Method for filling cracks in a concrete structure with foamable polyurethane prepolymer

Information

  • Patent Grant
  • 6309493
  • Patent Number
    6,309,493
  • Date Filed
    Thursday, February 11, 1999
    25 years ago
  • Date Issued
    Tuesday, October 30, 2001
    22 years ago
Abstract
A method for filling cracks in concrete surfaces using a one-component, hydrophilic polyurethane prepolymer without the addition of any granular impregnating agents The prepolymer is provided in a hand-held aerosol container and is injected into the cracks through hollow injection ports that are adhered in place on the surfaces over the cracks and subsequently closed off when filled. The crack is filled from the bottom up to prevent the formation of air pockets in the crack.
Description




BACKGROUND OF THE INVENTION




The present invention relates generally to systems for filling cracks in foundation walls, and more particularly, to a method of filling such cracks with an aerosol liquid and to a system for use with such a method.




Many methods of construction are not perfect. Homeowners that purchase newly built or older homes may discover cracks in the foundation walls of their homes. These cracks may be large in size, up to one-half inch in width or they may be small in size, up to three-sixteenths inch in width. Cracks in any foundation walls, no matter what the size of the crack, can unfortunately teak and admit water into the basement of the house, possibly damaging furnishings and finished areas of the basement. There are many compounds available in the marketplace for sealing such foundation cracks. Some of these compounds include two-component reactive epoxies, hydraulic cements or grouts and plastic-based fillers that are troweled into the crack.




It is also generally known to use polyurethane-based foams to seal such cracks. U.S. Pat. No. 3,847,722 that issued Nov. 12, 1974 describes a crack sealing apparatus and method utilizing a deformable and permeable substrate that is impregnated with a hydrophilic urethane prepolymer for filling cracks and preventing water from leaking through the crack. This substrate includes a complex web element that is formed from an expanded vermiculite. The web element must be impregnated with a separately provided urethane prepolymer by the user, by pouring it onto the web to saturate it entirely with the prepolymer. Once the web element is saturated, the web element is folded or rolled up and wedged or pushed into the crack. When the impregnated material contacts water passing through the crack, the prepolymer expands to form a water-insoluble polyurethane gel. The use of this urethane prepolymer in liquid form by the user is not only messy, but also the user must store the prepolymer in a moisture-proof container to avoid exposure to moisture and start the activation and curing of the prepolymer.




Another similarly complicated method of fixing cracks is described in U.S. Pat. No. 4,758,295, issued Jul. 19, 1988. This patent describes a method of sealing leaks in cracks of concrete walls using a moisture-cured polyurethane prepolymer that has a separate impregnating agent added to it in the form of a granular agent, such as cement or grout. Adding such an agent to a prepolymer is expensive. It may also likely affect the dispensing and injection characteristics of the prepolymer leading to application difficulties and necessitating the use of a high-pressure injection system that is beyond the expense and ability of an ordinary consumer and homeowner.




Neither of these two patents provide a user-friendly system for filling cracks that is simple to use by a homeowner and disposable. Accordingly, the present invention is directed to a method for filling cracks with a liquid hydrophilic urethane prepolymer utilizing a prepressurized aerosol delivery of the prepolymer into the crack and a kit of parts for utilizing such a method that is easily utilized by a consumer to fill cracks without any technical expertise.




SUMMARY OF THE INVENTION




It is therefore a general object of the present invention to provide a concrete crack filling system for use by consumers that is user-friendly and disposable.




It is another object of the present invention to an improved method for filling cracks in concrete by injecting a urethane prepolymer into a crack from a pressurized supply container utilizing an injection tube that enters the mouth of the crack, the injection tube and supply container being disposable.




It is a further object of the present invention to provide a method for filling cracks in concrete or stone walls that includes the steps of: cleaning out loose debris from the crack; applying one or more injection ports to the concrete or stone wall to provide one or more entryways into the crack; covering the exterior of the crack with a sealant material to enclose the crack and the injection ports; providing an amount of crack filling compound in the form of a moisture curable, one-component polyurethane prepolymer in a disposable, aerosol-pressurized container; providing a disposable dispensing nozzle for the aerosol container; injecting the prepolymer into the crack by way of the injection ports and letting the prepolymer cure and seal the crack.




