Information
-
Patent Grant
-
6358456
-
Patent Number
6,358,456
-
Date Filed
Friday, April 16, 199925 years ago
-
Date Issued
Tuesday, March 19, 200222 years ago
-
Inventors
-
Original Assignees
-
Examiners
Agents
-
CPC
-
US Classifications
Field of Search
US
- 264 267
- 264 2711
- 264 273
- 264 274
- 264 275
- 264 279
- 264 268
- 425 1291
- 428 664
- 428 666
- 428 357
-
International Classifications
- B29C7514
- B29C7074
- B29C7080
-
Abstract
A secondary molding body in which shrinkage and weld formation is avoided. Resin is molded within an annular molding portion (31) provided at a primary molding body (10) to form a secondary molding body integrally with the primary molding body thereby to form a molding body. The annular molding portion (31) is provided with a gate opening (33) and an overflow opening (34) with two flow paths therebetween. One of the two resin flow paths (31a and 31b) is set to be longer in the flowing distance and/or flowing resistance than the other of the two flow paths. The overflow opening (34) is arranged in a manner that the distance of the overflow opening (34) facing the one flow path having the larger flowing distance and/or flowing resistance is made longer than the distance thereof facing the other flow path. Thus, the flowing distances and/or flowing resistances of the flow paths (31a and 31b) flowing toward left and right direction within the annular molding portion (31) are made substantially same, so that the resin flowing through the two flow paths joins at the overflow opening (34) and then flow out of the overflow opening.
Description
BACKGROUND OF THE INVENTION
1. Field of the Invention
The present invention relates to a molding body and the fabricating method thereof in which resin is supplied to the annular molding portion of a primary molding body thereby to form a secondary molding body integrally with the primary molding body.
2. Discussion of Related Art
In the case of fabricating a molding body by forming a packing as a secondary molding body integrally with a primary molding body, the molding body is formed in a manner that an annular molding portion is formed on the primary molding body and then fused elastomer is injected in the annular molding portion by using the primary molding body as a drag or female mold.
FIGS. 8
to
11
are diagrams showing the conventional method of fabricating such a molding body. An annular molding portion
2
, shown in
FIGS. 10 and 11
, is formed on the bottom surface of a primary molding body
1
. The annular molding portion
2
is formed in such a manner that erected wall portions
3
are provided in an opposed state on the bottom surface of the primary molding body
1
to form the annular molding portion
2
between the erected wall portions
3
. The annular molding portion
2
is provided with a gate opening (not shown) for injecting the fused elastomer (fused resin) within the annular molding portion
2
and is also provided with an overflow opening
4
for allowing the fused resin to flow out of the annular molding portion. The overflow opening
4
is located on the opposite side of the gate opening so that the tip end portion of the fused resin injected into the annular molding portion from the gate opening flows out through the overflow opening so that the fused resin is filled entirely within the annular molding portion
2
.
In the case of forming such a molding body
8
, the bottom surface of the primary molding body
1
is brought into contact with a die or metal mold and the fused resin is injected through the gate opening into the annular molding portion
2
. The injected fused resin
6
is divided into two flow paths within the annular molding portion
2
, one flowing in the left direction from the gate and the other flowing in the right direction from the gate. Then, as shown by arrows
6
in
FIG. 10
, the two paths of resin join at the overflow opening
4
from the left and right direction. Thereafter, the tip portion of the fused resin flows out from the overflow opening
4
. Once the resin has flowed out through the opening
4
, it is determined that the annular molding portion
2
has been filled entirely with the fused resin. Thereafter, the fused resin is cooled so that the elastomer with elasticity is formed.
In
FIG. 11
, a reference numeral
7
depicts an elastomer serving as a secondary molding body formed in the annular molding portion
2
. When the elastomer
7
is integrally formed with the annular molding portion
2
in this manner, the fabrication of the molding body
8
is completed. After the fabrication of the mold body as described above, the resin that overflowed through the opening
4
is cut and removed.
FIG. 9
is a diagram showing the state where the molding body
8
fabricated in this manner is attached to a unit or device
5
. When the molding body
8
and the unit
5
are pressed to each other, the elastomer
7
closely contacts the unit
5
, so that the elastomer
7
serves as a packing for establishing a seal between the molding body
8
and the unit
5
.
