The invention relates to a method for non-destructive inspection of a colony of stress corrosion cracks in a pipe or vessel. The invention also relates to an inspection system for carrying out a method according to the invention.
Several pipeline failures around the world have been attributed to Stress Corrosion Cracking (SCC) since its discovery in pipelines in the 1960's including USA, Canada, Russia, France, Saudi Arabia, Australia and South America. While the number of incidents attributed to SCC is less than those attributed to other threats to pipelines such as corrosion or mechanical damage, it constitutes a challenge due to the following reasons:
no reliable, accurate and industry-accepted in-line-inspection tools or predictive modelling based tools exist that are capable of determining what locations along the pipeline are affected by SCC;
no reliable and widely accepted assessment tools exist for evaluation of SCC, once found; and
no reliable and widely accepted tools exist that are capable of measuring the depth of these cracks accurately.
Given these limitations, development of an effective SCC mitigation plan and assessment techniques has been slow. Recent developments in Inline Inspection (ILI) technology and increasing understanding of the phenomenon seem to show promise, but the lack of a reliable non-destructive means for measuring crack depths within an SCC colony makes it difficult to develop a comprehensive approach.
Currently, there are no standard practices for managing SCC. Most operators capitalize on available literature and their experiences to devise an appropriate SCC management and mitigation plan. These practices utilize hydrostatic testing, ILI or Direct Assessment.
In-line Inspection and Direct Assessment require some means of determining the impact of SCC on the integrity of the pipe affected. While several methods have been suggested for calculating the failure pressure, none of the methods have had extensive validation using full-scale burst tests and therefore, are not widely used.
Recent results from a joint initiatives program undertaken by Major North American Operators, accepted as part of the recent CEPA Stress Corrosion Cracking Recommended Practices, utilize a system of severity ranking of SCC into four categories. The categories are defined on the basis of predicted failure pressures. The implementation of such an approach, with the exception of hydrostatic testing, requires a means for the determination of the failure pressures and by extension, a means for accurate measurement of crack lengths, crack depths, and the interlinking crack lengths for an SCC colony.
Common practice in the industry is to use Magnetic Particle Inspection for the detection of SCC at excavation locations. It enables the measurements of colony dimensions with ease. However, due to the large number of cracks that may be present in a colony, crack specific measurements such as crack lengths, mutual separation and interlinking crack lengths are practical estimates.
The application of any of the Failure pressure calculation methods for SCC utilizes crack depth data as well. No widely acceptable, proven and reliable non-destructive technology exists that is capable of measuring the depth (sizing) of SCC. Incremental grinding or buffing remains the most accurate and widely applicable means for sizing SCC as found in the field. The lack of non-destructive sizing technology is also responsible for the lack of a validated SCC evaluation method.
It is an object of the present invention to provide an improved method for non-destructive inspection of a colony of stress corrosion cracks.
Accordingly, the invention provides a method for non-destructive inspection of a colony of stress corrosion cracks in a pipe or a vessel, comprising mapping the colony of stress corrosion cracks, identifying at least one individual crack to be sized within the colony, and sizing the at least one individual crack to be sized. Herein “sizing” refers to determining a depth of the crack. This method provides the advantage that the depth of one individual crack within the colony of stress corrosion cracks can be determined without interference from surrounding cracks within the colony. This provides a more accurate representation of the depth profile of the crack(s) identified to be sized within the colony of stress corrosion cracks, thereby enabling the prediction of the remaining strength of the affected pipe or vessel, e.g. the pipe or vessel comprising carbon steel or stainless steel. Moreover, the measured value of the depth of the individual crack allows calculation of the failure pressure of the colony.
Preferably the at least one individual crack to be sized is identified on the basis of a predetermined criterion, such as crack length. For example the longest crack may be identified as the crack to be sized. Hence, an operator independent identification of the individual crack(s) to be sized is obtained.
Preferably, the predetermined criterion is based on fracture mechanics and/or simulation. Thus, the at least one individual crack to be sized may be chosen such that it is representative for predicting a failure pressure of the stress corrosion cracking affected section of the pipe or vessel, for instance a crack or a group of cracks with a high probability of leading to failure.