Another object of the present invention is to provide a kit of parts for sealing cracks, the kit including a disposable pressurized container of one-component urethane prepolymer, a dispensing nozzle and injection tube that are attachable to the supply container, a plurality of injection ports and an epoxy compound for sealing the injection parts to the crack.




Yet still another object of the present invention is to provide a method for reliably filling cracks in a concrete or stone wall that includes the steps of: cleaning the crack to remove base debris; attaching a plurality of injection ports over the crack and in communication with the crack, the injection ports being spaced a predetermined distance apart from each other; sealing the outer surface of the crack to create a continuous internal cavity within the crack; testing the sealed crack for continuity; providing a disposable pressurized container containing a one-component urethane prepolymer that expands upon exit from the container and contact with water; methodically injecting, in a stepwise fashion, the prepolymer into the crack from the bottom up through one injection port at a time, permitting the injected prepolymer to flow into the crack to the level of the next injection port, capping off the lower injection port and injecting the prepolymer at the next injection port above the capped injection port.




These and other objects, features and advantages of the present invention will be clearly understood through consideration of the following detailed description.











BRIEF DESCRIPTION OF THE DRAWINGS





FIG. 1

is a process flow chart, illustrating schematically, the steps employed in the methods of the present invention;





FIG. 2

is perspective view of a kit of parts used in the methods of the present invention;





FIG. 2A

illustrates some alternate components that suitable for use in the kit of parts of

FIG. 2

;





FIG. 3

is a view illustrating the step of cleaning out a crack in a concrete or stone wall;





FIG. 4

is a view illustrating the step of drilling an injection opening in the crack;





FIG. 5

is a view illustrating the step of marking injection port locations at a desired spacing along the crack;





FIG. 6

is a view illustrating the step of attaching the injection ports to the crack and sealing the crack around the injection ports to provide an exterior cover for the crack;





FIG. 7

is a view illustrating the step of testing the injection ports and the covered crack for continuity;





FIG. 8

is a view illustrating the step of testing the sealed crack for leaks;





FIG. 9

is a view illustrating the step of assembling the foam injection assembly;





FIG. 10

is a view illustrating the step of injecting the crack-filling prepolymer into the crack in a stepwise fashion;





FIG. 11

is a view illustrating the step of closing off the injection port with different closure elements to prevent backflow of the crack-filling prepolymer out of the port;





FIG. 12

is a view illustrating the step of removing the injection ports once the crack-filling compound has cured;





FIG. 13

is a cross-sectional view of an alternative injection port that may be used with the present invention.











DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS




The present invention is directed to a method of filling cracks in solid, poured concrete and/or stone walls using a kit of parts


50


that are easily utilized by a homeowner. Such a kit


50


is illustrated in FIG.


2


. The kit


50


preferably contains a settable adhesive exterior covering compound


52


, shown as a two-part epoxy compound utilizing respective, separate amounts of A and B reactive components


54


,


55


with a spatula


53


for mixing the components together, a plurality of crack injection ports


56


, a plurality of caps


58


that fit over the ends of the injection ports


56


, a series of crimps


80


that fit on the injection ports


56


, a pressurized container


60


with a supply of an aerosol-driven, one-component prepolymer, and a dispenser assembly


62


that fits the supply container


60


and that mates with the injection ports


56


. A set of disposable gloves


64


may also be provided for the user in the kit


50


.




The supply container


60


preferably takes the form of disposable aerosol can


66


as shown in FIG. having a valve assembly


67


formed in one end


68


thereof by which the crack-filling compound exits from the container


60


when the valve assembly


67


is actuated. The dispenser assembly


62


illustrated can be seen to have a hollow base portion


70


that engages the valve assembly


67


of the aerosol can


66


and a body portion


71


that is interposed between the base portion


70


and an elongated nozzle


72


. An actuator lever


73


is joined to the body portion


71


and extends out from the central axis of the supply container


60


at an angle therefrom so that a user may contact it with one or more fingers while holding the container


60


. (

FIG. 9.

