Abstract
The invention solves the problem of the manner of obtainment of mass for production of shaped construction elements. The manner consists of the fact, that in the mechanical mixer a ceramic granulate is placed, preferably in the form of pearlite and is soaked, preferably with water until complete soaking of the granulate and is mixed with the binding agent until obtainment of the situation, where each loose grain (1) of the granulate is coated with a layer of moist binding agent, creating a coating (2) around the grain. Priorly prepared moulds are filled with the obtained mass. The mass for production of shaped construction elements consists of 15-25% of bond weight, preferably in the form of pearlite, 35-45% of binding agent weight, preferably in the form of plaster with improved resistance parameters and 35-45% of water weight.
Description

The subject matter of the invention is the manner of obtainment of mass for production of shaped construction elements and mass for production of shaped construction elements, which are useful in construction industry, and in particular in production of construction elements in module systems.


From the application on the Polish invention no. P-329 432, the manner of production, especially of microporous concrete mass, is known, which is useful for erection of concrete or reinforced concrete constructions.


The manner, according to application no. P-329 432, consists of dry mixing the powdered activator with powdered, priorly ground waste glass, in proportion of 1.5 to 2.5% activator and 97.5 to 98.5% glass dust. When the mixture obtains a uniform structure, it is poured in thin layer on a belt conveyor moving inside the furnace, and then it is heated to the temperature of 750 to 950° C. for a specified amount of time, and then rapidly cooled down. The dust poured on the conveyor belt, before heating, is grooved, by creating narrow strips connected with a thin layer formed between the poured powder. During rapid cooling, the formed strips crack, forming small lumps of granulated glass. Size of the lumps can be freely shaped depending on the thickness of the formed strips, cooling temperature and contents of activator. The activator allowing for foaming of the ground waste glass and production of such granulated glass is composed of 45 to 95 weight units of silicon carbide and 1 to 10 weight units of carbon, preferably in the form of soot and 20 to 50 weight units of borax or 1 to 10 weight units of manganese oxide or 20 to 26 weight units of lead oxide together with 20 to 26 weight units of copper oxide.


The substance of solution consisting in obtainment manner of mass for production of shaped tonstruction elements based on the fact, that in the mechanical mixer the ceramic granulate is placed, preferably in the form of pearlite and is soaked, preferably in water until total soaking of the granulate and is mixed with a binding agent, preferably with plaster with improved parameters, until obtainment of the state, where each loose granulate grain is covered with a layer of moist binding agent, creating a coating around the grain. Priorly prepared moulds are filled with the obtained mass and the mass is then subjected to stress treatment until obtainment of connection of individual gratiulate grains only with part of the surface, so there are free spaces left between the grains, filled with air. Stress treatment shall be applied until the pattern of the mould is impressed in the lump of construction element.


The mass for production of shaped construction elements, in accordance with the invention, consists of 15-25% of bond weight, preferably in the form of pearlite, 35-45% of binding agent weight, preferably in the form of plaster with improved quality and 35-45% of water weight.


Solution in accordance with the invention allows for production of individual construction elements with maintenance of hight precision of performance and repetition of the individual elements, constituting the system for construction of foundations, walls, ceilings and roofs of buildings. Owing to spatial distribution of bond grains, surrounded with microscopic construction of hardened binding agent in the mass for production of elements, these elements are characterized with significant resistance to stress with simultaneous maintenance of high thermal insulation which is particularly valuable in use for construction substances structures. Construction elements produced with the manners and of the mass, in accordance with the invention, are resistant to biological factors such as mildew, fungi, rodents, lichen.


The subject matter of the invention explained on the attached drawing, illustrating a construction element with a detail showing the structure of mass of which it was produced. Contents of mass was presented in the example.







EXAMPLE

In order to obtain 100 kg of mass for production of shaped construction elements, in accordance with the invention, the following need to be used:

    • 18.0 kg of bond in the form of granulated pearlite
    • 41.0 kg of binding agent in the form of plaster with improved quality
    • 41.0 kg of water


In priorly prepared mechanical mixer, 18 kg of bond material in the form of pearlite is mixed with 41 kg of water until total soaking of pearlite grains surface. Further, to the mass obtained in such manner, 41 kg of binding agent is added in the form of plaster and is mixed until obtainment of coating of each loose grain of 1 pearlite with coating of 2 moist binding agent. When the mass becomes a collection of identically formed loose grains 1 each coated with a layer of 2 moist binding agent, priorly prepared moulds are filled with it. The mass in moulds is subjected to stressing treatment, so that individual grains 1 only contacted each other partially, with maintenance of free spaces 3 between the coated grains 1. Free spaces 3 are filled with air. By stressing; impression on the element lump will be made of the mould shape. After forming, the completed elements are taken out of the moulds and left until obtainment of proper construction and resistance parameters.

Claims
  • 1. The manner of obtainment of mass for production of shaped construction elements, characterized in that, that in the mechanical mixer ceramic granulate is placed in the form of pearlite and is soaked, preferably in water, until complete soaking of the granulate and is mixed with the binding agent, preferably with plaster of higher class until obtainment of the situation where each loose grain (1) of the granulate will be coated with a layer of moist binding agent, creating a coating (2) around the grain, after which the obtained mass is placed with priorly prepared moulds until full and then it is stress treated until obtainment of connection of the grains with parts of their surfaces, so that there is free space (3) maintained between the grains, filled with air.
  • 2. The mass for production of shaped construction elements, characterized in that, that it consists of 15-25% of bond weight, preferably in the form of pearlite, 35-45% of binding agent weight, preferably in the form of plaster with improved resistance parameters and 35-45% of water weight.
Priority Claims (1)
Number Date Country Kind
P-392 960 Nov 2010 PL national
PCT Information
Filing Document Filing Date Country Kind 371c Date
PCT/PL2011/000116 11/10/2011 WO 00 5/6/2013