Preferably, mapping the colony of stress corrosion cracks, identifying at least one individual crack to be sized within the colony, and/or sizing of the at least one individual crack to be sized is performed automatically. Hence a partially or, preferably, fully automated method may be obtained. Thus, the method can be performed autonomously by an inspection system, and may be independent of an operator.
In an embodiment, the step of sizing is performed using laser ultrasonics. Laser ultrasonics proves to be highly suited for determining the depth of an individual crack within the colony of stress corrosion crack, due to its small footprint.
In an embodiment, the step of mapping is performed using one or more non-destructive examination techniques, such as eddy current, optical imaging, flash thermography and/or radiographic tomography.
It will be appreciated that it may be preferred to perform the step of sizing using a different technique from the technique used in the step of mapping. In this way the method for non-destructive inspection of a colony of stress corrosion cracks may be optimized, e.g. with respect to speed, cost, accuracy etc., by selecting the optimum technique for mapping and the optimum technique for sizing.
In an embodiment, the method is practised on a volume of solid material that comprises a metal, such as a volume of a metal pipeline, the mapping step comprises performing a method of non-destructive inspection along a surface of the volume of solid material (e.g. electromagnetic inspection), for determining the defect pattern and/or distribution along the surface, and the sizing step comprises performing a method of ultrasonic inspection determining a depth of an individual crack associated with a defect of the defect pattern. By using this method, a rather quick overview of defects can be obtained in the mapping step, whereafter an individual defect or set of defects can be sized with high accuracy in the sizing step. The method may thus integrate the advantages of electromagnetic inspection and ultrasonic inspection into a powerful inspection method.
Preferably, the sizing, e.g. the ultrasonic inspection, is performed only over part of the surface that is inspected by the mapping, e.g. the electromagnetic inspection. More preferably, the sizing is performed only adjacent to, close to, and/or near the individual crack(s) to be sized determined by the mapping and subsequent application of a predetermined criterion. In particular, the sizing is performed only for a selection of the defects of the defect pattern determined by the mapping.
Preferably, the mapping, e.g. the electromagnetic inspection, and the sizing, e.g. the ultrasonic inspection, are carried out as a combined scan step, for example substantially at the same time or substantially without waiting time between both methods. Each one of such spatial and temporal limitations on performing the sizing and/or the mapping reduce the inspection time of the method according to the invention.
In an embodiment, a frequency of the applied electromagnetic field in the solid material in the mapping step is varied at or adjacent to the inspection location. Preferably, a plurality of electromagnetic responses are received at or adjacent to the inspection location, influenced by one and the same part of the volume of solid material. This enables an estimate of the defect depth being larger than a predetermined value, thereby allowing a short listing of defects (cracks) that would not be significant enough to affect the strength of the structure
It is another object of the present invention to provide an improved system for carrying out the improved method.
Accordingly, the invention provides an inspection system for non-destructive inspection of a colony of stress corrosion cracks in a pipe or a vessel, comprising a mapping detector for mapping the colony of stress corrosion cracks and arranged for outputting mapping data representative of the colony, a processing unit for identifying at least one individual crack within the colony on the basis of the mapping data, and a sizing detector for sizing of the at least one individual crack.
Different parts of the inspection system may be separate from one another, for example the mapping detector may be separate from, and may be arranged to function independently from, the sizing detector. Preferably, the mapping detector and the sizing detector are integrated into a single inspection device.
In an embodiment, the volume of solid material is comprised by a pipe(line) or a vessel such as a storage tank, and the inspection system comprises positioning means for positioning the mapping detector and/or sizing detector with respect to the pipe or vessel, preferably in two mutually transverse directions with respect to the pipe or vessel. The two mutually transverse directions may be directed in a longitudinal direction of the pipe or vessel and in a circumferential direction of the pipe or vessel, respectively.
The invention will be described by, non-limiting, examples in reference to the accompanying drawing, wherein:
The inspection system 1 comprises a mapping detector 6 for mapping the colony of stress corrosion cracks. In this example, the mapping detector 6 comprises an electromagnetic mapping detector comprising a first electromagnetic transducer 8 for applying an electromagnetic field in the steel wall 4, and a second electromagnetic transducer 10 for receiving a resulting electromagnetic response of the steel wall 4. The electromagnetic mapping detector 6 is arranged for outputting mapping data representative of the detected electromagnetic response. More in general, the mapping detector 6 is arranged for outputting mapping data representative of a mapped colony of stress corrosion cracks.
