Disclosed are single crystal nickel-base superalloys exhibiting excellent high temperature creep resistance, while having a reduced or low rhenium content, without deleteriously affecting other relevant characteristics for many turbine engine airfoil applications.
Because of a worldwide growing demand for products that have customarily required substantial quantities of relatively scarce metal elements, both the demand and prices of rare metal elements have sharply increased. As a result, manufacturers are searching for new technologies that will reduce or eliminate the need for these metal elements.
Rhenium is an example of a truly rare metal that is important to various industries. It is recovered in very small quantities as a by-product of copper-molybdenum and copper production. In addition to its high cost, use of rhenium presents a supply chain risk of both economic and strategic consequence.
Rhenium has been widely employed in the production of nickel-base superalloys used to cast single crystal gas turbine components for jet aircraft and power generation equipment. More specifically, rhenium is used as an additive in advanced single crystal superalloys for turbine blades, vanes and seal segments, because of its potent effect at slowing diffusion and thus slowing creep deformation, particularly at high temperatures (e.g., in excess of 1,000 degrees C.) for sustained periods of time. High temperature creep resistance is directly related to the useful service life of gas turbine components and turbine engine performance such as power output, fuel burn and carbon dioxide emissions.
Typical nickel-base superalloys used for single crystal castings contain from about 3% rhenium to about 7% rhenium by weight. Although rhenium has been used as only a relatively minor additive, it has been regarded as critical to single crystal nickel-base superalloys to inhibit diffusion and improve high temperature creep resistance, it adds considerably to the total cost of these alloys.
From the foregoing discussion, it should be apparent that it would be extremely desirable to develop single crystal nickel-base superalloys that exhibit excellent high temperature creep resistance, while significantly reducing the need for rhenium alloying additions, and while retaining other desirable properties such as creep-rupture, low cycle fatigue (LCF) strength and oxidation coating performance.
The low rhenium single crystal nickel-base superalloys disclosed herein rely on, among other things, balancing the refractory metal elements (tantalum, tungsten, rhenium and molybdenum) at a total amount of from about 18% to 19% by weight in order to achieve good creep-rupture mechanical properties along with acceptable alloy phase stability, including freedom from excessive deleterious topological close-packed (TCP) phases that are rich in tungsten, rhenium and chromium, while substantially reducing the rhenium content.
It has been discovered that a low rhenium single crystal nickel-base superalloy exhibiting excellent high temperature creep resistance and other properties well suited for use in casting gas turbine components can be achieved in an alloy composition containing 5.60% to 5.80% aluminum by weight, 9.4% to 9.9% cobalt by weight, 4.9% to 5.5% chromium by weight, 0.08% to 0.35% hafnium by weight, 0.50% to 0.70% molybdenum by weight, 1.4% to 1.6% rhenium by weight, 8.1% to 8.5% tantalum by weight, 0.60% to 0.80% titanium by weight, 7.6% to 8.0% tungsten by weight, and the balance comprising nickel and minor amounts of incidental elements, the total amount of incidental elements being less than 1% by weight.
In the case of certain embodiments of the invention, the incidental elements of the nickel-base superalloy are present at maximum amounts of 100 ppm carbon, 0.04% silicon, 0.01% manganese, 3 ppm sulfur, 30 ppm phosphorous, 30 ppm boron, 0.10% niobium, 150 ppm zirconium, 0.01% copper, 0.15% iron, 0.10% vanadium, 0.10% ruthenium, 0.15% platinum, 0.15% palladium, 200 ppm magnesium, 5 ppm nitrogen (generally in the form of a metal nitride or carbonitride), 5 ppm oxygen (generally in the form of a stable metal oxide), and other trace elements present in amounts of about 25 ppm or less.
In accordance with certain embodiments, the trace elements of the incidental elements in the nickel-base superalloys are present at maximum amounts of 2 ppm silver, 0.2 ppm bismuth, 10 ppm gallium, 25 ppm calcium, 1 ppm lead, 0.5 ppm selenium, 0.2 ppm tellurium, 0.2 ppm thallium, 10 ppm tin, 2 ppm antimony, 2 ppm arsenic, 5 ppm zinc, 2 ppm mercury, 2 ppm cadmium, 2 ppm germanium, 2 ppm gold, 2 ppm indium, 20 ppm sodium, 10 ppm potassium, 20 ppm barium, 30 ppm phosphorous, 2 ppm uranium, and 2 ppm thorium.
In certain embodiments in which enhanced oxidation resistance and/or enhanced thermal barrier coating life are desired, sulfur is present at a maximum amount of 0.5 ppm, and lanthanum and yttrium are added to target an amount of total lanthanum and yttrium of from about 5 ppm to about 80 ppm in the single crystal components cast from the alloy.
In accordance with certain embodiments for large industrial gas turbine (IGT) single crystal applications in which a low angle boundary (LAB) strengthening of up to 12 degrees is desired, carbon is added in an amount from about 0.02% to about 0.05%, and boron is added in an amount of from about 40 ppm to about 100 ppm.
