This invention relates to the extraction and subsequent concentration of lithium from sedimentary clay. Specifically, this invention relates to a method of extracting and subsequent concentration of lithium from sedimentary rock contained within sedimentary clay.
Lithium and lithium compounds are vital components in industries such as energy storage, ceramics, electronics, lubrication, and metallurgy. While terrestrial sources of lithium are widespread, it is nonetheless difficult to obtain lithium in appreciable quantities. As described in the Handbook of Lithium and Natural Calcium, “Lithium is a comparatively rare element, although it is found in many rocks and some brines, but always in very low concentrations. There are a fairly large number of both lithium mineral and brine deposits but only comparatively few of them are of actual or potential commercial value. Many are very small, others are too low in grade.” Garrett Donald (2004) Handbook of Lithium and Natural Calcium, Academic Press.
Given this, there have been many attempts to extract lithium from different sources in efficient and economical ways. For example, U.S. Pat. No. 2,608,465 describes a method of extracting lithium sulfate from lithium phosphate deposits. Similarly U.S. Pat. Nos. 2,516,109; 2,801,153; 2,923,600; 2,972,517; and U.S. Pat. No. 3,007,770 describe methods of extracting lithium carbonate or lithium hydroxide from spodumene ores. Separately WO2017200408 and CN102041380 disclose methods of extracting lithium from lepidolite ore.
Sedimentary clays are another source of appreciable amounts of lithium Also known as secondary clays, sedimentary clays have been displaced and eroded by movements of the earth over geologic time scales. Embedded within sedimentary clays are sedimentary rocks containing detrital material and minerals such as clay minerals, zeolites, calcite, quartz, feldspar, plagioclase, dolomite, and fluorite. In particular, it has been found that clay minerals such as smectite and illite contain appreciable amounts of lithium.
To date, there does not appear to be any widely used method of extracting lithium from sedimentary clays. While CN103849761A discloses a method of lithium extraction from clays, the method still relies on costly and rate limiting pyrometallurgical processes similar to those used in processing of silicate ores such as spodumene. What is needed is an economical, efficient way to extract lithium from sedimentary clays.
In accordance with one aspect of the invention, there is provided a method of extracting lithium from sedimentary rock to produce lithium sulfate brine. The method includes the steps of sizing sedimentary rock, suspending the sized sedimentary rock in an aqueous solution, and separating the aqueous solution into lithium bearing slurry and low lithium containing coarse gangue. The lithium bearing slurry is then treated with an acid, dissolving lithium from the sedimentary rock and forming first precipitates, and the first precipitates are separated from the lithium bearing slurry, forming an acidic lithium sulfate solution. The pH of the acidic lithium sulfate solution is then modified to a pH of between approximately 4 and approximately 8, resulting in the formation of second precipitates, which are then separated from the neutralized lithium sulfate solution.
The neutralized lithium sulfate solution is then crystallized, forming magnesium sulfate crystals and magnesium-potassium sulfate crystals which are also separated, resulting in a neutralized lithium sulfate mother liquor. The neutralized lithium sulfate mother liquor is then treated with calcium hydroxide or quicklime (calcium oxide), soda ash, and oxalic acid forming third precipitates that are then separated from the liquor and recycled to the neutralization step. Finally, the resultant magnesium-free lithium sulfate mother liquor is processed through multiple resin beds to further remove contaminants via ion exchange, forming a purified lithium sulfate brine solution. The lithium sulfate brine may subsequently be processed into lithium carbonate or lithium hydroxide monohydrate.
In a preferred embodiment, the aqueous sedimentary rock is separated into lithium bearing slurry and gangue through the use of an attrition scrubber. Separately, the lithium slurry is preferably treated with sulfuric acid in segmented attack tank reactors. Precipitates formed in the attack tank reactors, as well as any undissolved solids, are preferably removed via pressure filtration. It has been determined that by using the above method, lithium sulfate brine can be extracted efficiently and economically from sedimentary clays.
In another aspect, a method of extracting and concentrating lithium from sedimentary rock comprises the steps of suspending the sedimentary rock in an aqueous solution; treating the aqueous solution to dissolve lithium and form first precipitates; filtering the aqueous solution to remove the first precipitates; neutralizing the aqueous solution to form second precipitates and removing the second precipitates; crystallizing the aqueous solution to form sulfate crystals and removing the sulfate crystals; and treating the aqueous solution with one or more cation precipitating agents to form third precipitates and removing the third precipitates.
