Priority is claimed to Swiss Patent Application No. 00197/11, filed on Feb. 3, 2011, the entire disclosure of which is hereby incorporated by reference herein.
The present invention relates to the field of working finished components and relates to a method for repairing or reconditioning a badly damaged component, in particular from the hot gas region of a gas turbine.
For reasons of good efficiency, gas turbines today have operating temperatures in the hot gas region in excess of 1400° C. It is therefore not surprising that many components of the gas turbines, such as for example moving blades, stationary blades or combustion chamber linings, are exposed to great thermal but also mechanical loads. Since these components are usually produced from expensive high-temperature materials, it is desirable to repair them instead of completely replacing them when they are damaged. In addition, there is often a need to upgrade already installed components, in order to improve their efficiency or adapt them to changing operating conditions.
EP 1 620 225 B1 describes a method for repairing and/or modifying components of a gas turbine in which first at least a portion of the component to be repaired or to be modified is extracted, in particular cut out, from the component. Subsequently, at least the first time this portion of the component is repaired or modified, a data record is created for a replacement part to be produced. The replacement part is then produced by means of a rapid manufacturing process.
After, or even before, the extraction, in particular cutting out, of the particularly damaged portion, and possibly of a tolerance portion adjoining the damaged portion, from the component to be repaired, a data record is created for the replacement part to be produced. In this connection, first a three-dimensional CAD data record is created for the replacement part to be produced. This 3D CAD data record for the replacement part to be produced is subsequently converted into a machine data record. First it is checked whether a 3D CAD data record for the component to be repaired or modified but in the undamaged state or a corresponding new part exists. It is disadvantageous here that an individual distortion (or distortion of a series) cannot be taken into account by the operation. There is always a discrepancy (mismatch) between the actual geometry at the time and the nominal geometry. If such a 3D CAD data record for the undamaged component exists, it is subsequently checked whether firstly there is systematic damage to the component and whether secondly the geometry of the damaged component is reproducible. In the case where there is systematic damage to the component and at the same time the geometry of the damaged component is reproducible, it is possible by taking as a basis statistical evaluations of the size of the damaged portion of the component to be repaired and taking into account during the repair a tolerance portion adjoining the damaged portion, the previously damaged regions of material and greatly stressed regions of the component to deduce the required geometry of the replacement part to be produced and to generate the 3D CAD data record from it.
If, on the other hand, there is no systematic damage to the component to be repaired and/or the geometry of the component that is damaged or to be modified is not reproducible, a reverse engineering of the component, or at least of the relevant regions of the component, is carried out. For carrying out the reverse engineering of the component or component region, first the particularly damaged portion and possibly in addition the tolerance portion adjoining the damaged portion is/are extracted from the damaged component to be repaired. This is followed by performing measurements on the component or component region, for example by mechanical or optical measured-value pick-ups or by computed tomography and subsequent reverse engineering. A 3D CAD data record of the component or component region that is damaged or to be modified, from which the damaged portion and possibly a tolerance portion have previously been extracted, is obtained as a result. From this 3D CAD data record of the worked component or component region, the 3D CAD data record of the replacement part to be produced is determined by establishing the difference in comparison with the 3D CAD data record of the undamaged component.
However, such reverse engineering is altogether very laborious.
WO 2008/034413 describes a method of repair for moving blades of a gas turbine in which a damaged portion of a damaged blade tip is removed by forming a parting surface and then the removed portion is reconstructed on the parting surface by means of a generative process (rapid manufacturing) using three-dimensional CAD structural data of the blade. Such a method of repair entails considerable restrictions concerning the choice of material and the geometry.
WO 2008/046386 describes the building up of a complete gas turbine component by such a rapid manufacturing method.
General methods for creating three-dimensional parts to which reference is made further below in the course of the description are described in, for example, EP 946325, DE 10219983, EP 1358855, U.S. Pat. Nos. 6,355,086, 6,811,744 and 7,537,722.
In an embodiment, the invention provides a method for repairing or reconditioning a damaged component. The damaged component is worked by removing a damaged region from the damaged component while creating a cutout corresponding to the damaged region so as to provide a worked component. The worked component is measured and a computer-aided design (CAD) model of a replacement piece based on the measuring and is configured to be inserted into the cutout of the worked component is created. The replacement piece is produced based on the CAD model. The replacement piece and the worked component are connected by joining.
