METHOD FOR DETERMINING PHYSICAL SIMILARITY SIMULATION MATERIAL OF SOLID BACKFILL BODY

Information

  • Patent Application
  • 20200003667
  • Publication Number
    20200003667
  • Date Filed
    November 16, 2017
    7 years ago
  • Date Published
    January 02, 2020
    4 years ago
Abstract
A method for determining a physical similarity simulation material of a solid backfill body is provided. A compaction test is run on a gangue backfill body in a lab, to obtain a ε-σ curve regarding the gangue backfill body in the compaction process. Backfill blocks are made by using a thin wood board, sponge, and a paper sheet in different proportions, and then an unconfined compression test is separately run on the backfill blocks used for physical similarity simulation, to obtain εi-σi curves regarding the backfill blocks in the compression process. A sum of squared errors Σ(εi−ε0)2 is introduced to separately calculate a sum of squared errors of the backfill block and that of the gangue backfill body, and accordingly an error between ε-σ curves regarding the test block and the gangue backfill body is determined. Finally, a backfill block for which the sum of squared errors is less than 0.5 is determined as a physical similarity simulation material of the gangue backfill body. By fabrication and selection of similar materials, the present invention can reduce an error caused by a selected backfilling material during a physical similarity simulation experiment, guaranteeing the accuracy of the physical similarity simulation experiment for solid backfill mining.
Description
BACKGROUND
Technical Field

The present invention relates to the field of experimental technologies of backfill mining, and in particular, to a fully mechanized method for determining a physical similarity simulation material of a solid backfill body.


Description of Related Art

With the wide application of fully mechanized solid backfill mining technology in our country, surrounding rock control for overlying strata has been intensively studied. The main methods for studying the movement law of the overlying strata include physical similarity simulation, theoretical analysis, and numerical simulation, among which the physical similarity simulation method is considered as the most direct and effective one. The mechanical properties of a solid backfilling material decisively affect the success of backfill mining technology. If the mechanical properties of the solid backfilling material can be precisely simulated, a control of a solid backfill body over the overlying strata in actual status in the scene can be thoroughly reflected, and the experiment precision can be greatly enhanced. Thus, selection of a solid backfilling material in actual production and an improvement to a backfilling method can be optimized in the future. Therefore, it is highly necessary to develop a method for determining a physical similarity simulation material of the solid backfill body.


SUMMARY

In view of the shortcomings in the prior art, the present invention provides a simple, high-precision, secure and reliable method for determining a physical similarity simulation material of a solid backfill body.


The present invention relates to a method for designing a backfill-mining mass ratio in solid backfill mining, including the following steps:


a running a compaction test on a gangue backfill body by using a servo testing machine, recording values of stress σ and strain ε in a loading process, and drawing a ε00 curve 1 regarding the gangue backfill body in the compaction process as a reference curve;


b. setting the excavation height of a physical similarity model to h, and the excavation step to s, to obtain the height of a backfill block h1=h/n, where the coefficient n in the equation is a real number not less than 1, that is, the height of the backfill block is less than or equal to the excavation height of the model;


c. designing dimensions of the backfill block: setting the length to the excavation step s, the width to that of the physical similarity model, and the height to the excavation height h of the physical similarity model;


d. selecting two categories of materials as a category-1 combined block and a category-2 combined block of the backfill block, separately cropping the two categories of materials according to the dimensions of the backfill block, separately piling up the two categories of materials till the respective aggregate thickness reaches the designed height of a backfill body, and recording the number K of pieces in each material category when the designed height is reached;


e. running an unconfined compression test:


running an unconfined compression test on the category-1 combined block by using the servo testing machine, recording stress σ and strain ε in a loading process, and drawing a ε11 curve 2 regarding the combined block of sponge and a thin wood board in the compression process; and running an unconfined compression test on the category-2 combined block by using the servo testing machine, recording stress σ and strain ε in a loading process, and drawing a ε22 curve 3 regarding the combined block of sponge, a thin wood board, and a common paper sheet in the compression process; and