In still another aspect, a method of extracting purified lithium sulfate brine from sedimentary rock comprises the steps of sizing the sedimentary rock; suspending the sized sedimentary rock in an aqueous solution; separating the aqueous solution into lithium bearing slurry and gangue; treating the lithium bearing slurry to form first precipitates; separating the first precipitates and sedimentary rock from the lithium bearing slurry to form a lithium sulfate filtrate solution; modifying a pH of the lithium sulfate filtrate solution to form second precipitates and a neutralized lithium sulfate solution; separating the second precipitates from the neutralized lithium sulfate solution; crystallizing the neutralized lithium sulfate solution to form sulfate crystals and a neutralized lithium sulfate mother liquor solution; separating the sulfate crystals from the neutralized lithium sulfate mother liquor solution; treating the neutralized lithium sulfate mother liquor solution to form third precipitates and a lithium sulfate solution; separating the third precipitates from the lithium sulfate solution; and treating the lithium sulfate solution to form a purified lithium sulfate brine.
The disclosed invention covers a method of extracting and concentrating lithium from sedimentary rock. The method includes the steps of sizing sedimentary rock, suspending the sized sedimentary rock in an aqueous solution, and separating the aqueous solution into lithium bearing slurry and gangue. The lithium bearing slurry is then treated with an acid, dissolving lithium from the sedimentary rock and forming first precipitates. The first precipitates are separated from the lithium bearing slurry, forming an acidic lithium sulfate solution. The pH of the acidic lithium sulfate solution is then modified to a pH between approximately 4 and approximately 8, resulting in the formation of second precipitates, which are then separated from the neutralized lithium sulfate solution.
The neutralized lithium sulfate solution is then crystallized, forming magnesium sulfate crystals and magnesium-potassium sulfate crystals which are separated from the solution, resulting in a neutralized lithium sulfate mother liquor. The neutralized lithium sulfate mother liquor is then treated with calcium hydroxide or quicklime (CaO), soda ash, and oxalic acid, forming third precipitates that are then separated from the lithium sulfate mother liquor, forming a magnesium-free lithium sulfate solution. The third precipitates, alkaline in nature, are recycled in the process and used to neutralize acidic lithium sulfate solution. Finally, the magnesium-free lithium sulfate solution is processed through multiple resin beds to further remove contaminants via ion exchange, forming a purified lithium sulfate brine solution that can be used to produce lithium carbonate or lithium hydroxide monohydrate.
The disclosed invention contemplates the extraction of lithium ore from various types of sedimentary rock. The method of extraction is not critical to the invention and can be accomplished through known methods in the art, such as methods used in the phosphate, coal, or clay industries whereby ore is slurried and classified to remove gangue. In one embodiment, the ore is extracted from sedimentary rock containing detrital material and several minerals typical of sedimentary basins, including clay minerals (illite, smectite, etc.) and zeolites. Preferably, the ore is extracted from sedimentary rock containing 100 ppm to 20,000 ppm lithium. More preferably, the ore is extracted from smectite/hectorite clay with a concentration greater than 2,000 ppm lithium. Most preferably, the mined ore is extracted from sedimentary rock containing an illite-type clay with a concentration of greater than 8,000 ppm lithium.
A preferred process for ore preparation is depicted in
Once the sedimentary rock ore 101 is appropriately sized, the material is fed to an attrition scrubber 103. An attrition scrubber is an agitated vessel whereby water 104 is added to the sized sedimentary rock ore 101, forming a slurry. A high-speed agitator causes slurry particles to impact one another, thereby creating a scrubbing effect between particles. The disclosed invention not only uses an attrition scrubber to scrub lithium bearing particles from larger non-lithium bearing particles, but it also uses an attrition scrubber for particle comminution. By exploiting differences in breakage characteristics between lithium and low lithium bearing particles, the attrition scrubber reduces lithium bearing particles to a size fraction less than approximately 100 microns, while harder low lithium bearing particles remain in a size fraction larger than approximately 100 microns. The attrition scrubber is tuned to maximize size reduction of lithium bearing particles by controlling slurry wt. % solids, retention time, and agitator tip speed, which may vary for different ore types and lithium concentrations. Slurry wt. % solids ranges from 10 wt. % to 40 wt. %, retention time ranges from 5 minutes to 30 minutes, and agitator tip speed ranges from 200 to 2,000 feet per minute. The amount of stages contained in the attrition scrubber 103 is dependent on the characteristics of the sized sedimentary rock ore 101 being processed.