In accordance with certain embodiments, the alloy has a density that is about 8.90 gms/cc or less, such as about 8.85 gms/cc (kg/dm3) at room temperature.
The low-rhenium nickel-base superalloys for single crystal casting disclosed herein will be designated “CMSX®-8” alloys, and will be referred to as such herein. The term “CMSX” is a trademark registered to Cannon-Muskegon Corporation for use in connection with the sale of a family of single crystal (SX) nickel-base superalloys.
Unless otherwise indicated herein, all amounts of elements are given as a percentage by weight or in parts per million (ppm) by weight based on the entire weight of the alloy composition.
Single crystal superalloys and castings have been developed to exhibit an array of outstanding properties including high temperature creep resistance, long fatigue life, oxidation and corrosion resistance, and solid solution strengthening, with desired casting properties with low rejection rates, and phase stability, among others. While it is possible to optimize a single additive for a particular property, the effects on other properties are often extremely unpredictable. Generally, the relationships among the various properties and various elemental components are extremely complex and unpredictable such that it is surprising when a substantial change can be made to the composition without deleteriously affecting at least certain essential properties.
With the embodiments disclosed herein, refractory metal elements (tantalum, tungsten, rhenium and molybdenum) (Table 1) were maintained at a total amount of from about 18% to about 19% by weight, while balancing the amounts of the refractory elements to achieve good creep-rupture mechanical properties along with acceptable alloy phase stability (freedom from excessive deleterious topological close-packed (TCP) phases—normally tungsten, rhenium and chromium rich in this type of alloy). Chromium and cobalt amounts are targeted accordingly to ensure this required phase stability. The high tantalum at approximately 8% is designed to give good single crystal castability and freedom from “freckling” defects, and, along with the 5.7% aluminum and the 0.7% titanium, appropriate γ′ volume fraction at approximately 70% and low negative γ/γ′ mismatch for high temperature creep strength, and acceptable room temperature density of about 8.85 gms/cc (kg/dm3). The density of CMSX-4® is 8.70 gms/cc (kg/dm3) and PWA 1484 is 8.95 gms/cc (kg/dm3). Aluminum, tantalum and titanium are targeted at γ′ volume fraction (Vf) attainment, along with low molybdenum for good high temperature oxidation properties. The small hafnium addition is required for coating life attainment at high temperatures.
Typical chemistry for the alloys disclosed and claimed herein are listed in Table 1. However, there are certain minor variations. First, in order to achieve enhanced oxidation resistance and/or enhanced thermal barrier coating life, it is desirable to add lanthanum and/or yttrium in amounts such that the total of lanthanum and yttrium is targeted to provide from about 5 to 80 ppm in the single crystal castings made from the alloys. As another variation, in the case of large industrial gas turbine (IGT) single crystal applications where low angle boundary (LAB) strengthening is provided up to 12 degrees, carbon and boron additions are targeted in the range from about 0.02% to 0.05% and 40-100 ppm, respectively.
The invention will be described below with respect to certain illustrative, non-limiting embodiments that will facilitate a better understanding.
A 470 lb 100% virgin initial heat of CMSX®-8 alloy was melted in May 2011 in the CM V-5 Consarc VIM furnace using aim chemistry to CM KH May 20, 2011 (CM CRMP #81-1708 Issue 1). The heat (5V0460) chemistry is shown in Table 2.
Two molds (#s 925 and 926) of SX NNS DL-10 test bars were cast to CMSX-4® casting parameters by Rolls-Royce Corporation (SCFO). DL-10 test bar yield at 23 fully acceptable out of a total 24 cast was excellent.
These DL-10 test bars were solutioned/homogenized and double aged heat treated at Cannon-Muskegon Corporation as follows—based on prior work with a precursor similar family alloy designated CMSX®-7.
Solutioning and Homogenization
Good microstructure attainment is evident in FIGS. 1-2—complete γ′ solutioning, little remnant γ/γ′ eutectic, no incipient melting and approximately 0.45 μm average cubic, aligned γ′, indicating appropriate γ/γ′ mismatch and γ/γ′ inter-facial chemistry, following the 4 hr/2050° F. (1121° C.) high temperature age.
Creep- and stress-rupture specimens were low stress ground and tested by Joliet Metallurgical Labs, with the results to date shown in Table 3. Larson-Miller stress-rupture and stress-1.0% creep (
Phase stability is surprisingly good with absolutely negligible TCP phases apparent in the post-test creep/stress rupture bars examined to date (
Recent work has shown it is possible to adequately solution/homogenize heat treat a single crystal test bar in the alloy (
Burner rig dynamic, cyclic oxidation and hot corrosion (sulfidation) testing is currently scheduled at a major turbine engine company.
Creep/stress-rupture data for fully heat treated solution/homogenized and double aged (DL-10s) test specimens for the disclosed alloys are presented in Table 4.
Mini-flat bar stress-rupture testing was performed on single crystal solid turbine blades 10 (
A Larson-Miller stress-rupture graph (
The embodiments disclosed herein are non-limiting examples that are provided to illustrate and facilitate a better understanding, the scope of the invention being defined by the appending claims as properly construed under the patent laws, including the doctrine of equivalents.