The inspection system 1 in
The scan frame 12 further comprises second positioning means 20A,20B for positioning the beam 16, and hence the mapping detector 6 in a tangential direction of the pipe 2. Thus the mapping detector 6 is positionably mounted to the scan frame 12 for scanning the mapping detector across a surface of the steel wall 4 of the pipe 2. In this example, the second positioning means 20A,20B each comprise a carriage movably mounted to a circumferential guide rail of the clamp 14A,14B. Here, each of the second positioning means 20A,20B also comprises a drive unit, such as an electric motor for positioning the second positioning means 20A,20B. Preferably, the respective drive units of the second positioning means are mutually synchronised. Preferably, the second positioning means 20A,20B also comprise a position detector, such as a linear encoder, for determining an absolute or relative position of the carriage with respect to a circumference of the pipe 2.
The inspection system 1 further comprises a sizing detector 22. The sizing detector is arranged for sizing an individual crack within a colony of stress corrosion cracks. In this example the sizing detector comprises an exciting laser 24 for generating a ultrasonic waves in the wall 4. The exciting laser 24 can be formed by a pulsed laser, for example a pulsed Nd:YAG laser, for example with a wavelength of 1064 nm, a pulse length of 10 ns, a pulse energy of 50 mJ and a pulse repetition rate of 10 Hz. The sizing detector 22 in this example further comprises a detection laser 26 for detecting an ultrasonic response of the wall 4 to the ultrasonic wave generated by the exciting laser 24. Unlike conventional ultrasonic testing, Laser Ultrasonics has a large frequency bandwidth and a tiny (˜0.5 mm) footprint. These characteristics make it ideally suited for application as a depth sizing tool for closely-spaced cracks in a colony. Laser Ultrasonics provides the ability to size an individual crack within the colony without interference from surrounding cracks within the colony.
In this example, the sizing detector 22 is also mounted to the first positioning means 18 and can hence also be scanned across the surface of the steel wall 4 of the pipe 2. It will be appreciated that it is also possible that the scan frame 12 comprises separate positioning means for the mapping detector 6 and for the sizing detector 22 for independently scanning the mapping detector 6 and the sizing detector 22.
In
It will be appreciated that the inspection system 1 shown in
The inspection system 1 described thus far can be used in a method for non-destructive inspection of a colony of stress corrosion cracks in a pipe or vessel according to the following first example.
In this example, the method starts with the mapping detector 6 scanning at least a part of the wall 4 for mapping the colony of stress corrosion crack. The mapping detector 6 is moved by the first and second positioning means 18,20A,20B. The mapping detector 6 may e.g. be moved in the axial direction for a number of consecutive tangential positions. In this example, the mapping detector only maps the wall 4 while moving in one direction for avoiding hysteresis effects. In this way, a defect pattern can be determined by the mapping detector 6, wherein the defect pattern includes defect locations and/or defect geometries along the surface of the wall 4. The defect geometry may include a length of the defect, a width of the defect, and/or a shape of the defect. The defects in the defect patter may e.g. be associated with locations where stress corrosion cracks are present in the wall 4. The mapping data output by the mapping detector 6 may for instance comprise a table of coordinates at which defects have been detected. If the wall 4 comprises a colony of stress corrosion cracks, the mapping detector 6 will also output mapping data representative of the colony. An example of a defect pattern is described below with respect to
Then, in this example, the processing unit 28, analyses the mapping data and identifies the individual crack or cracks to be sized in the colony. The crack(s) to be sized may e.g. be determined on the basis of a length of a defect in the defect pattern determined by the mapping detector 6. In this example, the processing unit identifies the longest defects in the defect pattern as the individual crack to be sized. Additionally, or alternatively, interaction rules between cracks may be used in determining which crack or cracks in the colony need be sized, or e.g. interlinking crack lengths (lengths between cracks prone to merge). It is also possible that the crack(s) to be sized is (are) determined on the basis of expected relevance of that crack on the local wall strength, e.g. on the basis of fracture mechanics and/or numerical simulation. It is possible to identify the crack(s) with a high probability of leading to failure as the crack(s) to be sized. Also, the processing unit 28 may be arranged to identify a predetermined number of individual cracks to be sized, e.g. the largest crack, or the largest five cracks of the colony.