f. marking twenty equally-spaced points on a coordinate horizontal axis, separately calculating a sum of squared errors between the ε00 curve 1 and the ε11 curve 2, and that between the ε00 curve 1 and the ε22 curve 3, and selecting a combined block corresponding to the curve meeting an expression of Σ(ε1−ε0)2≤0.5 as a physical similarity simulation material of a solid backfill body; or


if neither of the curves meets the expression of Σ(ε1−ε0)2≤0.5, increasing the number of pieces of the sponge to K+1, K+2, K+3, . . . , or K+i, till a curve meeting the expression of Σ(ε1−ε0)2≤0.5 is selected out.


The two categories of materials are described as follows: One category is formed by sponge and a thin wood board, where the sponge is fastened on the thin wood board with a transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and thin wood board equal to h1; and the other one is formed by sponge, a common paper sheet, and a thin wood board, where the sponge is fastened on the thin wood board with a transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and thin wood board equal to h1/2, and then the cropped common paper sheet is fixed on the backfill block formed by the sponge and thin wood board, to make the aggregate thickness of a backfill block formed by the sponge, thin wood board, and common paper sheet equal to h1.


The sponge is ordinary sponge with the thickness of 1.5 cm to 2.5 cm.


The thickness of the thin wood board is about 2 mm to 4 mm.


The common paper sheet is common A4 printing paper.


The excavation height h of the physical similarity model is not greater than 5 cm in general cases.


The beneficial effects are as follows: By use of the foregoing technical solutions, the present invention can reduce an error caused by a selected backfilling material during a physical similarity simulation experiment, and also can correctly design the thickness of similar materials such as sponge, a thin wood board, and a paper sheet, guaranteeing the accuracy of the physical similarity simulation experiment for solid backfill mining.





BRIEF DESCRIPTION OF THE DRAWINGS


FIG. 1 is a schematic diagram showing fabrication of a physical similarity simulation material of a solid backfill body according to the present invention; and



FIG. 2 shows stress-strain curves in a compaction process of solid backfilling materials according to an instance of the present invention.





DETAILED DESCRIPTION OF EMBODIMENTS

Embodiments of the present invention are further described below with reference to the accompanying drawings:


Embodiment 1

In a method for determining a physical similarity simulation material of a solid backfill body of the present invention, a test block of the physical similarity simulation material is fabricated using different combinations of sponge, a thin wood board, and a common paper sheet, and a compression test is run on the test block and an actual solid backfilling material separately with a servo testing machine. Afterwards, data is processed by making a map, to find out a simulation material that is closest to the actual solid backfilling material.


a. A compaction test is run on a gangue backfill body (selected from backfill gangue in a coal mine) by using the servo testing machine, stress σ and strain ε in a loading process are recorded, and a ε00 curve 1 regarding the gangue backfill body in the compaction process is drawn as a reference curve.


b. According to dimensions of a paved physical similarity model, it is determined that the excavation height of the model is h, and the excavation step thereof is s, to obtain the height of a backfill block h1=h/n, where n in the equation is a real number not less than 1, that is, the height of the backfill block is less than or equal to the excavation height of the model.


c. Dimensions of the backfill block are designed as follows: setting the length to the excavation step s, the width to that of the physical similarity model, and the height to the excavation height h of the model. Original materials including sponge, a thin wood board, a common paper sheet, and a transparent tape are acquired. Then, the sponge, thin wood board, and common paper sheet are cropped according to the dimensions of the backfill block.


d. The sponge is naturally piled up till its cumulative height is greater than the designed height h1 of the backfill block, and the number K of pieces of the sponge in this case is recorded.


e. The backfill block is designed to include two categories. One category is formed by the sponge and thin wood board, where a sponge combination is fastened on the thin wood board with the transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and thin wood board equal to h1. The other one is formed by the sponge, common paper sheet, and thin wood board, where a sponge combination is fastened on the thin wood board with the transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and thin wood board equal to h1/2, and then the cropped common paper sheet is fixed on the backfill block formed by the sponge and thin wood board, to make the aggregate thickness of a backfill block formed by the sponge, thin wood board, and common paper sheet equal to h1.