The present invention will be described in even greater detail below based on the exemplary figures. The invention is not limited to the exemplary embodiments. Other features and advantages of various embodiments of the present invention will become apparent by reading the following detailed description with reference to the attached drawings which illustrate the following:
An embodiment of the invention provides a method for repairing or reconditioning a badly damaged component that manages without a parametric CAD model of the component and of the cutout part comprising the damaged region, can be used easily and flexibly and is distinguished by a reduced reject rate.
In an embodiment, the method according to the invention for repairing or reconditioning a badly damaged component, in particular from the hot gas region of a gas turbine, is distinguished by the following steps:
In an embodiment of the invention an individual cutting line is defined for cutting out the damaged region.
According to another refinement of the invention, the removal of the damaged region is performed by a working process. In particular, an EDM process may be used as the working process. However, it is also conceivable to use a milling process as the working process.
In an embodiment, at the same time, to simplify matters, the working process can be carried out without regard for retaining the geometry of a cutout part. In such a case, a complex line can be used as the cutting line.
In an embodiment of the invention the damaged component is likewise measured before the working.
In particular, the measuring may be carried out by means of a mechanically or optically sensing method. A 3D scanning process is preferably used for the measuring.
According to a further refinement, the outer contour of the replacement piece is virtually reconstructed by CAD modeling on the basis of measurement data.
In other cases, it is of advantage if the outer contour of the replacement piece is virtually reconstructed by subtraction of measurement data for the unworked damaged component and measurement data for the worked damaged component.
It is also conceivable that, in the course of the invention, a cutout part is obtained during the working process, and for making further use of its geometry, the cutout part is measured.
In particular, the inner contour of the replacement piece may be virtually reconstructed by using the measurement data of the worked and/or unworked damaged component and/or of a cutout part.
In this connection, it is advantageous if a virtual reconstruction of the replacement piece is created by combining its obtained outer contour and inner contour.
Another refinement of the invention is distinguished by the fact that the CAD model of the replacement piece comprises information concerning the outer contour, the inner structure and cooling air holes on the basis of measurement data.
It is also conceivable within the implementation of the repair that the geometry of the replacement piece is modified by reverse engineering for specific cases of damage or for meeting specific new requirements.
In an embodiment of the invention the replacement piece is produced on the basis of the created drawings or digital models.
According to a further refinement, the replacement piece is produced by casting, a generative process or by a machining process.
The replacement piece is preferably produced by selective laser melting as a generative process.
The replacement piece may, however, also be produced by machining, in particular by milling or electrochemical working.
Furthermore, it is conceivable that the contour of the replacement piece is re-worked to prepare the contact surfaces before the joining.
The re-working of the contour may preferably be carried out by adaptive working in dependence on the required gap tolerance of the joining process and the production tolerance of the replacement piece.
However, it is also conceivable that additional geometrical structures that cannot be created during the production of the replacement piece are created by re-machining of the replacement piece.
According to a further refinement of the invention, the produced replacement piece is connected to the component with a material bond by manual welding or automatic welding or high-temperature brazing or a combination thereof.
The produced replacement piece is preferably connected to the component by high-temperature brazing.
A further refinement of the invention is characterized in that, after the joining of the component and the replacement piece, a re-working of the contour is performed. The re-working is in this case preferably performed by adaptive machining, or adaptively and by machine.
In the case of the proposed method for repairing a removed component, in particular from the hot gas region of a gas turbine, the damaged region is worked by means of methods which make it possible to minimize the loss of material when cutting out the region, which is then replaced by a matching replacement piece. This replacement piece may be produced by a generative production process (“rapid manufacturing process”), such as for example selective laser melting (SLM), selective laser sintering (SLS), electron beam melting (EBM) or standard methods, such as for example a lost-wax method, or a working process, such as for example milling.
In an advantageous embodiment of the invention (
On the basis of the measurement data thereby obtained (virtual worked component Bvirtual in
The final CAD data record ECAD of the replacement piece is virtually reconstructed by combining the outer contour and the inner contour of the cutout part, in that the CAD model of the component with the inner geometry IG, DCAD with IG, and the CAD model of the worked component, BCAD, are combined with each other (
An additional production tolerance may be added in the region of the parting line to the geometry data record of the cutout part or of the replacement piece. This makes it possible to compensate for the loss of material during the cutting and preparing of the parting line surface and, if necessary, to carry out a final or individual adaptation of a standard replacement piece to the individual removed component to be repaired.