According to such a molding method, in order to ensure a proper seal, the overflow opening
4
cannot be formed so that it is flush with the bottom surface of the primary molding body
1
. Thus, a gas pocket is likely generated at the time of molding the fused resin, so that the fused resin cannot flow smoothly within the annular molding portion
2
due to the presence of the gas pocket. Further, when the length of the two flow paths from the injection gate to the overflow opening
4
differ from each other, the two flowpaths will merge together at a location that is displaced from the overflow opening
4
. As a result, the resin
6
flowing through the two paths cannot flow smoothly through the overflow opening
4
. If such a phenomenon occurs, shrinkage of the resin
7
results and welds are generated, so that the intensity of the drawing tension of the secondary molding body is degraded. As a result, the secondary molding body is likely to be cut. Further, as shown by a circle
9
in
FIG. 11
, there arises a problem that the close adherence between the erected wall portions
3
and the elastomer
7
can not be achieved.
SUMMARY OF THE INVENTION
Accordingly, an object of the present invention is to provide a molding body and a fabricating method thereof in which the secondary molding body, which is integrally formed with a primary molding body, does not experience shrinkage or the generation of welds. Another object is to ensure that the leading end of the resin flows through an overflow opening so that the secondary molding body is completely formed.
In order to achieve the aforesaid objects, the molding body of the present invention is characterized in that resin is molded within an annular molding portion provided on a primary molding body to form a secondary molding body integrally with the primary molding body. According to the invention, the annular molding portion is provided with a gate opening and an overflow opening and defining two flow paths therebetween. One of the paths is set to have a larger flowing distance and/or resistance than the other flow path, and the overflow opening is arranged in a manner that a length of the overflow opening facing the flow path having the larger flowing distance and/or flowing resistance is made larger than a length thereof facing on the other flow path.
In the present invention, since the overflow opening is arranged in this manner, the resin of the two flow paths can surely join at the overflow opening and then flow out of the overflow opening even when the flowing distances and/or flowing resistances of the two flow paths of the resin differ from each other. Thus, shrinkage of the resin and generation of welds in the resin are avoided. Thus, the intensity of the drawing tension is not reduced. Further, since a gas pocket is prevented from being generated, it is not necessary to lower the overflow opening to the bottom surface of the primary molding portion in order to prevent the generation of the gas pocket, so the resin can surely perform the sealing property.
According to the invention, the secondary molding body is made of elastomer. Therefore, when the elastomer has been molded, the resulting secondary molding body is elastic, so that the secondary molding body can function as a seal with the unit or the like.
The method of fabricating a molding body is further characterized in that the molding body is formed in a manner that flowing distances and/or flowing resistances of two flow paths of the resin from the gate opening to the overflow opening are adjusted to be substantially the same. Therefore, the resin of the two flow paths can surely join at the overflow opening and then flow out through the overflow opening. Therefore, the molding can be performed without generating shrinkage and welds in the resin.
BRIEF DESCRIPTION OF THE DRAWINGS
FIG. 1
is a perspective view of a built-in connector type casing serving as a primary molding body according to an embodiment of the present invention;
FIG. 2
is a bottom plan view of the built-in connector type casing;
FIG. 3
is a front view of a gate opening provided at an annular molding portion;
FIG. 4
is a front view of an overflow opening provided at the annular molding portion;
FIG. 5
is a sectional view of the annular molding portion showing the flow of resin;
FIG. 6
is a sectional view of the built-in connector type casing taken along a line
6
—
6
in
FIG. 2
;
FIG. 7
is an enlarged sectional view of a portion C in
FIG. 6
;
FIG. 8
is a front view of an overflow opening of a conventional annular molding portion;
FIG. 9
is a sectional view showing a state where a molding body is brought into contact with a unit;
FIG. 10
is a sectional view of the conventional annular molding portion showing the flow of resin flowing therein; and
FIG. 11
is a sectional view of an elastomer formed by the conventional method.
DETAILED DESCRIPTION OF THE INVENTION
The present invention will be explained concretely with reference to
FIGS. 1
to
7
.
FIG. 1
is a perspective view of a primary molding body according to an embodiment of the present invention,
FIG. 2
is a bottom plan view thereof, and
FIGS. 3 and 4
are diagrams showing a gate opening and an overflow opening, respectively.
The primary molding body according to the embodiment of the present invention is a built-in connector type casing
10
which includes a main body
13
having a substrate attachment portion
11
and a connector portion
12
. A lid body (not shown) covers the substrate attachment portion
11
of the main body
13
.
