The inventive subject matter generally relates to turbine engine components, and more particularly relates to nickel-based superalloys for manufacturing turbine engine components, such as turbine blades.
Turbine engines are used as the primary power source for various kinds of aircraft. The engines may also serve as auxiliary power sources that drive air compressors, hydraulic pumps, and industrial electrical power generators. Most turbine engines generally follow the same basic power generation procedure. Compressed air is mixed with fuel and burned, and the expanding hot combustion gases are directed against stationary turbine vanes in the engine. The vanes turn the high velocity gas flow partially sideways to impinge onto turbine blades mounted on a rotatable turbine disk. The force of the impinging gas causes the turbine disk to spin at high speed. Jet propulsion engines use the power created by the rotating turbine disk to draw more air into the engine, and the high velocity combustion gas is passed out of the gas turbine aft end to create forward thrust. Turbine engines are also used to drive one or more propellers, electrical generators, or other devices.
Turbine engine blades and vanes are fabricated from high temperature materials such as nickel-based superalloys. Although nickel-based superalloys have good high temperature properties and many other advantages, they may be susceptible to corrosion, oxidation, thermal fatigue, and erosion damage in the harsh environment of an operating turbine engine. These limitations may be undesirable as there is a constant drive to increase engine operating temperatures in order to increase fuel efficiency and to reduce emission. Replacing damaged turbine engine components made from nickel-based superalloys may be relatively expensive. Hence, significant research is being performed to find cost-effective ways to improve the temperature properties of these components.
Accordingly, there is a need for methods and materials for improving turbine engine components such as turbine blades and vanes. There is a particular need for environment-resistant materials that will improve a turbine component's durability. Furthermore, other desirable features and characteristics of the inventive subject matter will become apparent from the subsequent detailed description of the inventive subject matter and the appended claims, taken in conjunction with the accompanying drawings and this background of the inventive subject matter.
Nickel-based superalloys, turbine blades, and methods of manufacturing turbine blades are provided.
In an embodiment, by way of example only, a nickel-based super alloy includes, by weight, about 1.5% to about 5.5% chromium, about 8% to about 12% aluminum, about 4% to about 8% tantalum, about 1.5% to about 5.5% tungsten, less than about 1% of one or more of elements selected from a group consisting of carbon, boron, zirconium, yttrium, hafnium, and silicon, and a balance of nickel.
In another embodiment, by way of example only, a nickel-based super alloy includes, by weight, about 1.5% to about 5.5% chromium, about 8% to about 12% aluminum, about 4% to about 8% tantalum, about 1.5% to about 5.5% tungsten, less than about 1% total combined weight of each of the following elements: carbon, boron, zirconium, yttrium, hafnium, and silicon, wherein each of the said elements is present in an amount greater than 0.01%, and a balance of nickel.
In still another embodiment, by way of example only, a method of manufacturing a turbine blade includes applying a nickel-based superalloy over an area of the blade, the nickel-based-superalloy including, by weight, about 1.5% to about 5.5% chromium, about 8% to about 12% aluminum, about 4% to about 8% tantalum, about 1.5% to about 5.5% tungsten, less than about 1% of one or more of elements selected from a group consisting of carbon, boron, zirconium, yttrium, hafnium, and silicon, and a balance of nickel.
This summary is provided to introduce a selection of concepts in a simplified form that are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.
The inventive subject matter will hereinafter be described in conjunction with the following drawing figures, wherein like numerals denote like elements, and
The following detailed description is merely exemplary in nature and is not intended to limit the invention or the application and uses of the invention. As used herein, the word “exemplary” means “serving as an example, instance, or illustration.” Thus, any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments. Furthermore, as used herein, numerical ordinals such as “first,” “second,” “third,” etc., such as first, second, and third components, simply denote different singles of a plurality unless specifically defined by language in the appended claims. All of the embodiments and implementations of the stator airfoil assemblies and methods for the manufacture thereof described herein are exemplary embodiments provided to enable persons skilled in the art to make or use the invention and not to limit the scope of the invention, which is defined by the claims. Furthermore, there is no intention to be bound by any expressed or implied theory presented in the preceding technical field, background, brief summary, or the following detailed description.
An improved, nickel-based superalloy is provided that has superior elevated-temperature properties over those of conventional superalloys. In an embodiment, the nickel-based superalloy has improved oxidation-resistance when exposed to engine operating temperatures, such as turbine inlet temperatures greater than about 2200° F. (1205° C.). In an example, the nickel-based superalloy may have improved properties, such as resistance to creep, oxidation, thermal fatigue, and other hazards when used for high pressure turbine (HPT) components such as turbine blades and vanes.
