The present invention relates to methods for mitigating acid rock drainage (ARD) or acid mine drainage (AMD) potential through the smoldering combustion of organic materials, including the smoldering combustion of organic liquids or solids embedded or mixed with porous mine tailings.
Recent advances in the field of contaminant hydrogeology have demonstrated that organic contaminants can be remediated through smoldering combustion. This process is known commercially as the Self-sustaining Treatment for Active Remediation (STAR) technology and is the subject of U.S. Pat. No. 8,132,987.
Smoldering refers to combustion of a material at the surface of the solid or liquid material itself. For example, when a combustible material (e.g., tobacco) is compacted to form a porous solid (e.g., a cigarette) and is ignited, the oxidant (e.g., oxygen) diffuses into the surface of the material and the combustion proceeds at the surface of the tobacco leaf fragment. Smoldering is referred to as a heterogeneous combustion reaction because the oxidant (gas) and the fuel (liquid or solid) are distinct phases. This is in contrast to flaming combustion which is a homogeneous reaction occurring in a single (gas) phase.
The smoldering combustion process results in the generation of energy, water, and vaporous emissions, primarily carbon dioxide, carbon monoxide, and to a lesser extent volatile organic compounds and other compounds depending on the conditions of the smoldering system.
Smoldering combustion requires a short duration energy input, and the addition of an oxidant (e.g., oxygen, air, etc.) to initiate and sustain the smoldering combustion reaction. An example of a smoldering combustion reaction is that of a burning charcoal briquette. Smoldering combustion is only possible in the presence of a fuel source and a porous matrix. For the case of a charcoal briquette, the charcoal is both the fuel and the porous matrix; whereas for the STAR process, the fuel is the organic contaminant and the porous matrix is a volume of soil.
Acid rock drainage (ARD) or acid mine drainage (AMD) is an environmental hazard characteristic of mining and other large construction activities, usually within rocks containing an abundance of sulfide minerals. ARD/AMD is often associated with mine tailings (i.e., waste rock), and is characterized as the low pH liquid, often containing toxic metals such as copper or iron draining from these piles, which can have a detrimental impact on streams other aquatic environments.
Acidic conditions are generated primarily through the oxidation of acid-progenitors, the most common of which are metal sulfides (often pyrite, which is iron sulfide) when tailings and other waste rocks are exposed to air and water. Such tailings and other waste rocks are typically present in the form of a porous matrix, which is categorized herein as a porous acid-progenitor matrix. Many acid rock discharges also contain elevated levels of potentially toxic metals that dissolve in the low pH liquid associated with ARD/AMD, especially nickel and copper with lower levels of a range of trace and semi-metal ions, including lead, arsenic, aluminum, and manganese ions.
At some mines, acidic drainage is detected within 2-5 years after mining begins; whereas at other mines, it is not detected for several decades. However, acidic drainage may be generated for decades or centuries after it is first detected. Thus, ARD/AMD is considered a serious long-term environmental issue associated with mining.
Numerous management strategies exist for ARD/AMD including passive and active approaches. Passive approaches include long-term monitoring, with many discharges from abandoned mines being exempt from regulatory control, or the use of constructed wetlands in which metals are precipitated through oxidation or undergo complexation with organic matter after drainage waters are neutralized, typically through a limestone-based treatment process.
Constructed wetlands are a relatively low-cost solution but are limited by the metal loading capacity and the need for wetland sediments to remain largely or permanently submerged (since some metal precipitates retained in sediments are unstable when exposed to oxygen such as copper sulfide or elemental selenium).
There are numerous active technologies for treating ARD/AMD. The most common commercial process is lime (CaO) precipitation in a high-density sludge (HDS). In this application, a slurry of lime is dispersed into a tank containing acid mine drainage and recycled sludge to increase water pH to about 9. At this pH, most toxic metals become insoluble and precipitate, aided by the presence of recycled sludge. In some applications air may be introduced to oxidize and precipitate iron and manganese. The resulting slurry is directed to a sludge-settling vessel, such as a clarifier.