f. An unconfined compression test is run with the servo testing machine on the backfill block formed by the sponge and thin wood board, stress σ and strain ε in a loading process are recorded, and a ε11 curve 2 regarding the backfill block formed by the sponge and thin wood board in the compression process is drawn. An unconfined compression test is run with the servo testing machine on the combined block of the sponge, thin wood board, and common paper sheet, stress σ and strain ε in a loading process are recorded, and a ε22 curve 3 regarding the combined block of the sponge, thin wood board, and common paper sheet in the compression process is drawn.


g. Twenty equally-spaced points are marked on a coordinate horizontal axis, and a sum of squared errors between the curves 1 and 2 and that between the curves 1 and 3 are calculated separately. After calculation, it is learned that the sum of squared errors between the curves 1 and 2 is less than 0.5. Therefore, a combined block corresponding to the curve 2 is selected as the physical similarity simulation material of the solid backfill body.


Embodiment 2

A method for determining a physical similarity simulation material of a solid backfill body of the present invention includes the following steps.


a. A compaction test is run on a gangue backfill body (selected from backfill gangue in a coal mine) by using a servo testing machine, stress σ and strain ε in a loading process are recorded, and a ε00 curve 1 regarding the gangue backfill body in the compaction process is drawn as a reference curve.


b. According to dimensions of a paved physical similarity model, it is determined that the excavation height of the model is h, and the excavation step thereof is s, to obtain the height of a backfill block h1=h/n, where n in the equation is a real number not less than 1, that is, the height of the backfill block is less than or equal to the excavation height of the model.


c. Dimensions of the backfill block are designed as follows: setting the length to the excavation step s, the width to that of the physical similarity model, and the height to the excavation height h of the model. Original materials including sponge, a thin wood board, a common paper sheet, and a transparent tape are acquired. Then, the sponge, thin wood board, and common paper sheet are cropped according to the dimensions of the backfill block.


d. The sponge is naturally piled up till its cumulative height is greater than the designed height h1 of the backfill block, and the number K of pieces of the sponge in this case is recorded.


e. The backfill block is designed to include two categories. One category is formed by the sponge and thin wood board, where a sponge combination is fastened on the thin wood board with the transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and thin wood board equal to h1. The other one is formed by the sponge, common paper sheet, and thin wood board, where a sponge combination is fastened on the thin wood board with the transparent tape, to make the aggregate thickness of a combined block of the sponge and thin wood board equal to h1/2, and then the cropped common paper sheet is fixed on the backfill block formed by the sponge and thin wood board, to make the aggregate thickness of a backfill block formed by the sponge, thin wood board, and common paper sheet equal to h1.


f. An unconfined compression test is run with the servo testing machine on the combined block of the sponge and thin wood board, stress σ and strain ε in a loading process are recorded, and a ε11 curve 2 regarding the combined block of the sponge and thin wood board in the compression process is drawn. An unconfined compression test is run with the servo testing machine on the combined block of the sponge, thin wood board, and common paper sheet, stress σ and strain ε in a loading process are recorded, and a ε22 curve 3 regarding the combined block of the sponge, thin wood board, and common paper sheet in the compression process is drawn.


g. Twenty equally-spaced points are marked on a coordinate horizontal axis, a sum of squared errors between the curves 1 and 2 and that between the curves 1 and 3 are calculated separately, and a combined block corresponding to the curve meeting an expression of Σ(ε1−ε0)2≤0.5 is selected as a physical similarity simulation material of a solid backfill body.


h. If neither of the curves meets the expression of Σ(ε1−ε0)2≤0.5, the number of pieces of the sponge is increased to K+1, K+2, K+3, . . . ; and steps d to g are repeated till a backfill block meeting the expression of Σ(ε1−ε0)2≤0.5 is selected out.