In an embodiment, the base material 202 comprises a first nickel-based superalloy. For example, the first nickel-based superalloy may be selected from a high performance nickel-based superalloy, including, but not limited to IN792, C101, MarM247, Rene80, Rene125, ReneN5, SC180, CMSX 4, and PWA1484. The base material 202 may have a single crystal microstructure, in an embodiment. In other embodiments, the base material 202 may comprise a directionally solidified or an equiaxed microstructure.
The enhanced portion 204 includes a second nickel-based superalloy having a composition that may or may not be different than the composition of the first nickel-based superalloy. Generally, in an embodiment, the second nickel-based superalloy includes elements selected from nickel, chromium, aluminum, tantalum, hafnium, silicon, and yttrium. In other embodiments, in addition to the previously-mentioned elements, the second nickel-based superalloy may include one or more elements selected from carbon, boron, and zirconium. In yet another embodiment, the nickel-based superalloy further may include tungsten. In still another embodiment, the nickel-based superalloy may include incidental impurities (e.g., trace amounts of additional elements that are not intentionally included in the composition), but does not include other elements other than those listed previously.
In accordance with an embodiment, the second nickel-based superalloy includes, by weight, about 1.5% to about 5.5% chromium, about 8% to about 12% aluminum, about 4% to about 8% tantalum, about 0.05% to about 0.25% hafnium, about 0.01% to about 0.05% yttrium, about 0.1% to about 0.5% silicon, about 1.5% to about 5.5% tungsten, and a balance of nickel. In still another embodiment, the second nickel-based superalloy optionally or additionally may include, by weight, up to about 0.1% carbon (in an amount greater than about 0.01%). In still yet another embodiment, the second nickel-based superalloy optionally or additionally may include, by weight, up to about 0.1% zirconium (in an amount greater than about 0.01%). In still yet another embodiment, the second nickel-based superalloy optionally or additionally may include, by weight, up to about 0.1% boron (in an amount greater than about 0.01%).
Chromium is included to enhance the alloy's oxidation resistance. Inclusion of aluminum promotes formation of a gamma prime strengthening phase and formation of a protective aluminum oxide layer on a surface of the enhanced portion 204. The protective oxide layer protects the outer surface of the enhanced portion 204 against oxidation. Tantalum may partition into gamma prime phase (e.g., segregate into particles within a gamma matrix of the superalloy) to improve the elevated-temperature creep and fatigue resistance properties of the nickel-based superalloy. This composition produces a single phase gamma prime (Ni3Al) phase that is strengthened with W and Ta to resist creep. The gamma prime phase has a lower coefficient of thermal expansion than the blade alloys which are a composite of gamma and gamma prime phases. The aluminum concentration at about 8 wt % to about 12 wt % is much higher than the substrate, and in combination with the other elements, will form only the gamma prime phase. In addition the higher aluminum content produces a superior thermally grown oxide (TGO) dominated by Al2O3. Elemental additions such a Zr, Y, Hf and Si are also known to improve the thermal cyclic resistance of the TGO. Further, although the strengthening elements W and Ta have previously been known in the art to be detrimental to the TGO, it has been found unexpectedly by the inventor herein that they are much less detrimental than the combination of elements use in known blade alloys.
Further, hafnium, yttrium, zirconium, and rare earth elements may improve adhesion of the protective oxide layer to the enhanced portion 204. Specifically, the hafnium atoms of the nickel-based superalloy may diffuse into grain boundaries of the aluminum oxide scale that thermally grows very slowly on the surface the nickel-based superalloy of the enhanced portion 204 so that the protective oxide layer remains relatively thin. As a result, spallation of the protective oxide layer may be minimized. Moreover, hafnium, yttrium, and/or other reactive elements such as zirconium or the rare earth elements may be included in the composition of the nickel-based superalloy to tie up the sulfur impurities that may be present in the material of the enhanced portion 204. In particular, yttrium and/or other reactive elements may react with sulfur to form stable oxysulfides or sulfides to prevent the sulfur from diffusing to the surface of the superalloy. This may also improve the adherence of a protective thin layer alumina scale to the alloy. Silicon in the nickel-based superalloy may also contribute to the adhesion protective oxide layer, which may be comprised predominately of alumina.
Carbon and boron may be included to strengthen grain boundaries that may be present in the superalloy when multiple grains are present. Total amounts of these elements are preferably minimized, because inclusion of increased quantities of these elements may adversely affect oxidation resistance at higher temperatures.