Next, the inspection system 1 positions the sizing detector 22 at or adjacent the crack to be sized and sizes that crack. It will be appreciated that the sizing detector 22 may be moved towards the individual crack to be sized at a greater speed than at which the sizing detector 22 is moved while sizing the crack to be sized. Here sizing the individual crack indicates determining the depth of the individual crack. Examples of how the individual crack can be sized are described with respect to
Once the individual crack(s) to be sized has(have) been sized, data representative of the determined crack depth(s) can be stored into memory and/or further processed, e.g. for predicting, e.g. calculating, the failure pressure. It is also possible to measure crack length and/or interlinking crack length using the mapping detector and/or sizing detector, e.g. for calculating the failure pressure. The determined crack depth(s) and/or the calculated failure pressure may provide a quantitative indication of the safety risk posed by the inspected colony of stress corrosion cracks. The failure pressure may give a quantitative indication of the remaining strength of the affected wall 4.
In this example, the method starts with the mapping detector 6, here an eddy current detector, scanning at least a part of the wall 4 for mapping (101) the colony of stress corrosion crack. In this way, again a defect pattern can be determined by the mapping detector 6. Here the mapping detector 6 outputs a table of coordinates (102) at which defects have been detected. If the wall 4 comprises a colony of stress corrosion cracks, the mapping detector 6 will also output mapping data representative of the colony (103), e.g. in the form of an SCC colony map.
Then, in this example, the processing unit 28, analyses the mapping data and identifies the individual crack or cracks to be sized in the colony. The crack(s) to be sized are in this example determined (104) on the basis of a depth of a defect in the defect pattern as determined by the mapping detector 6. In this example, the processing unit identifies the deepest defects in the defect pattern as the individual crack to be sized. Additionally, or alternatively, interaction rules between cracks may be used in determining which crack or cracks in the colony need be sized, or e.g. interlinking crack lengths (lengths between cracks prone to merge). The processing unit filters (106) the SCC colony map to remove (105) less relevant cracks.
Next, the inspection system 1 positions the sizing detector 22, here the laser ultrasonics sizing detector, at or adjacent the selected cracks to be sized and sizes these selected cracks (107). Once the selected individual cracks to be sized have been sized, data representative of the determined crack depths can be provided as crack depth profiles (108). Next, the data representative of the determined crack depths can be assessed (109) and a predicted failure pressure of the SCC colony can be calculated (110).
In general, the method comprises the steps of mapping a colony of stress corrosion cracks, identifying at least one crack within the colony of stress corrosion cracks, and sizing the at least one crack. It will be appreciated that the processing unit 28 may be arranged for identifying at least one individual crack within the colony of stress corrosion cracks which at least one individual crack should be sized using the sizing detector 22. The processing unit 28 may identify such relevant crack to be sized on the basis of the mapping data received from the mapping detector 6. It will be appreciated that the processing unit may also comprise a number of separate units, some of which may be integrated with the mapping detector 6 and/or the sizing detector 22.
In the above examples, the inspection system 1 automatically performs the steps of mapping a colony of stress corrosion cracks, identifying at least one crack within the colony of stress corrosion cracks, and sizing the at least one crack. Thus, an automated measurement method is obtained.
It will be clear that such automated mapping and sizing provides the advantage that only individual cracks fulfilling objective criteria, i.e. cracks identified as cracks to be sized by the processing unit 28, will be sized, which reduces inspection time. Also, automatically determining which individual cracks in the colony need to be sized reduces inspection time, as interpretation by an operator is not required, and enhances reproducibility of the inspection.
In these examples, the step of mapping the colony of stress corrosion cracks includes positioning the first electromagnetic transducer 8 at or adjacent to an inspection location of the surface of the wall 4, and applying an electromagnetic field in the wall 4 by using the first electromagnetic transducer 8. Applying the electromagnetic field, for example as an electromagnetic pulse, may result in an eddy current in the wall 4. The eddy current will decay and diffuse away from the first electromagnetic transducer 8 into the wall 4, and create a magnetic field as a resulting electromagnetic response of the wall 4.
