase change material.
US Referenced Citations (47)
Number Name Date Kind
2694606 Etzkorn Nov 1954
2785086 Strobino Mar 1957
3493460 Windecker Feb 1970
3852401 Suzuki et al. Dec 1974
4048359 Shibanai et al. Sep 1977
4226906 Jacob Oct 1980
4230808 Pietersen Oct 1980
4273825 Nishiyama et al. Jun 1981
4296174 Hanzel et al. Oct 1981
4428998 Hawkinson Jan 1984
4441508 Buirley et al. Apr 1984
4457460 Hirsch et al. Jul 1984
4470917 Hawe et al. Sep 1984
4510188 Ruggeri Apr 1985
4513106 Edgren et al. Apr 1985
4514461 Woo Apr 1985
4524529 Schaefer Jun 1985
4528226 Sweeny Jul 1985
4561981 Characklis Dec 1985
4572864 Benson et al. Feb 1986
4581286 Föttinger et al. Apr 1986
4605586 Lane Aug 1986
4609587 Giordano et al. Sep 1986
4623583 Mischutin Nov 1986
4659619 Tate Apr 1987
4675161 Hashimoto et al. Jun 1987
4681791 Shibahashi et al. Jul 1987
4751116 Schaefer et al. Jun 1988
4756958 Bryant et al. Jul 1988
4807696 Colvin et al. Feb 1989
4911232 Colvin et al. Mar 1990
4923732 Schaefer May 1990
5141079 Whitney et al. Aug 1992
5224356 Colvin et al. Jul 1993
5290904 Colvin et al. Mar 1994
5366801 Bryant et al. Nov 1994
5415222 Colvin et al. May 1995
5499460 Bryant et al. Mar 1996
5532039 Payne et al. Jul 1996
5637389 Colvin et al. Jun 1997
5677048 Pushaw Oct 1997
5708979 Redwood et al. Jan 1998
5722482 Buckley Mar 1998
5759706 Widdemer Jun 1998
5763335 Hermann Jun 1998
5804297 Colvin et al. Sep 1998
5811122 Schlup et al. Sep 1998
Foreign Referenced Citations (2)
Number Date Country
WO 9534609 Dec 1995 WO
9534609 Dec 1995 WO