As the sedimentary rock is processed through the attrition scrubber, the rock is reduced to a water-based slurry containing lithium bearing fine particles and low lithium containing coarse gangue particles. The gangue is then separated from the slurry through classification methods known in the art such as wet screening and hydrocycloning. Classification by wet screening is preferably accomplished through the use of one or more vibrating screens 105, whereas classification by hydrocycloning is accomplished through one or more stages using a hydrocyclone cluster 106 comprising one or more hydrocyclones. Preferably, hydrocyclone clusters 106 are configured to separate gangue coarser than 100 microns from smaller lithium bearing particles but may be configured to separate particles as small as 30 microns. The hydrocyclone underflow containing the coarse gangue from the final stage of classification is then discarded or stored in a tailings or waste rock storage area 107.
In the event that lithium bearing sedimentary clay is still present in the gangue, the coarse gangue can be recycled back to the attrition scrubber or sent to a regrind or crushing circuit utilizing size reduction equipment to liberate the softer sedimentary clay from the coarse gangue. The regrind or crushing equipment could include equipment known in the art such as high-pressure grinding rolls (HPGR) 108, impact crushers, autogeneous grinding mills, or semi-autogenous grinding mills. Following size reduction, the coarse gangue is returned to the attrition scrubber 103. The hydrocyclone overflow containing the lithium bearing slurry is thickened in a standard process thickener or paste thickener 109 with flocculating and coagulating polymers to 20 wt. % to 55 wt. % solids. Preferably, the flocculants are anionic polyacrylamides, while the coagulants are organic polyamines. The resulting thickened ore slurry 110 is then sent to the lithium dissolution circuit 200, while the overflow from the thickener 109 is recycled back to the attrition scrubber 103 to slurry new ore.
A flow chart depicting the lithium dissolution circuit 200 is shown in
As the slurry is treated, acid 203 is added to one or more reactors to maintain an excess sulfuric acid concentration ranging from 10 to 50 g/L in the aqueous phase; however, the ideal sulfate concentration may change based on lithium bearing slurry characteristics such as the concentration of sulfuric acid consumers such as calcium and magnesium. Water or dilute aqueous lithium solutions from downstream processing may also be added to control slurry wt. % solids in the reactor. Preferably, excess acid concentration is monitored by acid-base or thermometric titration, however other monitoring methods known in the art may be used. Preferably, slurry wt. % is monitored by radiometric sensor; however, other monitoring methods known in the art may be used. Other parameters that are used to control the lithium dissolution process in the attack tank reaction circuit include acid addition rate, filtrate recirculation rate, slurry recirculation rate, retention time, and reaction temperature. The sulfuric acid 203 addition rate ranges from 100 kg to 600 kg of sulfuric acid per dry tonne of lithium bearing fine particles feeding the attack circuit, the overall retention time ranges from 3 hours to 8 hours, the reaction temperature ranges from 20° C. to 90° C., with a preferred temperature of approximately 80° C., and wt. % solids ranges from 20 wt. % to 50 wt. %. Preferably, reaction temperature is controlled by heat transfer from steam 205. Acidic lithium bearing filtrate and acidic slurry may be recycled to the lithium dissolution circuit to increase the concentration of lithium and reduce overall acid consumption; however, lithium concentration in the aqueous phase is maintained below the solubility limit of lithium sulfate double salts, specifically, the lithium-potassium sulfate double salt.
After the ore slurry 110 is passed through a first attack tank reactor 201, where slurry temperature after acid addition is maintained at approximately 80° C., the slurry may be passed through one or more additional attack tank reactors. Variations in the operating parameters, including the amount of attack tank reactors 201 are dependent upon the characteristics of the ore slurry 110. Commercially available systems useful in this step are those such as systems manufactured by Jacobs Engineering Systems.
The attack tank treatment depicted in
The acidified slurry 212 is added to filter press feed tank of the pressure filtration circuit, where the slurry is heated to 82° C. if not already up to temperature as a result of processing in the lithium dissolution circuit. The acidified slurry 212 is then pumped to the recessed chamber membrane filter press until the filter press chambers are filled with filter cake. After filter press is filled with cake, the filter cake is hydraulically squeezed with hot water at a pressure ranging from 400 kPa(g) to 2,000 kPa(g), and preferably 600 kPa(g) to 1800 kPa(g). While the filter cake is squeezed, recycled water 302 from elsewhere in the process is pumped through the filter cake thereby washing residual lithium and acidity from the filter cake,
The neutralization 400 of the acidic lithium filtrate solution 304 is depicted in
As the acidic lithium filtrate 300 is neutralized, contaminants such as iron, aluminum, and manganese are precipitated from the solution. In a preferred embodiment, compressed air 402 is added to the neutralization reactors 405 and 407 to promote the oxidation and subsequent precipitation of contaminates. The contaminants are recirculated with a thickener 411 to increase solid density. The thickened slurry is purged to a pressure filtration system 413 that is similar in design and operation to the method for pressure filtration of acidified slurry 212. Pressure filtration results in the formation of a contaminants filter cake, which is washed and discarded similarly to the method for pressure filtration of acidified slurry 212. The overflow from the neutralization thickener 411 and the filtrate from pressure filtration 413 are then combined to produce a neutralized lithium sulfate solution 414 and sent to magnesium sulfate and magnesium-potassium sulfate crystallization 500 for removal of magnesium sulfate and as much potassium as possible as a magnesium-potassium sulfate salt.