In addition, in these examples the step of mapping the colony of stress corrosion cracks includes positioning the second electromagnetic transducer 10 at or adjacent to the inspection location, and receiving the resulting electromagnetic response of the wall 4 using the second electromagnetic transducer 10. The first electromagnetic transducer 8 may be integrated with the second electromagnetic transducer 10 into an integrated mapping detector 6 as shown in
Here, the step of identifying at least one crack within the colony of stress corrosion cracks includes inferring from the electromagnetic response an electromagnetic conductivity of the wall 4. A, e.g. numerical, model for the electromagnetic response may be used wherein the electromagnetic conductivity is a parameter of the model. Such a model is known to the person skilled in the art. By adjusting the parameter that represents the electromagnetic conductivity to match a model response with a measured response, the electromagnetic conductivity can be inferred.
A frequency of the applied electromagnetic field in the solid material may be varied at or adjacent to the inspection location. The frequency may, for example, be in a range from 50 kHz to 250 kHz, for example approximately equal to 130 kHz, within a range of ±10%.
In these examples, the step of mapping the colony of stress corrosion crack comprises positioning the first electromagnetic transducer, applying the electromagnetic pulse, positioning the second electromagnetic transducer, receiving the electromagnetic response, and inferring the electromagnetic conductivity for a plurality of measuring locations along the surface of the wall 4. In this way, a defect pattern can be inferred from the conductivity pattern, wherein the defect pattern includes at least defect locations and defect geometries along the surface. A defect geometry may include a length of the defect, a width of the defect, and/or a shape of the defect. The defects in the defect patter may e.g. be associated with locations where stress corrosion cracks are present in the wall 4.
The step of identifying at least one crack to be sized may include applying an interaction criterium to at least two defects 46 of the defect pattern, for determining whether the at least two defects 46 are interacting. Thereto two distances x and y are defined, that form a box whose opposing corners are approximately coinciding with neighbouring ends of the defects 46, for example neighbouring fracture tips 48 of two cracks, also termed fractures 46.
In these examples, the step of sizing a crack in the colony of stress corrosion cracks includes performing ultrasonic inspection for determining a size of the defect of the defect pattern in a direction transverse to the surface of the wall 4, i.e. determining the depth of that crack. The method of ultrasonic inspection may include selecting the defect from the defect pattern and determining the location of the defect from the defect pattern, and generating a bulk ultrasonic signal in the solid wall 4 at a first position adjacent to the location of the defect. Generating the bulk ultrasonic signal may include applying an excitation laser beam at the first position using the exciting laser 24.
In this example, the step of sizing the individual crack further includes measuring a bulk ultrasonic response signal at a second position adjacent to the location of the defect. The bulk ultrasonic response signal originates from the bulk ultrasonic signal by interaction with the defect in the volume of wall 4. In addition, sizing may include determining at least a first time difference from a moment of generation of the bulk ultrasonic signal at the first position to a moment of arrival of the bulk ultrasonic response signal at the second position, and determining a size of the defect transverse to the surface using at least the first time difference.
In general, the sizing may include a Time-of-Flight-Diffraction (ToFD) measurement.
According to the ToFD method, the size of the fracture 46, in this example the fracture depth d, can now be determined. In order to do this, a first distance c from the first position to the second position can be determined. In addition, or as an alternative, for example a second distance a is determined from the second position 60 to a fracture location 64, being an example of the defect location, in this example the position of the fracture 46 at the surface 56. The first distance c and/or the second distance a can for example be determined by visual inspection, for example by using a ruler. The first distance c and/or the second distance a can also be determined automatically by using ultrasonic waves, for example the surface waves 58. Determining the second distance a in addition to determining the first distance c can also be omitted, for example by positioning the excitation laser beam 52 and the sensing laser beam 62 such that the first and second position 54 and 60 are at substantially equal distances from the fracture location 64. Alternatively, the fracture location 64 can for example be assumed to be at substantially equal distances from the first and second position 54 and 60, while substantially ignoring the actual fracture location 64 between the first and second position 54 and 60. The depth d determined by the ToFD method is relatively insensitive for an error in fracture location 64 made in this way.
