This application claims priority to European Patent Application No. 22152340.0, the disclosure of which is incorporated herein by reference in its entirety.
The present teaching relates to a method for connecting an electrical cable to a plurality of electrical strands with a contact piece, wherein a crimp region having a central recess, which is at least partially surrounded by a crimp tab, is formed on the contact piece, and the axial ends of the plurality of electrical strands are inserted into the recess and are pressed together to produce an electrical connection to the crimp tab.
When assembling electrical cables, a contact piece, such as a cable lug or a contact pin, is often attached to one end of the cable, with which an electrical connection can be established between the cable and a cable connection when the cable is used. In order to connect the cable to the contact piece, crimp connections are often used by means of which the electrical cable (or its electrical conductor) is pressed in a crimping section of the contact piece. In order to produce an operationally reliable, permanently fixed and electrically good connection between the contact piece and the cable, the cable and the contact piece can also be welded after crimping, for example by means of laser welding. Such connecting methods are known from DE 103 58 153 A1 or DE 10 2009 056 799 A1.
However, such connection methods are complex in terms of process engineering and associated with difficulties. First, an electrical insulation of the cable must be removed in order to expose the electrical conductors of the cable without damaging the conductors. Then the exposed conductor portion has to be arranged in the crimping section and pressed therein. Attention has to be paid to produce a good electrical connection without damaging the electrical conductors. During welding, welding spatter, oxidation or powder traces can occur, which can also impair the cable. If electrical conductors made of aluminum are used, there is also the problem that, on the surface of aluminum, an electrically insulating oxide layer quickly forms, which can impair electrical conductivity and can also lead to impairments during welding.
It is an object of the present teaching to improve process stability during the creation of a connection between a contact piece and a cable, as well as the quality of such a connection.
This object is achieved by the fact that the axial ends of the plurality of electrical strands are fixed by a clamping tool before being inserted into the recess, so that the axial ends of the plurality of electrical strands protrude axially out of the clamping tool and the ends of the plurality of strands protruding axially from the clamping tool are sheared off in the transverse direction with a cutting tool, so that at the axial end of the strands a closed end face is produced, that the axial end of the plurality of electrical conductors is inserted into the recess, and that the plurality of strands are welded to the contact piece by melting the closed end face arranged in the recess by means of radiation energy of a radiation directed onto the end face.
By shearing-off the strands, a closed end face is produced at the axial end of the cable, which on the one hand facilitates the insertion of the cable into the crimping region and, on the other hand, also improves the end-face welding after the crimping. Both increase the process stability of the connection process and also the quality of the produced connection.
The end-face welding can be improved if the closed end face is arranged axially offset in the recess from an end edge of the crimping region facing away from the cable.
Depending on the application, the ends of the plurality of strands protruding axially from the clamping tool can be sheared off normal to the longitudinal axis of the cable so that the end face is aligned normal to the longitudinal axis of the cable, or is sheared off at an angle to the longitudinal axis of the cable, so that the end face is aligned at an angle to the longitudinal axis of the cable.
An oblique end face has certain advantages. On the one hand, radiation, such as a laser beam, which is to impinge substantially normal to the end face, is aligned in a direction deviating from the longitudinal axis of the cable. This can increase safety during welding because radiation cannot escape from a lock of a welding chamber in which the cable is inserted in the longitudinal direction of the cable. Contact pieces can thus also be welded in which the radiation cannot be directed in the longitudinal direction of the cable through a functional part of the contact piece. Not least, an oblique end face also improves the tensile strength and also the electrical conductivity of the connection.
In order to prevent shadowing of the radiation at the end face arranged in the recess, it can be provided that a recess in the crimp tab is provided in the region of the end edge.
Shadowing can also be prevented if the end edge is beveled at an angle to the longitudinal axis of the cable and the end face is beveled at a steeper angle than the angle of the end edge. In this case, a region of the end face is arranged closer to the end edge than is the rest of the end face. A larger region of the end face is thus accessible for the radiation.
The axial end of the strands is advantageously pressed in the radial direction, preferably pressed in a gas-tight manner, before shearing. The resulting region, compressed by the pressing, with fewer cavities between the strands, can on the one hand improve the electrical conductivity. On the other hand, the welding can also be improved because the radiation energy of the radiation can penetrate better into the axial end.