)




Alternatively, as illustrated in

FIG. 2A

, the disposable container may take the form of a larger container


200


, commonly referred to in the art as a “


180


” container that is filled with approximately 30 pounds of sealing material. This container is also known by its DOT designation as a DOT-39 NRC 260/325 container. This container is disposable in the sense that it is manufactured as a thin-walled container that cannot be refilled under federal law. The container


200


has associated therewith, a delivery hose


201


, a valve assembly


204


and a hand-operated dispensing gun


208


through which the contents of the container may be discharged. The gun


208


preferably has a tip that mates with the body portions


77


of the injection ports


56


. Such a gun is commonly sold by the assignee of the present invention under the trade names “Pro-Gun” or “Great-Gun” and are used to dispense one-component polyurethane prepolymers. The structure of such guns are described in US Pat. Nos. 5.615,804 and 5,549,228, the disclosures of which are herein incorporated by reference.




As further shown in

FIG. 2

, the kit


50


includes a plurality of injection ports


56


that have flat, perforated base portions


76


for attachment to the surfaces surrounding the crack


90


. The perforations


75


in the base portions


76


of the ports


56


permit the adhesive


52


to securely mount them to and over the crack


90


. The injection ports


56


further include a tubular, hollow body portion


77


that is open at both ends thereof. This body portion


77


defines a hollow injection passage


78


through the ports


56


into the crack.




A series of closure elements, such as crimps


80


may be supplied with the kit


50


that may be applied to the body portions


77


of the injection ports


56


in order to constrict the size of the passage in the injection port body portion


77


or to close off the passage altogether. These crimps


80


preferably take the form of hollow metal collars


81


that are sized to fit onto and over the injection port body portions


77


. When squeezed by a pliers


82


or other tool as shown in detail “A” of

FIG. 11

, the crimps


80


deform and serve to pinch the injection port body portions


77


closed or to at least partially collapse them to prevent the flow of prepolymer back out of the injection port


56


. The kit


50


may further include a set of caps


58


(shown in detail “C” of FIG.


11


), in place of the crimps


80


, that fit over the free ends of the injection ports


56


for sealing the free ends


61


of the ports


56


. As shown in detail “B” of

FIG. 11

, plugs


59


that are insertable into the open ends


61


of the injection ports may also accompany the kit in lieu of the crimps


80


or caps


58


.




As stated previously, the kit


50


includes a hand-held, pressurized supply container


60


that contains a predetermined amount of an injectable crack filling compound. This compound is preferably a one-component polyurethane prepolymer that is moisture-cured, i.e., hydrophilic in nature, and which is easily dispensed under aerosol pressure and which expands and foams when dispensed from its supply container


60


and when it contacts moisture. The composition of this compound includes a polyester polyol, an isocyanate, a catalyst such as a B-B′dimorpholinodiethylether and a plasticizer such as a mixture of dibutyrate ester isomer. When the isocyanate is reacted with the aforementioned polyol, a polyurethane liquid with an affinity for water is created. The crack filling compound has an excess amount of isocyanate to make it hydrophilic. A propellant is provided in the supply container


60


that drives the compound out of the container


60


and assists in partly forming the foamed end product. A charge of nitrogen having a pressure of about 125 psi is used as the propellant in order to drive the prepolymer out of the supply container and into the crack as explained in greater detail below.




Importantly, unlike the aforementioned prior art, the crack filling compound does not include a granular material as a crack impregnating agent, such as a water-reactive cement or grout. With the use of such a material, as taught by U.S. Pat. No. 4,758,295, care must be taken by the applicator to ensure the proper ratio of materials so as not to affect the curing characteristics thereof. Additionally, because the present invention does not utilize any additional granular component or additive such as cement or grout, the crack filling prepolymer of the present invention is more inexpensively made and may be easily dispersed from an aerosol container, such as the hand-sized can


66


depicted.




The implementation the methods of the present invention shall now be discussed. The preliminary step in this inventive method is illustrated in FIG.


3


and involves cleaning of the crack


90


by using a brush or compressed air or other similar means in order to remove loose debris, dirt and from the crack


90


. The size of the crack


90


is first determined, and if the crack is less than one-quarter to one-eighth inch in width, injection holes


91


are drilled into the surface


92


and crack


90


at intervals of about 8 to 10 inches beginning at the base of the crack


90


and ending beneath the top of the crack, preferably about 5 to 6 inches below the top. (

FIG. 4.