In addition, the first time difference from the moment of generation of the bulk ultrasonic signal at the first position 54 to the moment of arrival of the bulk ultrasonic response signal at the second position 60 can be determined. From the first time difference and known or predetermined velocities of the bulk ultrasonic waves 50A and/or 50B in the wall 4, a summed length of a ray path 66A and a ray path 66B of respectively the generated bulk ultrasonic signal and the bulk ultrasonic response signal that originates from the bulk ultrasonic signal, can be determined. In order to do this, an orientation and shape of the fracture 46 is assumed. In first order, it is assumed that the fracture 46 is oriented perpendicularly to the surface 56 and has a planar shape. However, if a-priori information about the fracture orientation and shape is available, for example as a result of a dominant stress loading of the wall 4 in use, or as a result of analysing other fractures in the wall 4, another orientation and/or shape can be assumed. By combination of the summed length of the ray path 66A and 66B, the first and second distance c and a, a size, in this case the depth d, of the fracture 46 can be determined. This can be done using mathematical methods known as such to the person skilled in the art.
The detection laser 26 is in this example a Nd:YAG Diode-Pumped Solid-State (DPSS) laser, for example with a wavelength of 532 nm and a power of 200 mW. Preferably, the bulk ultrasonic response signal is retrieved from the signal carried by the sensing laser beam 62 by demodulation. Alternatively, or additionally, the bulk ultrasonic response signal is retrieved by using an optical interferometer, that makes use of the sensing laser beam 62. Alternatively or additionally, the bulk ultrasonic response signal may also be received by using a piezoelectric ultrasonic transducer.
In general, the sizing may include a Crack-Tip-Diffraction (CTD) measurement method.
Determining the first and second distance c and a may also both be omitted. This can be done for example if the first distance c and/or the second distance a are known, for example by being predetermined. Also, this can be done for example when the fracture depth d is much larger than the first distance c. This can be relevant for example when a fracture 46 has a separation to surrounding defects of the defect pattern that is much smaller than the depth d of the fracture 46, so that the first and second position are chosen relatively close to the fracture location 64.
The sizing can also include determining a second time difference, from a moment of generation of the bulk ultrasonic signal at the first position 54 to a moment of arrival of another bulk ultrasonic response signal at the second position 60. The first time difference in general is different from the second time difference if the other response signal related to the second time difference is caused by another part of the defect, for example another fracture tip, than the response signal related to the first time difference.
In general, methods for determining the depth d of the fracture 46 described with reference to
After determining the fracture depth d or d′, the fracture may be grinded out. The depth of the fracture determined by grinding out can be compared with the fracture depth d or d′ determined as described with reference to
When applying the ToFD or CTD method of
During the scan method of
During the scan methods of
The excitation laser beam 52 and the sensing laser beam 62 are applied at a mutual distance, being equal to the first distance c in
In the foregoing specification, the invention has been described with reference to specific examples of embodiments of the invention. It will, however, be evident that various modifications and changes may be made therein without departing from the broader spirit and scope of the invention as set forth in the appended claims.
In the examples, the mapping detector is arranged for inducing and detecting eddy currents, however, other techniques are suitable for the mapping detector. The mapping detector may e.g. be designed as an optical imaging apparatus, flash thermography apparatus and/or radiographic tomography apparatus.
Due to the small footprint of the exciting laser beam on the wall, laser ultrasonic detection is presently preferred for the sizing detector. Nevertheless, other sizing techniques may be suitable for sizing the individual crack within the colony of stress corrosion cracks.
However, other modifications, variations and alternatives are also possible. The specifications, drawings and examples are, accordingly, to be regarded in an illustrative rather than in a restrictive sense.
In the claims, any reference signs placed between parentheses shall not be construed as limiting the claim. The word ‘comprising’ does not exclude the presence of other features or steps then those listed in a claim. Furthermore, the words ‘a’ and ‘an’ shall not be construed as limited to ‘only one’, but instead are used to mean ‘at least one’, and do not exclude a plurality. The mere fact that certain measures are recited in mutually different claims does not indicate that a combination of these measures cannot be used to advantage.