The crystallization of the neutralized lithium sulfate solution 414 is depicted in
The resulting lithium sulfate mother liquor 503 from crystallization 501 is further processed to remove any remaining magnesium. Preferably, the mother liquor 503 is fed into a grinding mill slaker 505 where a pH modifier, preferably quicklime (CaO) 404, is added. The grinding mill slaker 505, ensures a high utilization of calcium oxide despite the presence of sulfate. In addition to quicklime (CaO) 404, overflow from the magnesium precipitation thickener 515 and recycled water 302 is also added to the grinding mill slaker 505 to facilitate the slaking process. Next, the slaked mother liquor 503 is fed into one or more magnesium precipitation reactors 509, where cation precipitating agents and pH modifiers are added to precipitate magnesium hydroxide, magnesium sulfate, calcium sulfate, calcium oxalate, and magnesium/calcium carbonates. Preferred pH modifiers include soda ash solution 511, while preferred cation precipitating agents include soda ash solution 511 and oxalic acid 513. Preferably, this results in the pH of the mother liquor 503 being increased to above 11, resulting in a mixed slurry of magnesium hydroxide, magnesium sulfate, calcium sulfate, calcium oxalate, and magnesium/calcium carbonates. The number of precipitation reactors 509 utilized is dependent on the quality of the ore that is initially mined. Similar to neutralization 400, the precipitants are recirculated with a thickener 515 to increase density of the underflow. The thickened slurry is purged to a pressure filtration system 517 (not shown) that is similar in design and operation to the method for pressure filtration of acidified slurry 212. Pressure filtration results in the formation of an alkaline filter cake 518, which is used for neutralization of acidic lithium filtrate 304. The overflow from the thickener 515 and the filtrate from pressure filtration system 517 are then combined to produce a magnesium-free lithium sulfate solution 519 that is sent to ion exchange cation removal resin beds 520.
To remove trace concentrations of divalent cations, magnesium-free lithium sulfate solution 519 is passed through a series of ion exchange cation removal resin beds 520. As the liquor is processed through the resin beds, cation contaminants not completely removed by the precipitation process such as magnesium, calcium, and iron are removed by ion exchange. The process is sequential (loading, regeneration, settling), and requires multiple resin beds operating in parallel to ensure removal of the target elements, and maintain a roughly continuous flow of finished lithium sulfate brine. Preferably, ion exchange cation removal resin beds 520 are either batch or carousel systems with a lead-lag arrangement. Preferably, the resins utilize a divinyl-benzene crosslinked microporous resin with either sulfate or a chelating group. Additionally, a sodium chloride and/or sodium hydroxide solution 521 and hydrochloric acid solution 522 may be used for resin regeneration and stripping. Contaminants removed by the ion exchange resin are discarded. The amount of pressure filters 517 and ion exchange cation removal resin beds 520 utilized is dependent on the quality of the ore that is initially mined.
The resulting purified lithium sulfate brine 523 can then be processed to multiple end products. The most commercially important end products are lithium hydroxide monohydrate and lithium carbonate. Both can be produced directly from the purified lithium sulfate brine 523 at a quality that can be used for the energy storage industry, pharmaceutical, grease, and glass industries.
Although the invention has been described by reference to its preferred embodiment as is disclosed in the specification and drawings identified above, many more embodiments of the invention are possible without departing from the invention. Thus, the scope of the invention should be limited only by the appended claims.
The present application is a continuation of U.S. patent application Ser. No. 17/442,961, filed on Sep. 24, 2021, which is a national stage entry of PCT Application No. PCT/US2020/024152, filed Mar. 23, 2020, which claims the benefit of U.S. Provisional Application No. 62/826,107, filed Mar. 29, 2019, each of which is hereby specifically incorporated by reference herein in its entirety.
Number | Date | Country | |
---|---|---|---|
62826107 | Mar 2019 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 17442961 | Sep 2021 | US |
Child | 18890246 | US |