The substrate attachment portion
11
includes a hood portion
14
, over which the lid body is placed and to which a substrate (not shown), such as a printed circuit board, is attached, and a cylindrical portion
15
integrally and continuously provided at the lower portion of the hood portion
14
. A plurality of recess portions
16
are formed within the hood portion
14
and projection terminals
17
are disposed within the recess portions
16
. A portion of a bus bar is formed within the hood portion
14
and is exposed in a linear manner to form terminal portion
18
. The bus bar is insert molded in the substrate attachment portion
11
and the connector portion
12
when they are formed. The terminal portion
18
is connected by means of a wire bonding to a pattern formed on a substrate which is attached to the substrate attachment portion
11
.
The connector portion
12
is integrally formed with the substrate attachment portion
11
so as to extend from the side wall on the rear of the substrate attachment portion
11
. The connector portion
12
is coupled with the substrate attachment portion
11
by means of an interconnection portion
19
provided therebetween. When a partner side connector (not shown) is fitted into the connector portion
12
, the connector portion is electrically connected with the partner side connector. In order to perform such an electrical connection, the connector portion
12
is provided with a cylindrical connector insertion opening
20
directed to the substrate attachment portion
11
side into which the partner side connector fits. A plurality of contact terminals
21
, serving as one terminal of the bus bar, are disposed within the connector insertion opening
20
.
Such a built-in connector type casing
10
is fixed to a panel of an automobile (not shown) in a state that the elastomer, serving as a secondary molding body, is molded as described later. In order to fix the built-in connector type casing to the panel, fixing portions
22
to be fixed to the panel are integrally formed on the cylindrical portion
15
of the substrate attachment portion
11
and on the connector portion
12
.
As shown in
FIG. 2
, the projection terminals
17
, provided in the hood portion
14
, are exposed on the bottom side of the casing
10
. In order to electrically insulate the exposed portions of the projection terminals
17
, the cylindrical portion
15
is provided with an annular molding portion
31
for surrounding the exposed portions of the projection terminals
17
. The annular molding portion
31
is formed by providing erected wall portions
32
,
32
on the bottom surface of the cylindrical portion
15
so as to be opposed to each other, as shown in FIG.
5
. The lower end surface of the annular molding portion
31
is opened as shown in
FIGS. 6 and 7
.
According to one embodiment, fused resin is supplied within the annular molding portion
31
and molded thereby to form the secondary molding body serving as a packing which is integral with the primary molding body
10
. In order to supply the fused resin to the annular molding portion
31
, a gate opening
33
for injecting the fused resin within the annular molding portion is provided at the one end side of the annular molding portion
31
. Further, an overflow opening
34
is provided at the opposite side of the gate opening
33
. The resin may be one having elasticity around the room temperature, and so resin such as synthetic rubber, polyisobutylene, polyethylene or the like may be employed as the resin.
The molding operation for forming the secondary molding body can be performed in a manner that the built-in connector type casing
10
, serving as the primary molding body mold, contacts a female mold (not shown). That is, first, the bottom surface of the cylindrical portion
15
of the casing is brought into close contact with the female mold. In this state, the resin
35
is injected through the gate opening
33
within the annular molding portion
31
. The injected resin
35
is then divided into two flow paths, one flowing to the left in the annular molding portion
31
and one flowing to the right. Then, as shown in
FIG. 5
, the flowpaths of the fused resin are joined at the overflow opening
34
, whereupon the fused resin flows out through the overflow opening
34
. When the resin is molded in this manner, the fused resin
35
fills the annular molding portion
31
so as to form an elastomer (secondary molding body)
36
having elasticity, which can serve as a packing.
According to the invention, the flowing distances and/or flowing resistances of the two flow paths from the gate opening
33
to the overflow opening
34
are adjusted to be substantially the same. In this particular embodiment, as shown in
FIG. 2
, one flow path
31
a
of the two flow paths is set to be longer than the other flow path
31
b
. However, referring to
FIG. 4
, the overflow opening
34
is arranged to shift a side of the flow path
31
a
in such a manner that an opening of the overflow opening
34
opens toward the flow path
31
a
. As a consequence, the distances of the two flow paths
31
a
and
31
b
within the annular molding portion
31
are made substantially same, so that the fused resin
35
flowing in the flow paths are surely joined at the overflow opening
34
portion and then flow out of the overflow opening
34
.