A coating, for example a nickel layer, is often present on the surface of the contact piece. Such a coating on the surface of the contact piece can be removed at least in regions in the crimping region before the crimping in order to improve the electrical connection. Such a coating on the surface of the contact piece can also be removed at least in regions in the welding region and/or in the region in front of the end face in the recess before the welding in order to improve the welding quality. In a particularly advantageous embodiment, the coating is removed with the radiation which is also used for welding.
The present teaching is described below in greater detail with reference to Figs. la to 8, which show schematic and non-limiting advantageous embodiments by way of example. The drawings show:
In
At one axial end, the contact piece 5 has a crimp tab 7 which in
After reshaping on the peripheral surface, the crimp tab 7 usually abuts one another at a crimp tab scarf interface 4 (
The step of forming the crimping region 6, as described for example with reference to
In
In step
The cable 1 is then brought with the crimped contact piece 5 into a welding chamber 20, in which the strands 3 are welded to the crimp tab 7 (
The heating of the end face 9 by the radiation is preferably carried out in such a way that first the edge region of the pressed strands 3 and then the inner region of the pressed strands 3 is heated.
Before inserting the strands 3 into the recess 8 of the crimping region 6, the axial end of the strands 3 is pretreated according to the present teaching, as described with reference to
The axial end of the strands 3 is fixed in a clamping tool 33, for example in the form of two clamping jaws 30, 31 which are movable relative to one another, wherein the axial end of the strands 3 protrudes freely from the clamping tool 33 by a certain axial length L. The axial end of the strands 3 protruding from the clamping tool 33 is sheared off with a cutting tool 32 in the transverse direction Q (transversely to the longitudinal direction of the strands 3). As a result of shearing-off in the transverse direction Q, not only a clean end face 9 is created, but also a closed cut surface results at the interface by the deformation during shearing, since the ends of the strands 3 are compressed or even cold-welded. The finished cut surface forms the end face 9 of the strands 3. The cutting edge 34 of the cutting tool 32 is preferably at an obtuse angle because this assists the production of the closed end face 9. The cutting edge 32 can also be designed to be concave or convex, if necessary, as indicated by dashed lines in
The strands 3 can not only be fixed by the clamping tool 33, but the axial end of the strands 3 can also be pressed in a radial direction, preferably pressed in a gas-tight manner. During pressing, the strands 3 are compressed in the radial direction, for example by the clamping jaws 31, 32, in order to reduce cavities between the individual strands 3 in the pressing region. In the case of gas-tight pressing, cavities in the pressing region are eliminated. Such pressing can improve electrical conductivity at the transition between the strands 3 and the contact piece 5. For pressing, a corresponding radial pressure is exerted on the strands 3.
However, such a pressing can also be a separate process step. In this case, the axial end is pressed with a clamping tool before shearing-off in a separate device.
The clamping jaws 31, 32 advantageously have a non-circular, such as an elliptical or oval, inner shape for the pressing. Gas-tight pressing above all can be realized more easily in a non-circular form.
In addition, the axial end of the strands 3 can also be shaped in the axial direction during pressing, preferably according to the shape of the crimping region 6. Advantageously, during pressing at the axial end, a cylindrical region is formed which merges into a conical region and can then optionally also transition into a rounded inlet region. Such a shape in the axial direction can advantageously be used in a crimping region 6 as shown in Fig. la. If the axial end of the strands 3 is formed analogously or diametrically opposed to the crimping region 6, less forming work has to be applied during crimping due to the preforming. In the case of a gas-tight pressing, the strands 3 are pressed in a gas-tight manner in the region of the cylindrical region, that is to say at the axial end of the strands 3.
However, the end of the strands 3 does not necessarily have to be sheared off at right angles to the longitudinal axis of the strands 3 or of the cable 1, but instead the end face 9 can also be formed at a certain angle a to the longitudinal axis, as shown in
The closed end face 9 produced by shearing has advantages in particular during the end-face welding of the strands 3 with the crimp tab 7. On the one hand, the axial end of the strands 3 can thereby be inserted into the recess 8 more easily and more reliably because no individual strands 3 are able to bend. On the other hand, the end face 9 can thus be better heated with the radiation, preferably the laser beam 21. Both lead to a higher process stability. If the axial end of the strands 3 is additionally compressed, the end face region for welding can be heated even better.