In another embodiment of the invention (
After the scanning, the damaged region is removed by a working process (
After the working process, the worked component B with the cutout is measured for a second time by a mechanically or optically sensing method (scanned with a scanner 16; see
The final CAD data record of the replacement piece is virtually reconstructed by combining the outer contour and the inner contour of the cutout part. In this way, the resultant geometry data record of the replacement piece comprises information concerning the inner surface, possible defects, local changes in the wall thickness and positions of cooling air holes of the removed component.
Here, too, an additional production tolerance may be added in the region of the parting line to the geometry data record of the cutout part or of the replacement piece. This makes it possible to compensate for the loss of material during the cutting and preparing of the parting line surface and, if necessary, to carry out a final or individual adaptation of a standard replacement piece to the individual removed component to be repaired.
On the basis of the created geometry data record of the replacement piece, this replacement piece may be produced by a generative production process (“rapid manufacturing process”), such as for example selective laser melting (SLM), selective laser sintering (SLS), electron beam melting (EBM) or laser deposition welding (DMD). Standard methods, such as for example a lost-wax method, or a working process, such as for example milling, may also be used. The decision on the production technology that is used also depends on the degree of damage, the number of pieces and the complexity of the cutout part.
Before the produced replacement piece is connected to the removed component, each replacement piece may be worked in the contour in order to achieve optimum conditions at the parting line surface for the final joining process (for example roughness, gap geometry/gap tolerance). Depending on the procedure selected, the contour working step may be performed by removing a constant thickness or by individual, adaptive working Depending on the working process, other steps apart from the contour working may be necessary prior to joining, such as for example thermal treatments to improve the weldability or stress relief annealing of replacement pieces produced by generative processes.
The joining of the produced replacement piece and the component may be carried out by conventional joining processes, such as for example brazing or welding or a combination of the two. In addition, a subsequent thermal treatment and after-working may be performed at the end of the reconditioning steps performed on the component.
The various possibilities of the method according to the invention can be summarized in a flow diagram such as that depicted in
The thus-worked component with the cutout is in both cases measured (once again by a 3D scanning process) in order to create a corresponding record of measurement data. If the cutout part (17 or Ccutout in
The replacement piece produced is then re-worked with a view to surfaces suitable for the joining and/or required tolerances or additional properties. The re-worked replacement piece is then connected with a material bond to the worked component by joining, in order finally to obtain a repaired component.
With the method according to the invention, the following properties and advantages are obtained:
While the invention has been described with reference to particular embodiments thereof, it will be understood by those having ordinary skill the art that various changes may be made therein without departing from the scope and spirit of the invention. Further, the present invention is not limited to the embodiments described herein; reference should be had to the appended claims.
Number | Date | Country | Kind |
---|---|---|---|
197/11 | Feb 2011 | CH | national |
Number | Name | Date | Kind |
---|---|---|---|
6215093 | Meiners et al. | Apr 2001 | B1 |
6355086 | Brown et al. | Mar 2002 | B2 |
6811744 | Keicher et al. | Nov 2004 | B2 |
7537722 | Andersson et al. | May 2009 | B2 |
7810237 | Lange et al. | Oct 2010 | B2 |
20030105538 | Wooten | Jun 2003 | A1 |
20040031780 | Hagemeister et al. | Feb 2004 | A1 |
20070084047 | Lange et al. | Apr 2007 | A1 |
20090144980 | Rangarajan et al. | Jun 2009 | A1 |
20090271985 | Lange | Nov 2009 | A1 |
20110099810 | Stankowski et al. | May 2011 | A1 |
20110264413 | Stankowski et al. | Oct 2011 | A1 |
Number | Date | Country |
---|---|---|
10219983 | Dec 2003 | DE |
946325 | Oct 1999 | EP |
1358855 | Nov 2003 | EP |
1620225 | Jul 2006 | EP |
2070641 | Jun 2009 | EP |
2317075 | May 2011 | EP |
2317076 | May 2011 | EP |
2347850 | Jul 2011 | EP |
2007278995 | Oct 2007 | JP |
2010207884 | Sep 2010 | JP |
WO 2004096487 | Nov 2004 | WO |
WO 2008034413 | Mar 2008 | WO |
WO 2008046386 | Apr 2008 | WO |
Entry |
---|
European Patent Office, Examination Report in Swiss Patent Application No. CH 01972011 (May 16, 2011). |
European Search Report dated Feb. 29, 2012, issued by European Patent Office in corresponding European Patent Application No. 12152794.9 (10 pgs). |
Number | Date | Country | |
---|---|---|---|
20120198676 A1 | Aug 2012 | US |