Accordingly, shrinkage and welds are prevented from being generated at the elastomer
36
thus molded. Thus, the elastomer
36
can be prevented from being reduced in the intensity of its drawing tension and further the elastomer
36
can be prevented from being cut. Further, since the shrinkage and weld are prevented from being generated, as shown in
FIG. 7
, the elastomer
36
can be surely filled within the annular molding portion
31
and closely contact the erected wall portions
32
. Therefore, the elastomer
36
is securely retained, and the elastomer can surely perform the sealing even when it is brought into contact with the unit
5
(see FIG.
9
). Further, since a gas pocket is prevented from being generated, the fused resin
35
can flow within the annular molding portion
31
smoothly. As a result, it is not necessary to lower the overflow opening
34
so that it is flush with the bottom surface of the cylindrical portion
15
in order to prevent the generation of the gas pocket, and so the elastomer
36
can surely perform the sealing property.
In the aforesaid embodiment, the flowing distances of the two flow paths of the resin flowing toward left and right direction within the annular molding portion
31
are adjusted to be substantially the same. However, in the case where the flowing resistances of the two flow paths of the resin flowing toward left and right direction differ to each other, for example, when the flowing resistance of the flow path
31
a
is larger than that of the flow path
31
b
due to the fact that there is a narrow portion(s) or many bent portions at the flow path
31
a
or the flow path
31
b
is inclined downward rather than the flow path
31
a
, the flowing resistances of the two flow paths
31
a
and
31
b
can be made substantially same by making the length of the overflow opening
34
facing on the flow path
31
a
larger than the length thereof facing on the flow path
31
b
. As a result, it is possible to mold the elastomer without generating shrinkage or welds. Further, the resin supplied to the annular molding portion
31
may be resin other than an elastomer.
Claims
- 1. A molding body comprising:a primary molding body; a secondary molding body formed integrally from the primary molding body; and an annular molding portion provided on said primary molding body for molding resin therein, said annular molding comprising: a gate opening for injecting the resin; and an overflow opening for ejecting excess resin, wherein two different flow paths fluidly connect said gate opening and said overflow opening, such that a first one of said flow paths is longer than a second one of said flow paths, and wherein said overflow opening is arranged in a manner that a length of said overflow opening facing said first flow path is greater than a length of said overflow opening facing said second flow path such that the flow paths are one of the same length and the same flow resistance.
- 2. In the molding body of claim 1, wherein said secondary molding body is made of an elastomer.
- 3. A method of fabricating a molding body, comprising the following steps:providing a primary mold body having an annular molding portion therein, said annular molding portion having a gate opening at one location and an overflow opening at another portion, and two flow paths defined therebetween, wherein a distance of a first one of said flow paths is greater than a distance of a second of said flow paths and said overflow opening is arranged in a manner that a length of said overflow opening facing said first flow path is greater than a length of said overflow opening facing said second flow path; and injecting resin into said gate opening, thereby causing the resin to flow in the two flow paths and to join at said overflow opening formed in said annular molding portion and overflow therefrom, such that a secondary molding body is integrally molded with said primary molding body.
- 4. The method of claim 3, wherein said resin is an elastomer.
- 5. A molding body comprising:a primary molding body; a secondary molding body formed integrally from the primary molding body; and an annular molding portion provided on said primary molding body for molding resin therein, said annular molding portion having a gate opening for injecting the resin and an overflow opening for ejecting excess resin, wherein two flow paths are defined between the gate opening and the overflow opening, and wherein the overflow opening is positioned to adjust the flow paths to one of the same length and the same flow resistance.
- 6. In the molding body of claim 5, wherein said secondary molding body is made of an elastomer.
- 7. A method of fabricating a molding body, comprising the following steps:providing a primary mold body having an annular molding portion therein, said annular portion having a gate opening at one location and an overflow opening at another portion and two different flow paths defined therebetween, wherein the flow paths are adjusted by the overflow opening such that the flow paths are one of the same length and the same flow resistance; and injecting resin into said gate opening, thereby causing the resin to overflow from said overflow opening formed in said annular molding portion such that a secondary molding body is integrally molded with said primary molding body.
- 8. The method of claim 7, wherein said resin is an elastomer.
Priority Claims (1)
Number |
Date |
Country |
Kind |
10-106555 |
Apr 1998 |
JP |
|
US Referenced Citations (12)