Further, in some embodiments, tungsten may be included in order to improve alloy creep strength properties of the superalloy. Tungsten is preferably minimized to less than about 5.5%, or preferably less than about 4.5%, or more preferable about 3.5% because inclusion of increased quantities of tungsten, as noted above in addition to tantalum, may adversely affect oxidation resistance at higher temperatures and alloy stability.
To further protect the turbine engine component 200 which may be exposed to the harsh operating temperatures, the protective coating system 210 is optionally included, in an embodiment.
In another embodiment, the bond coating 302 may be an overlay coating comprising MCrAlX, wherein M is an element selected from cobalt, nickel, or combinations thereof, and X is one or more elements selected from hafnium, zirconium, yttrium, tantalum, palladium, platinum, silicon, or combinations thereof. Some examples of MCrAlX compositions include NiCoCrAlY and CoNiCrAlY. In still another embodiment, the bond coating 302 may include a combination of two types of bond coatings, such as a diffusion aluminide coating formed on an MCrAlX coating. In any case, the bond coating 302 may have a thickness in a range of from about 25 microns (μm) to about 150 μm, according to an embodiment. In other embodiments, the thickness of the bond coating 302 may be greater or less.
The thermal barrier coating 304 may be formed over the bond coating 302 and may comprise, for example, a ceramic. In one example, the thermal barrier coating 304 may comprise a partially stabilized zirconia-based thermal barrier coating, such as yttria stabilized zirconia (YSZ). In an embodiment, the thermal barrier coating may comprise yttria stabilized zirconia doped with other oxides, such as Gd2O3, TiO2, and the like. In another embodiment, the thermal barrier coating 304 may have a thickness that may vary and may be, for example, in a range from about 50 μm to about 300 μm. In other embodiments, the thickness of the thermal barrier coating 304 may be in a range of from about 100 μm to about 250 μm. In still other embodiments, the thermal barrier coating 304 may be thicker or thinner than the aforementioned ranges.
The thermally-grown oxide layer 306 may be located between the bond coating 302 and the thermal barrier coating 304. In an embodiment, the thermally-grown oxide layer 306 may be grown from aluminum in the above-mentioned materials that form the bond coating 302. For example, during the deposition or a subsequent heat treatment of the thermal barrier coating 304, oxidation may occur on the bond coating 302 to result in the formation of the oxide layer 306. In one embodiment, the thermally-grown oxide layer 306 may be relatively thin, and may be less than 2 μm thick.
To manufacture a turbine engine component, a method 400, depicted in a flow diagram provided in
In another embodiment of step 402, the turbine engine component may be mechanically prepared. Examples of mechanical preparation include, for example, pre-machining and/or degreasing surfaces in order to remove any oxidation, dirt or other contaminants that may be present from previous manufacturing steps. In another embodiment, additional or different types and numbers of preparatory steps can be performed. It will be appreciated that the present embodiment is not limited to these preparatory steps, and that additional, or different types and numbers of preparatory steps can be conducted.
Once the turbine engine component has been prepared, a nickel-based superalloy in accordance with the present disclosure may be applied to, for example, the tip region of the blade, step 404, to form layer 204 as shown in
To laser-weld the nickel-based superalloy to the component, the nickel-based superalloy powder may be used in conjunction with a CO2 laser, a YAG laser, a diode laser, or a fiber laser. In an embodiment, a welding process includes laser powder fusion welding, in which the nickel-based superalloy is laser deposited onto a degraded area to restore both geometry and dimension with metallurgically sound buildup. Both automatic and manual laser welding systems are widely used to perform laser powder fusion welding processes. An exemplary manual welding repair is described in detail in U.S. Pat. No. 6,593,540 entitled “Hand Held Powder-Fed Laser Fusion Welding Torch,” the contents of which are hereby incorporated by reference in their entirety.
In accordance with an embodiment in which the component comprises a directionally solidified or single crystal microstructure, the powder particles may be deposited over the desired region, i.e. the blade tip, and a laser may be employed to melt the powder particles and an underlying portion of the component. The melted powder particles and melted portion of the component may solidify into a layer with a directionally solidified microstructure or single crystal microstructure having at least a predetermined primary orientation. As used herein, the term “predetermined primary orientation” may be defined as a direction perpendicular to a crystal lattice plane of a component. In an embodiment, the predetermined primary orientation in a component comprising a nickel-based superalloy may be denoted as a [001] direction. In an embodiment, the component may serve as the seed crystal, and the desired orientation may be in a direction that provides the component with improved creep strength and/or improved thermal fatigue strength. Hence, the improved or restored portion may grow epitaxially from the crystal structure of the component to form an extension of the single crystal microstructure of the component.