) Where the width of the crack


90


is greater than one-eighth to one-fourth inches, injection port registration marks


93


are placed at intervals of about 10 to 12 inches. (

FIG. 5.

)




A series of injection ports


56


are then applied to the crack


90


at the marked intervals and in alignment with the injection holes


91


. These ports


56


are applied to the crack by first mixing the adhesive components


54


,


55


supplied in the kit


50


and applying it to the edges of the crack


90


. The injection ports


56


have the mixed epoxy


52


applied to them using the spatula


52


, or a trowel, so that the port base portions


76


are firmly embedded in it and excess epoxy flows through the perforations


75


in the port base portions


76


. (FIG.


6


). Once all of the injection ports


56


are attached, the remaining epoxy


52


is used to form a cover


89


extending over the crack


90


in order to completely cover the crack


90


and the base


76


of each port


56


.




Once the epoxy has cured, typically about


24


hours, the crack


90


is tested for continuity by injecting a bubble-forming compound, such as a soapy water solution


92


, into each of the ports


56


. Air is applied to the bottom port of the crack


90


and the other ports are examined to determine the formation of bubbles


91


at the other ports


56


. If bubbles form at the other ports, it indicates that there is continuity between all of the ports through the length of the crack


90


.




The crack


90


and its epoxy cover


89


is then tested for leaks by placing caps


50


over all of the injection ports


56


except one, preferably the bottom port. Soapy water


92


is again preferably sprayed into the open injection port and then air is injected into the open port


56


via a suitable means, such as the squeeze bottle


94


illustrated in FIG.


7


. The epoxy cover


89


is then examined for bubbles


91


that would indicate leaks in it. Any such leaks that are found may then be sealed with a fast-set epoxy.




The foam dispenser is then assembled by engaging the dispenser assembly


62


to the valve assembly


67


of the supply container


60


. (

FIG. 9.

) The dispenser nozzle


72


is then mated to the bottom injection port


56


after inverting the can


60


by inserting the tip thereof in to the injection port body portion


77


and the dispenser actuator lever


72


is depressed by the user in order to open the valve assembly


67


. (

FIG. 10.

) The prepolymer then exits the container


60


and flows through the bottom port


56


into the crack


90


up to the next injection port


56




a


located above it. A crimp


80


(

FIG. 11

, detail “A”) is then crimped to the port body portion


77


in order to seal the lower port. Alternatively, the dispenser is then removed and a cap


58


or plug


57


(details “B” and “C” of FIG.


11


), may then be applied to the end of the port. The dispenser is then moved to the next highest port and the process repeated until foam is injected into the topmost injection port and appears at the top


95


of the crack.




The polyurethane prepolymer is injected from the bottom up along the crack


90


because it is desirable to have the foaming material push itself up through the crack in order to avoid the formation of air pockets. As the prepolymer meets and reacts with water in the crack


90


, it forces air in the crack upward and out of the crack at the top


95


of the concrete wall.




Alternatively as shown in

FIG. 13

, injection ports


56


′ having check or one-way valves


96


incorporated therein may be used to provide a connecting passage between the dispenser and the crack. The valve


96


of the port


56


′ will eliminate the need for the applicator to apply either a crimp


80


or a plug


58


to the port


56


′. Such a valve


96


may include a diaphragm, or skirt member


97


that is located within the injection port body portion


77


′.




After the injection process is completed, the prepolymer is allowed to cure which will take about 7 to 10 days. It should be noted that the injecting of soapy water into the crack is beneficial in that it provides moisture that promotes the foaming of the prepolymer into an expandable foam. Standing water in the crack will also serve the same purpose. The water injection may also be easily accomplished via a conventional squeeze bottle


94


. If, however, for any reason, no water is injected into the crack prior to injecting the prepolymer, the prepolymer will draw moisture out of the concrete and from the atmosphere for curing. Once the polyurethane foam has cured, the injection ports


56


may then be sawn off near their base portions


76


. (

FIG. 12.