Less complex variants of this process, such as simple lime neutralization, may involve no more than a lime silo, mixing tank and settling pond. These systems are far less costly to build, but are also less efficient (i.e., longer reaction times are required, and they produce a discharge with higher trace metal concentrations, if present).
Other active techniques include calcium silicate neutralization, carbonate neutralization, ion exchange, and metal sulfide precipitation.
In the calcium silicate process, a calcium silicate feedstock, made from processed steel slag, is used to neutralize the liquid by removing free hydrogen ions from the bulk solution, thereby increasing pH. With carbonate neutralization, limestone chips are used to create a neutralizing effect. In cation exchange processes, a resin issued to remove potentially toxic metals (cationic resins), or chlorides, sulfates and uranyl sulfate complexes (anionic resins) from mine water. For metal sulfide precipitation, base metals in the acidic solution are precipitated through contact with free sulfide to produce a base metal-free effluent that can be discharged or further treated to reduce sulfate, and a metal sulfide concentrate with possible economic value.
Many technologies exist for the treatment of ARD/AMD, from traditional high cost water treatment plants to simple in situ water treatment reagent dosing methods. In all cases, these techniques manage the problem once it exists. That is, these techniques are designed to treat acidic, metal ion-bearing water. However, the root cause of ARD/AMD is the generation of acidic conditions through the oxidation of metal sulfides when tailings and other waste rocks are exposed to air and water. Thus, ARD/AMD can be prevented or substantially reduced if metal sulfides are removed from the tailings and waste rocks prior to disposal or as part of a post-disposal remediation strategy.
Metals sulfides can be removed from rocky materials such as tailings and mine waste rock via thermal methods. For example, pyrite will undergo thermal decomposition into elemental sulfur and iron sulfide when heated to a temperature of approximately 540 degrees Celsius, while eliminating sulfur in a concentrated source (usually pyrite) is best suited to roasting temperatures in the range of 600 to 1000 degrees Celsius.
Embodiments described herein rely on the principles of self-sustained smoldering combustion of organic materials and provide benefits over currently available techniques for managing ARD/AMD due to low energy requirements and low cost. Specifically, a liquid or solid organic material (e.g., carbon) can be admixed with a porous acid-progenitor matrix, such as mine tailings and combusted via a self-sustaining smoldering combustion reaction within a combustion front to remove acid progenitors including sulfur, sulfur compounds, and other compounds that react with air and water to create acidic conditions. As smoldering combustion occurs, the combustion front moves through the mixture, removing acid progenitors, and leaving behind a zone of acid-progenitor-depleted material. The organic material is admixed with the tailings or other porous acid-progenitor matrices to produce a mixture through which an oxidant is forced and smoldering is initiated with a heat source. The heat source is then removed or terminated while the oxidant feed is maintained so as to sustain progression of the smoldering reaction through the mixture and the removal of acid progenitors.
In an embodiment of the invention a method is provided for removing acid progenitors through smoldering combustion of an organic material, the method including (1) providing a mixture of the organic material, and a porous acid-progenitor matrix to an impoundment, (2) heating a portion of the mixture, and (3) exposing the mixture to at least one oxidant so as to initiate self-sustaining smoldering combustion of the mixture, thereby creating a zone of smoldering combustion and leaving behind a zone of acid-progenitor-depleted material.
In some embodiments, the acid progenitors are sulfur containing species, such as are present in a porous acid-progenitor matrix composed of tailings. In some embodiments, the impoundment is a pile. In other embodiments, the impoundment is a reaction vessel or a depression. In some embodiments, the mixture is provided to the impoundment and acid-progenitor-depleted material is removed from the impoundment by means of a process selected from a group consisting of a continuous process, a semi-continuous process, and a batch process.
In some embodiments a mixing tool admixes the organic material with the porous matrix in the impoundment to produce the mixture. In some embodiments providing the mixture to the impoundment includes (1) forming a permanent or semi-permanent confinement bed comprising the porous matrix and (2) continuously pouring the organic material into the confinement bed.