The turbine blade may thereafter be subjected to a solution heat treatment above the gamma prime solvus temperature of the nickel-based superalloy for a period in a range of about 1 to 10 hours. In other embodiments, the solution heat treatment may be longer or shorter than the aforementioned time period. The piece is then cooled to room temperature (e.g., about 20° C. to about 25° C.). The blade may be cooled to room temperature at a rate of about 50° C. per minute. In other embodiments, cooling may occur within a longer or shorter time period. By cooling the piece in a relatively short time period, an array of cuboidal gamma prime phase particles may precipitate, which may enhances creep strength in the tip region, for example. The blade may thereafter be machined to a desired shape and dimension. Although a turbine blade would be commonly heat treat by both a solution heat treatment but also a precipitation heat treatment that brings out the cuboidal gamma prime particles. However the composition of the weld tip does not require a heat treatment as such since its microstructure from solidification is predominately if not completely gamma prime. Sometimes blades can be tip welded also with a full heat treatment which typically requires an additional thermal process if the blades are platinum aluminide coated.
Returning to the flow diagram of
An exemplary alloy compositions A is provided in Table 1 and compared with the conventional SC180 single crystal turbine blade material. This exemplary alloy has a composition tailored for both improved resistance to cyclic oxidation and creep, relative to SC180. This combination of improved properties is expected to improve the oxidation and thermal fatigue life of turbine blade tips. Formulations for each nickel-based superalloy composition are included in Table 1, by weight:
A novel nickel-based superalloy and methods of manufacturing turbine engine components have now been provided. The novel nickel-based superalloy may provide improved oxidation-resistance over conventional nickel-based superalloys when subjected to engine operating temperatures. Additionally, the methods in which the novel nickel-based superalloys are used may be employed not only on blades, but also on other turbine components, including, but not limited to, vanes and shrouds. The method may also improve the durability of the turbine component, thereby optimizing the operating efficiency of a turbine engine, and prolonging the operational life of turbine blades and other engine components. Though the nickel-based superalloy is described above as being used for improvement of turbine blade tips, the superalloy may alternatively be employed for casting new turbine components. In one example, the inventive alloy described herein could be employed as a blade substrate, as opposed to being used solely in the tip region.
While at least one exemplary embodiment has been presented in the foregoing detailed description of the inventive subject matter, it should be appreciated that a vast number of variations exist. It should also be appreciated that the exemplary embodiment or exemplary embodiments are only examples, and are not intended to limit the scope, applicability, or configuration of the inventive subject matter in any way. Rather, the foregoing detailed description will provide those skilled in the art with a convenient road map for implementing an exemplary embodiment of the inventive subject matter. It being understood that various changes may be made in the function and arrangement of elements described in an exemplary embodiment without departing from the scope of the inventive subject matter as set forth in the appended claims.
Number | Name | Date | Kind |
---|---|---|---|
4152488 | Schilke et al. | May 1979 | A |
5366695 | Erickson | Nov 1994 | A |
5395584 | Berger et al. | Mar 1995 | A |
5622638 | Schell et al. | Apr 1997 | A |
5705281 | Reeves et al. | Jan 1998 | A |
20050194363 | Hu et al. | Sep 2005 | A1 |
20050224144 | Pollock et al. | Oct 2005 | A1 |
20050238526 | Schall | Oct 2005 | A1 |
20060219330 | Hu et al. | Oct 2006 | A1 |
20060239852 | Shipton et al. | Oct 2006 | A1 |
20090117282 | Arikawa et al. | May 2009 | A1 |
20090123290 | Imano et al. | May 2009 | A1 |
20090196760 | Harada et al. | Aug 2009 | A1 |
20090252613 | Gorman et al. | Oct 2009 | A1 |
20100012235 | Gleeson et al. | Jan 2010 | A1 |
20100279148 | Hu | Nov 2010 | A1 |
20110097599 | Hu | Apr 2011 | A1 |
20110103968 | Hoebel et al. | May 2011 | A1 |
Number | Date | Country |
---|---|---|
0683239 | Jan 1999 | EP |
1201778 | May 2002 | EP |
1930455 | Jun 2008 | EP |
2110449 | Oct 2009 | EP |
Entry |
---|
EP Search Report, EP 13187625.2-1353 dated Mar. 18, 2014. |
EP Communication, EP 13 187 625.2-1353 dated Aug. 4, 2014. |
Number | Date | Country | |
---|---|---|---|
20140134353 A1 | May 2014 | US |