)




It will be appreciated that the present invention has a novel disposable nature in that all of its components may be discarded by the user after use. The prepolymer has no impregnating agent and comes in a pressurized supply container that is ready to use by a homeowner without the need for mixing or utilizing a separate dispensing system. The dispensing nozzle easily mates with the injection ports which also simplifies the implementation of the method so that a homeowner of average skill may use it to effectively seal cracks. Additionally, the polyurethane prepolymer is adhesive in nature so that it will adhere to the opposing surface of the crack and remain in place within the crack. It has a desirable viscosity that facilitates its injection into the crack, and it has a desirable flexibility that permits the cured foam to slightly expand and contract within the crack under various climatic conditions.




While the preferred embodiments of the invention have been shown and described, it will be apparent to those skilled in the art that changes and modifications may be made therein without departing from the spirit of the invention, the scope of which is defined by the appended claims.



Claims
  • 1. A method of filling in a crack in a surface of a concrete structure, comprising of steps of:(a) providing a plurality of injection port members for application to said crack, the injection port members having flat base portions and tubular body portions, the tubular body portions defining hollow passages that extend through said injection port members, said members having free, open ends opposite their base portions; (b) applying said injection port members to said concrete structure surface at predetermined intervals along said crack such that said injection port member hollow passages are aligned with and directed toward said crack, and adhering said injection ports to said concrete structure surface with a settable adhesive; (c) covering the remainder of said crack with said settable adhesive while leaving an opening at a top portion of said crack and letting said settable adhesive set to define a sealed, inner passage extending through said crack in communication with said injection port hollow passages; (d) providing a supply of an injectable crack-filling material in the form of a hydrophilic one-component polyurethane prepolymer that expands and foams in response to contact with water said prepolymer not containing any granular impregnating agent entrained within it, said prepolymer supply including a disposable, aerosol supply container having dimensions such that it may be easily held and grasped in a single hand of a user, said supply container further having a dispenser assembly attached thereto with a dispensing nozzle extending therefrom, the dispensing nozzle having a tip that is engageble with said injection port members by way of said dispensing nozzle tip fitting into said injection port member free ends into communication with said injection port member hollow passages; (e) dispensing said prepolymer into said crack in a stepwise fashion from top to bottom along said crack by first engaging said prepolymer supply container dispensing nozzle tip with the lowermost injection port member hollow passage and dispensing said prepolymer into said crack through said lowermost injection port member hollow passage until said prepolymer appears at an injection port member located immediately above said lowermost injection port member; (f) closing off said lowermost injection port member by applying a deformable crimping collar to said lowermost injection port member body portion prior to engaging said, lowermost injection port member body portion with said dispensing nozzle and removing said dispensing nozzle tip from said lowermost injection port member and then applying pressure to said crimping collar sufficient to substantially collapse said lowermost injection port member hollow passage; and, (g) repeat steps (e) and (f) for subsequent injection port members positioned above said lowermost injection port member.
  • 2. The method of claim 1, further including a step of cleaning out loose debris from said crack prior to injecting said prepolymer therein.
  • 3. The method of claim 1, further including a step of injecting water into said crack prior to injecting said prepolymer therein to promote foaming and expansion of said prepolymer.
  • 4. The method of claim 1, wherein said dispenser assembly has an actuating lever that when depressed, opens said dispensing nozzle so that said prepolymer will flow out of said supply container and through said dispensing nozzle, the actuating lever extending away from said dispensing assembly at an angle that permits actuation thereof by said user's hand holding said supply container.