In some embodiments the organic material admixed with the porous matrix is chosen from the group consisting of a liquid, an emulsion, a solid, a slurry, and combinations thereof. Some embodiments of the method include causing propagation of the combustion away from a point of ignition of the combustion. In some embodiments, the mixture is continuously fed into a zone of smoldering combustion.
In some embodiments, initiating smoldering combustion includes applying heat to the mixture from at least one internal conductive heating source in direct contact with the mixture. In some embodiments, initiating smoldering combustion includes applying heat to the mixture from at least one convective heating source coupled to the mixture. In some embodiments the at least one convective heating source is external to the mixture. In other embodiments the at least one convective heating source is located within the mixture. In further embodiments initiating smoldering combustion includes applying radiative heat to the mixture.
In some embodiments, exposing the mixture to at least one oxidant includes forcing oxidant through the mixture to initiate self-sustaining smoldering combustion of the mixture and cause the removal of acid-progenitors, thereby creating a zone of acid-progenitor-depleted material. In some embodiments, the oxidant is forced through the mixture by injecting air into the mixture through one or more injection ports. In yet other embodiments, the oxidant is forced through the mixture by creating a vacuum that sucks oxidant through the mixture. In some embodiments, air is forced through the mixture at a linear velocity of between 0.0001 and 100 centimeters per second.
In some embodiments, the method further comprises admixing a porous matrix material with the organic material using a helical mixing tool to produce the mixture, supplying the mixture via a first conveyor system into the zone of smoldering combustion, and removing the acid-progenitor-depleted material via a second conveyor system.
Some embodiments of the method further comprise carrying out the smoldering combustion at a temperature within a range between 200 and 2000 degrees Celsius.
In some embodiments, smoldering combustion is initiated by applying heat to the mixture from one or more internal conductive heating sources. In other embodiments, smoldering combustion is initiated by applying heat from one or more convective heat sources, where the convective heat sources may be external to the mixture, or located within the mixture. In yet other embodiments, the heat is applied as radiative heat.
In some embodiments, the porous matrix containing acid progenitors is subjected to one or more pre-treatment steps to increase smoldering temperature, or to increase sulfur reactivity. In some embodiments, the one or more pretreatment steps include pretreating the porous matrix containing acid progenitors with substances selected from the group consisting of acids, bases, activating compounds, catalysts, chelators, oxidants, and reducing agents, and any combination thereof.
It will be appreciated that while typically porous tailings material will provide the acid progenitors to be removed by smoldering combustion, the methods described herein will apply equally well to other porous acid-progenitor matrices.
In each of the above described embodiments, it is desired to promote/maintain self-sustained smoldering combustion as a method of removing acid-progenitors, including sulfur and other ARD/AMD-generating compounds from materials with the potential to generate acidic conditions.
The foregoing features of embodiments will be more readily understood by reference to the following detailed description, taken with reference to the accompanying drawings, in which:
Embodiments of the present invention are based on using smoldering combustion to remove acid-progenitors, including sulfur and other ARD/AMD-generating compounds from materials with the potential to generate acidic conditions.
In embodiments of the present invention, the porous matrix is the material to be treated and serves as a scaffold to entrap the organic material in an environment that facilitates smoldering combustion. For a solid organic material, the porous matrix required to facilitate smoldering may partially be the organic material itself, but for organic liquids, the porous matrix is a separate material. Smoldering combustion is maintained through the efficient recycling of energy within the system. First, the organic material is combusted, giving off heat energy which is retained by the porous matrix. Second, the retained heat energy is returned to the system from the porous matrix to pre-heat organic material farther removed from the point in space where the combustion process was initiated. Thus, following a short duration energy input to initiate the process, smoldering combustion is self-sustaining (i.e., it uses the energy of the combusting organic materials, along with a supply of oxidant, to maintain the reaction) and is capable of propagating away from the point of ignition through the combustible matter. Smoldering is the only type of combustion reaction that can propagate through an organic material/porous matrix mixture (i.e., flames are not capable of propagating through such a system). In a self-sustaining process, the heating source is terminated following the initiation of smoldering combustion.