However, shearing-off can also easily be incorporated into the overall process of manufacturing the electrical connection. The shearing-off requires only a short time and can be carried out shortly before the welding. This is particularly advantageous when the strands 3 are made of a material, such as aluminum, that rapidly oxidizes in the ambient atmosphere, such as in ambient air. The shearing results in a bare, oxide-free surface, which improves the welding, but also increases the quality of the electrical connection produced.
A holding device 28 can also be provided in the welding chamber 20 to hold the contact element 5, preferably in the region of the crimping region 6, at least during welding.
The laser beam 21 can be generated by a laser 22 and coupled into the welding chamber 20 via a window 24. However, the laser 22 can also be arranged in the welding chamber 20.
The laser 22 comprises, if required, known devices to guide the laser beam 21 to different points of a certain region, for example the end face 9.
A shielding-gas nozzle 27 can also be provided in the welding chamber 20 to supply shielding gas to the welding point during welding. The quality of the welded joint can thus be increased.
An extraction port 26 can also be provided in the welding chamber 20, preferably in the vicinity of the welding point, to extract welding vapors and possibly shielding gas. This can improve the welding quality.
An air flow can be generated by means of an extraction device 26 and/or a supply of shielding gas to the welding point, which can reduce disadvantageous welding effects, such as oxidation, welding spatter, powder traces, etc.
The advantage of an inclined end face 9 of this kind is that the radiation, for example the laser beam 21, which is to impinge substantially normal to the end face 9, is by default oriented in a direction deviating from the longitudinal axis of the cable 1. In this way radiation can be prevented from escaping through the lock 23 of the welding chamber 20 without the cable 1 having to be bent in the welding chamber 20, as can be seen in
Furthermore, an oblique end face 9 enables the processing of contact pieces 5 whose functional part does not provide a passage for the radiation, for example the laser beam 21, such as for example in the case of a full contact pin.
An oblique end face 9 also improves the tensile strength and the electrical conductivity of the connection.
However, due to the oblique end edge 10, it can happen that the radiation, such as the laser beam 21, does not reach a certain region of the end face 9 in the recess 8 of the crimping region 6 because said region is shadowed by the end edge 10. In order to prevent this, a recess 14 can be provided in the crimp tab 7 in the region of the end edge 10, through which recess the radiation can also reach previously shadowed regions of the end face 9. This is shown in
Such a recess 14 can be produced after crimping by machining, such as milling or grinding, or can already have been prefabricated on the crimp tabs 7, for example when punching the contact piece 5 out of a sheet metal. It is also possible to burn away with the radiation, such as laser beam 21, the part of crimp tab 7 that is disruptive during welding. For this purpose, radiation could be generated, for example, with different power levels. In a further alternative, the angles of the end edge 10 and the end face 9 could be selected differently. In the area of radiation shadowing, the end face 9 could be arranged less far from the end edge 10 and the end face 9 could be arranged at a steeper angle to the end edge 10.
The contact pieces 5 are often punched out of a strip material and bent into the desired shape. The strip material frequently receives a protective coating on the surface, such as a nickel layer. Such a nickel layer can impair not only the electrical conductivity but also the weld quality. For this reason, it is advantageous to remove a coating, if present, before the crimping, at least at locations of the contact piece 5 where an electrical connection is created or where welding is performed. The (partial) removal of the coating can be carried out mechanically, thermally or chemically. For mechanical removal of the coating, for example, the inner surface of the crimp tab 7 can be machined with an abrasive brush. For chemical removal, etching pins or spray nozzles can be used. Thermal removal can be effected by vaporization in the intended region by means of radiation, such as by means of a laser, for example. In an advantageous embodiment, after the crimping and before the welding directly in front of the end face 9 in the recess 8, the coating is removed on the inside of the crimp tab 7 in the welding station 20 by means of the laser beam 21.
The strands 3 and the contact piece 5 can also be first crimped within the welding chamber 20. In such a configuration, the radiation, such as the laser beam 21, can also be used to remove a coating of the contact part at least in regions in the crimping region.
Number | Date | Country | Kind |
---|---|---|---|
22152340.0 | Jan 2022 | EP | regional |