  • 5. A method of filling a crack in a concrete wall so as to top leakage of water through the crack, the method comprising: providing predetermined supply of a one-component, hydrophilic polyurethane prepolymer in a pressurized, disposable container; cleaning said crack to remove loose debris therefrom; determining the size of said crack; forming a series of openings in said crack if said crack does not exceed a threshold size; providing a series of injection ports having flat base portions with hollow, tubular body portions projecting therefrom; installing said injection ports onto a surface surrounding said crack in alignment with and over said crack; applying an adhesive compound to areas of said crack at predetermined intervals along the length of said crack; applying said injection ports to said surface surrounding said crack in a manner such that said injection port tubular body portions open into said crack; covering said crack with the adhesive compound to create a sealed, interior passage within said crack that extends the length of said crack; applying a dispensing nozzle to said supply container; engaging said dispensing nozzle to an open end of the lowermost injection port; actuating said nozzle to dispense said prepolymer into said lowermost injection port and into said crack until said prepolymer appears at a second injection port disposed above said lowermost injection port; closing the lowermost injection port to prevent backflow of prepolymer out of said lowermost injection port; removing said dispensing nozzle from engagement with said lowermost injection port and engaging said second injection port with said dispensing nozzle; actuating said dispensing nozzle to inject an amount of prepolymer through said second injection port and into said crack until said prepolymer appears at a third injection port disposed above said second injection port; closing off said second injection port to prevent backflow of said prepolymer through said second injection port and subsequently removing said dispensing nozzle from said second injection port; and, engaging subsequent, higher injection ports with said dispensing nozzle and injecting said prepolymer therein until said prepolymer enters said crack and appears at injection ports above the level of the injection port at which said injection is occurring; and, closing off said injection ports by providing deformable metal sleeve crimping collars, by applying said crimping collars to said injection port body portions prior to injecting said prepolymer into said injection ports, and by deforming said crimping collars to substantially collapse said injection port body portions.
  • 6. The method according to claim 1, further including steps of testing for leaks in said adhesive compound after it has been applied over said crack, and sealing any leaks found in said adhesive compound.
  • 7. The method according to claim 5, further including a step of allowing said prepolymer to cure within said crack and subsequently removing said injection ports from said surface surrounding said crack.
  • 8. The method according to claim 7 wherein said dispensing nozzle includes a dispensing gun having a free nozzle end dimensioned to fit within said injection port free ends.
  • 9. The method according to claim 5, wherein said prepolymer supply container has a size that permits it to be held in one hand by a user.
  • 10. The method according to claim 9, wherein said dispensing nozzle has a nozzle free end that extends away from said prepolymer supply container and said dispensing nozzle further includes an actuating level extending away from a central axis of said prepolymer supply container and positioned for actuating by one hand of said user.
  • 11. The method to claim 1, further including a step of checking continuity of said sealed interior passage formed in said crack by spraying a liquid into said injection ports hollow passages, injecting air into said crack at one of said injection ports and checking for appearance of said liquid at the remaining injection ports.
  • 12. The method according to claim 11, wherein said liquid promotes foaming and expansion of said prepolymer.
US Referenced Citations (26)
Number Name Date Kind
1883196 Wertz Oct 1932
1953452 Wertz Apr 1934
2313110 Wertz Mar 1943
3236005 Tomosy et al. Feb 1966
3593799 Boughton et al. Jul 1971
3826680 Rio et al. Jul 1974
3847722 Kistner Nov 1974
3917771 Basile Nov 1975
4240995 Milne Dec 1980
4360994 Hodges Nov 1982
4414347 Reich et al. Nov 1983
4555286 Orikasa et al. Nov 1985
4555295 Orikasa et al. Nov 1985
4703089 Damico Oct 1987
4758295 Sawaide et al. Jul 1988
4855001 Damico et al. Aug 1989
4861401 Miura et al. Aug 1989
4930281 Martin et al. Jun 1990
4986862 Matsufuru Jan 1991
5000890 DiStefano et al. Mar 1991
5063006 Tahara Nov 1991
5096962 Holmes-Farlet et al. Mar 1992
5155965 Tabei et al. Oct 1992
5186949 Lai Feb 1993
5253957 Fujikawa Oct 1993
5732530 Pfaff Mar 1998
Non-Patent Literature Citations (5)
Entry
Avanti International Technical Information Sheets AV-510, AV-530 & AV 540—Fall 1995.
SPECCO Industries Data Sheets for U-Mix Urethane Injection Resins 1:1, 40:1, W-10 Waterstopper Cemnet & 301 HVM Mercapton Epoxy gel Oct. 1995.
Polygem “Liquid Concrete Repair” Mixing and application Directions 1995.
Lily Corporation, “Bill of Wares”, 1997.
Flexible Products Company, “Insta-Seal” brochure 1997.