The self-sustaining smoldering combustion process can be extended to the treatment of ARD/AMD-generating materials to remove sulfur and other compounds, if appropriate organic materials are present or added to the porous ARD/AMD-generating materials and if the following conditions are met: (1) the organic material contains sufficient inherent energy to sustain a smoldering combustion process (i.e., it is a combustible material); (2) the ARD/AMD-generating materials act as a porous matrix to enable the smoldering process; (3) a heat source is provided to initiate the process; and (4) at least one oxidant (e.g., oxygen, air) initiates and maintains the process.
The efficiency of the smoldering combustion process in removing sulfur and other compounds may be improved by conducting pre-treatment steps. Pre-treatment methods to increase smoldering temperature and/or ensure high reactivity of sulfur may enhance sulfur release or transformation during remediation. Chemical pre-treatments may include treatment with acidic, alkaline, activating, catalytic, chelating, oxidizing, reducing, or other substances to manipulate the valence state of sulfur substances and enhance their reactivity during smoldering.
The self-sustaining smoldering combustion treatment method can use solid or liquid organic materials, slurries formed from solid and liquid material, or emulsions with an organic phase.
The self-sustaining smoldering combustion process has numerous advantages over traditional ARD/AMD treatment techniques. For one, the compounds that can lead to the generation of acidic conditions are removed; thus, the smoldering combustion process mitigates the problem before it can occur. Second, the process is self-sustaining (i.e., it uses the energy of the combusting organic materials, along with a supply of oxidant, to maintain the reaction). Therefore, the smoldering combustion process avoids the need for the continuous addition of energy, heat, or fuels to maintain the high temperatures required for the removal of metal sulfides and other acid progenitors.
Definitions. As used in this description and the accompanying claims, the following terms shall have the meanings indicated, unless the context otherwise requires.
The term “porous matrix” refers to a solid material having pores (open spaces) and wherein the solid material may be a single piece having pores or a collection of granular solids having pores formed by the void spaces between granules. Examples of materials suitable for the porous matrices of embodiments of the present invention include mine tailings, crushed mine waste rock, sand, gravel, crushed stone, and combinations thereof.
The term “acid progenitor” refers to chemical species that react with air and water to create acidic conditions.
The term “acid-progenitor-containing material” refers to a material that contains an acid-progenitor. As used herein, the terms acid-progenitor containing material and ARD/AMD-generating materials are synonymous.
The term “porous acid-progenitor matrix” refers to an acid-progenitor-containing material that is structurally a porous matrix capable of self-sustaining smoldering combustion when combined with suitable organic materials. Examples of materials suitably embodying porous acid-progenitor matrices of the present invention include mine tailings, crushed mine waste rock, sand, gravel, crushed stone, and combinations thereof. As used herein, the terms “porous acid-progenitor matrix” and “porous matrix of ARD/AMD-generating materials” are synonymous.
The term “smoldering combustion” refers to the act or process of burning without flame; a rapid oxidation accompanied by heat and light but not flame. In smoldering combustion, the combustion occurs on the surface of the fuel (i.e., not in the gas phase above the fuel as with a flame), in this case, the organic material.
The term “combustion front” refers to the region within the mixture where smoldering combustion is occurring.
The term “zone of acid-progenitor-depleted material” refers to the region within the mixture where smoldering combustion has occurred, and that is depleted of acid-progenitor when compared to the same region prior to the occurrence of smoldering combustion.
The term “organic material” refers either a liquid or a solid containing organic carbon compounds or combustible compounds.
“Self-sustaining” refers to reaction conditions wherein smoldering combustion propagates through the organic material without the application of external energy; that is, when the already smoldering organic material produces sufficient heat to elevate the temperature in the adjacent material to its combustion point. Conditions may be self-sustaining even if initially the application of heat is required to initiate smoldering combustion.
The term “matrix pile” refers to any pile, mound or conglomeration of a porous matrix material. The matrix pile may be either permanent or semi-permanent.
The term “ignition” refers to the process of initiating smoldering combustion.
The term “conductive heating” refers to the transfer of thermal energy by direct physical contact.
The term “convective heating” refers to the transfer of thermal energy by the movement of fluids.
The term “radiative heating” refers to the transfer of thermal energy by electromagnetic radiation.