Among the original materials, the sponge is ordinary sponge with the thickness of about 2 cm; the thickness of the thin wood board is about 3 mm; and the common paper sheet is common A4 printing paper.


The excavation height of the physical similarity model of the solid backfill body is not greater than 5 cm in general cases.

Claims
  • 1. A method for designing a backfill-mining mass ratio in solid backfill mining, comprising the following steps: running a compaction test on a gangue backfill body by using a servo testing machine, recording values of stress σ and strain ε in a loading process, and drawing a ε0-σ0 curve 1 regarding the gangue backfill body in compaction process as a reference curve;setting an excavation height of a physical similarity model to h, and an excavation step to s, to obtain a height of a backfill block h1=h/n, wherein coefficient n is a real number not less than 1, the height of the backfill block is less than or equal to the excavation height of the model;designing dimensions of the backfill block: setting a length to the excavation step s, a width to a width of the physical similarity model, and a height to the excavation height h of the physical similarity model;selecting two categories of materials as a category-1 combined block and a category-2 combined block of the backfill block, separately cropping the two categories of materials according to the dimensions of the backfill block, separately piling up the two categories of materials till a respective aggregate thickness reaches a designed height of a backfill body, and recording a number K of pieces in each material category when the designed height is reached;running an unconfined compression test: running an unconfined compression test on the category-1 combined block by using the servo testing machine, recording stress σ and strain ε in a loading process, and drawing a ε1-σ1 curve 2 regarding the combined block of sponge and a thin wood board in compression process; andrunning an unconfined compression test on the category-2 combined block by using the servo testing machine, recording stress σ and strain ε in a loading process, and drawing a ε2-σ2 curve 3 regarding the combined block of sponge, a thin wood board, and a common paper sheet in compression process; andmarking twenty equally-spaced points on a coordinate horizontal axis, separately calculating a sum of squared errors between the ε0-σ0 curve 1 and the ε1-σ1 curve 2, and a sum of squared errors between the ε0-σ0 curve 1 and the ε2-σ2 curve 3, and selecting a combined block corresponding to the curve meeting an expression of Σ(εi−ε0)2≤0.5, wherein i=1 or 2, as a physical similarity simulation material of a solid backfill body; orif neither of the curves meets the expression of Σ(εi−ε0)2≤0.5, increasing the number of pieces of the sponge till a curve meeting the expression of Σ(εi−ε0)2≤0.5 is selected out.
  • 2. The method for designing a backfill-mining mass ratio in solid backfill mining according to claim 1, wherein the two categories of materials are as follows: one category is formed by sponge and a thin wood board, the sponge being fastened on the thin wood board with a transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and the thin wood board equal to h1; and the other category is formed by sponge, a paper sheet, and a thin wood board, the sponge being fastened on the thin wood board with a transparent tape, to make the aggregate thickness of a backfill block formed by the sponge and the thin wood board equal to h1/2, and then the cropped paper sheet being fixed on the backfill block formed by the sponge and the thin wood board, to make the aggregate thickness of a backfill block formed by the sponge, the thin wood board, and paper sheet equal to h1.
  • 3. The method for designing a backfill-mining mass ratio in solid backfill mining according to claim 2, wherein the sponge is ordinary sponge with the thickness of 1.5 cm to 2.5 cm.
  • 4. The method for designing a backfill-mining mass ratio in solid backfill mining according to claim 2, wherein the thickness of the thin wood board is about 2 mm to 4 mm.
  • 5. The method for designing a backfill-mining mass ratio in solid backfill mining according to claim 2, wherein the paper sheet is A4 printing paper.
  • 6. The method for designing a backfill-mining mass ratio in solid backfill mining according to claim 1, wherein the excavation height h of the physical similarity model is not greater than 5 cm.
Priority Claims (1)
Number Date Country Kind
201710156494.6 Mar 2017 CN national
PCT Information
Filing Document Filing Date Country Kind
PCT/CN2017/111280 11/16/2017 WO 00