The term “mixing tool” refers to an implement that when in use combines or blends the organic material and porous matrix into a mass or mixture.
An “impoundment” of organic material is an aggregation of organic material in a vessel, in a pile on the ground, or in a below ground-level depression.
The term “continuous process” refers to a process whereby a mixture of organic material and porous acid-progenitor matrix is added continuously to an impoundment and acid-progenitor-depleted material is removed continuously from the impoundment.
The term “batch process” refers to a process whereby a bolus of organic material and porous matrix is added to an impoundment, smoldering combustion is allowed to occur, and acid-progenitor-depleted material is removed from the impoundment.
The term “semi-continuous process” refers to a process whereby smolderable material is added in boluses and smoldered material is removed in boluses, while smoldering occurs continuously.
A mixing vessel 11 may be a manufactured cylindrical column or rectangular box (e.g. stainless steel, double walled vessel) or bin, an excavated hole, designated pile, or walled-in enclosure in which a porous media of ARD/AMD-generating materials is emplaced and mixed with an organic material in preparation for application of the smoldering process.
The porous matrix may naturally contain the organic material.
Mixture emplacement may be achieved manually, via backhoe or excavator, or automatically via screw conveyor or conveyor belt systems. Liquid emplacement may be achieved via pouring, pumping, conveying by belt, or gravity feed (e.g., siphoning).
Many organic materials may be used as the fuel source for the smoldering combustion process embodied in the methods disclosed herein. Examples of organic materials for which the methods are particularly effective include hydrocarbon mixtures such as coal, coal tar and creosote, charcoal, tar, shredded tires, agricultural waste, petroleum hydrocarbons, and waste sludges. Methods described here are particularly well suited to solid or liquid organic materials such as vegetable oil, woodchips, and granular activated carbon (GAC).
The mixing tool may be a mechanical mixer 12 such as an auger or a screw or other rotating devices. Mixing may also be achieved via vibration, or rotation (flipping) of the entire vessel. The mixing may also be achieved passively by adding organic material in the form of a liquid, a slurry, or an emulsion to the porous matrix within the vessel and allowing it to disperse naturally due to gravity or capillarity or by injecting such material under pressure into the bottom of the vessel, filling the pore space of the matrix as it migrates to the top of the vessel. The organic material may be added to the porous matrix as a flow or stream of fluids through a pipe, chute, or other emitter.
The mixing process may take place within the same vessel used for the smoldering process in a continuous, batch or semi-continuous process, or completed in a separate dedicated mixing vessel, or without any vessel (i.e., in a pile).
Addition of the matrix of ARD/AMD-generating materials 23 may be achieved manually, via backhoe or excavator, or automatically via screw conveyor or conveyor belt systems.
The conveyor system may be a screw or belt conveyor system leading from a mixing vessel to the reaction vessel and from the reaction vessel to a matrix pile. The admixture conveyor may be a screw conveyor or other mechanical conveying device or be a release mechanism to allow the gravity-fed passage of treated material through the reaction vessel.
Embodiments of the invention include impoundment of organic material with a porous acid-progenitor matrix in an above-ground vessel. However, it is also possible for the impoundment to be below ground (i.e., below the surface of the earth) in a depression.
Further embodiments are possible where the organic waste impoundment is above-ground in a matrix pile or mound.
An example of a matrix pile 42 may be a pile of material excavated for the construction of a depression such as a mine, or a tailings or waste rock pile. The organic material may be applied or admixed with the matrix pile by pouring the organic material onto the surface of the matrix pile through a pressurized or gravity-fed pipe, chute, or emitter, and allowing it to percolate into the matrix pile under gravity or forced pressure, tilled into the matrix pile via tillers or hoes, mixed via backhoe, excavator or soil mixing/drilling rigs.
In the embodiment of
Further embodiments are possible where the organic material 52 is also part of the ARD/AMD-generating solid particle 51 and may not be added to the pore spaces 54 of the porous matrix.
Although the principle of heat recirculation is readily understood, its practical application requires balancing many variables to ensure efficiency, control combustion intensity (i.e., to maintain smoldering), and control the requisite temperature for treatment. Particular attributes of the porous matrix that may require optimization include porous matrix particle size, pore size, and permeability. Particular attributes of the organic material that require optimization include state, chemical composition, concentration, viscosity, density, volatility, and wettability. Particular attributes of the combustion system that require optimization include pre-heating intensity, pre-heating duration, initial oxidant flow rate, maintained oxidant flow rate, air pressure, and oxidant content.
Ignition of smoldering combustion requires both a heating source to initiate combustion and a source of oxidant to initiate and maintain combustion. In the embodiment of
In various embodiments, the oxidant source may be an air compressor, blower, or passive source connected to the reaction vessel through piping or tubing with regulated or unregulated pressure or flow. The air supply port may be a series or singular section of perforated pipe, a port, or an open cavity (plenum) to distribute oxidant in the desired pattern across the surface of the admixture. The heating element may be an electrically-powered cable heater, electrically-powered cartridge heater, electro-magnetically activated heating system, or radiative tube heater in which propane or other external fuel source is internally supplied and combusted.
In some embodiments, the air supply ports are perforated plates, screens, perforated carbon-steel, stainless-steel or other material rods, carbon-steel, stainless-steel or other material wells with wire-wrapped or slotted screens installed within the vessel. The heating elements may be electrical resistive heaters or radiative heaters installed or placed within or adjacent to the air supply ports, installed in or adjacent to the mixture surrounding the supply ports, or an element heating air passing through the supply ports and into the mixture.
In particular embodiments, the oxidant is oxygen supplied as a component of atmospheric air. The reaction is controllable such that terminating the supply of oxygen to the reaction front terminates the reaction. Increasing or decreasing the rate of oxygen flux to the reaction front will also increase or decrease the rate of combustion and, therefore, the propagation rate of the reaction front, respectively.
It should be appreciated that combustion can be monitored according to methods known to those of skill in art to determine the amounts of oxygen, air or other oxidant required to maintain smoldering combustion. Combustion temperatures are commonly monitored with thermocouples which can be placed throughout the volume of material being combusted.
Combustion gases and other vaporous compounds generated by the process are collected at the outlet of the reaction vessel or at the surface of the admixture of organic and porous matrix material.
As illustrated in
The air supply ports may be perforated direct-push carbon-steel, stainless-steel or other material rods, carbon-steel, stainless-steel or other material wells with wire-wrapped or slotted screens installed horizontally through the matrix pile or depression. Air supply ports may also be perforations in the engineered structure supporting the mixture. The heating elements may be electrical resistive heaters or radiative heaters installed or placed within or adjacent to the air supply ports, installed in the matrix pile surrounding the air supply ports, or an above-ground element heating air passing through the air supply ports and into the matrix pile.
Embodiments of the present invention may be designed such that a combustion front propagates through a reaction vessel, depression or matrix pile. The combustion front may be directed through heating and air flow spatial manipulations to proceed upwards, downwards, or laterally in any direction.
The embodiment of
In some embodiments, the organic material/porous matrix is conveyed to the combustion front.
The embodiments of the invention described herein are intended to be merely exemplary; numerous variations and modifications will be apparent to those skilled in the art. All such variations and modifications are intended to be within the scope of the present invention as defined in any appended claims.
Remediation of AMD-Generating Waste Solids
1. Material Preparation
Tailings samples containing porous acid-progenitor matrix materials from a gold mine were received in two approximately 20 L buckets with lids and stored at room temperature. One of the buckets was opened and surface water was drained to expose the solid sediments. Material was extracted from the bucket and placed into a glass container and allowed to air dry for 7 days. After 7 days, the material was crushed lightly with ceramic mortar and sealed in the same container.
Batches of approximately 3 kg of dry tailings solids were prepared for smoldering using a mass ratio of 1 part tailings solids to 1 part coarse sand (Chelford Dry Screen Grit, Sibelco, UK). The sample was then mixed with water to achieve a dry basis moisture content of 15% then sunflower oil was introduced to achieve a dry basis fuel content of 5% by mass. Following mixing, the material was immediately transferred to the column for smoldering.
In the smoldering column (Quartz glass column 138 mm in diameter and 275 mm in height (Multi-lab Ltd, UK)) the air diffuser was buried in coarse sand before the coiled cable heater (130 mm OD coil of 3.25 mm2 cross-section×762 mm length incolnel-sheathed cable heater (240 V, 450 W, Watlow Ltd., UK) was placed above. The tailings mixture was transferred to the column in three lifts then six 1.5 mm OD, 500 mm long type N Nicrotherm D sheath thermocouples (TC Direct, UK) were emplaced along the centerline and connected to a data acquisition system to record temperatures within the column during smoldering. A 20 mm layer of clean sand was added above the mixture as a cap.
2. Smoldering
A convective ignition protocol was used to initiate smoldering of the tailings mixture. Self-sustaining smoldering was achieved (as indicated by the detection of combustion gases in the vapor emissions) after approximately 60 min of pre-heating once a temperature of approximately 350° C. was achieved at the thermocouple embedded 10 mm above the igniter within the column. Following ignition, airflow was increased to 35 litres per minute to initiate robust smoldering in the column. After the temperature reached its peak at the first thermocouple, airflow was increased to 50 litres per minute for the remainder of the process. Power supply to the igniter was switched off after the second thermocouple registered its peak temperature. Airflow continued to be supplied to the process throughout smoldering and subsequent cool-down, terminated once temperatures returned to ambient 20° C. (the airflow was typically left running overnight for convenience).
3. Analysis
3.1. Preparation
Once materials were cooled to 20° C., the column was excavated to collect samples for analysis. The sand from the cap was removed and set aside for reuse. The post-treatment tailings mixture was excavated, placed into plastic bags, and sealed for storage for subsequent analyses.
3.2. Total Potentially Toxic Elements Including Sulphur
All materials were tested for total potentially toxic element content following USEPA Method 3051A. Samples of 0.2 g were pre-digested in a mixture of 2 mL concentrated hydrochloric acid (HCl) and 8 mL concentrated nitric acid (HNO3) in unsealed digestion vessels and allowed to rest overnight. The vessels were sealed the following morning and heated to 175° C. for a period of 10 min in a CEM MARSXpress microwave digester (CEM Microwave Technology Ltd, Buckingham, UK), cooled, and diluted to 100 mL with nanopore water. Samples were analysed by induction coupled plasma optical emission spectrometry (ICP-OES). Triplicate samples were analysed for all materials.
4. Results
4.1. Combustion Test
4.2. Total S Content
Table 1 presents total sulfur (i.e., “Total S”) of the samples before (i.e., “Untreated”) and after (i.e., “Smoldered”) smoldering treatment, indicating 75-79% reduction in total sulfur content.
As indicated above, the peak temperatures observed within the sample ranged from approximately 800° C. to 1050° C. which is consistent with previous smoldering tests at this scale. Higher and more consistent combustion temperatures can be achieved through the smoldering of different fuels (e.g., granular activated carbon) and it is anticipated that greater total S removal can be achieved at higher temperatures.
The present application claims the benefit of U.S. Provisional Patent Application No. 62/835,629, filed Apr. 18, 2019. The disclosure of this application is incorporated by reference herein in its entirety.
Number | Name | Date | Kind |
---|---|---|---|
20120272878 | Grant | Nov 2012 | A1 |
20140241806 | Rockwell | Aug 2014 | A1 |
20140288833 | Lee | Sep 2014 | A1 |
Number | Date | Country |
---|---|---|
2012154402 | Nov 2012 | WO |
2014093469 | Jun 2014 | WO |
2017091623 | Jun 2017 | WO |
2018220492 | Dec 2018 | WO |
Entry |
---|
International Searching Authority—International Search Report—International Application No. PCT/US2020/027896 dated Jul. 27, 2020, together with the Written Opinion of the International Searching Authority, 13 pages. |
Number | Date | Country | |
---|---|---|---|
20200331043 A1 | Oct 2020 | US |
Number | Date | Country | |
---|---|---|---|
62835629 | Apr 2019 | US |