Information
-
Patent Grant
-
6614182
-
Patent Number
6,614,182
-
Date Filed
Thursday, December 20, 200123 years ago
-
Date Issued
Tuesday, September 2, 200321 years ago
-
Inventors
-
Original Assignees
-
Examiners
Agents
- Scully, Scott, Murphy & Presser
-
CPC
-
US Classifications
Field of Search
US
- 313 491
- 313 582
- 313 584
- 313 585
-
International Classifications
-
Abstract
A plasma display panel (PDP), in which a high quality image is displayed by making its luminance and its luminance efficacy high and also its power consumption is reduced, is provided. The plasma display panel provides a group of plural pairs of sustaining electrodes covered with a dielectric layer on a first glass substrate by placing a discharge gap between the pair of sustaining electrodes, and a gas being filled up between the first glass substrate and a second glass substrate facing the first glass substrate. And an image is displayed on the PDP by irradiating ultraviolet light, which is obtained by making the group of plural pairs of the sustaining electrodes on the first glass substrate discharge by applying voltages to the group of plural pairs of the sustaining electrodes, on a fluorescent material. And a sustaining electrode in the pair of sustaining electrodes disposed on the nearly flat surface of the first glass substrate provides a discharge gap region electrode, a main surface discharge electrode, and an aperture disposed between the discharge gap region electrode and the main surface discharge electrode. And the main surface discharge electrode is composed of plural fine patterned wires and/or opening parts where electrodes are not formed.
Description
BACKGROUND OF THE INVENTION
The present invention relates to a plasma display panel (PDP), being flat and capable of displaying a color image, whose screen size can be made to be large, and which is used such as for a personal computer (PC), a work station, and a wall TV set, and in which its luminance becomes higher and its power consumption is reduced.
DESCRIPTION OF THE RELATED ART
Conventionally, a surface discharge type PDP has been used. This conventional PDP provides a group of many pairs of sustaining electrodes covered with a dielectric layer on a first glass substrate. And a gas is filled in a space between the first glass substrate and a second glass substrate facing the first glass substrate, and a discharge is generated by applying voltages to these pairs of sustaining electrodes, and ultraviolet light is obtained. The obtained ultraviolet light is irradiated to a fluorescent material and visible rays are obtained.
FIG. 1
is a plane view and a sectional view showing a structure of a first conventional PDP.
FIG. 2
is a perspective view showing the structure of the first conventional PDP. And
FIG. 3
is a plane view and a sectional view showing a structure of a second conventional PDP. As shown in
FIGS. 1
to
3
, a pair of sustaining electrodes
11
is formed on a first glass substrate
10
in a first substrate
1
for a unit discharge cell
300
, and the pair of sustaining electrodes
11
is covered with a dielectric layer
12
made of low-melting glass. At this time, the thickness of the dielectric layer
12
on the pair of sustaining electrodes
11
becomes nearly uniform.
In a case that a structure, in which the thickness of the dielectric layer
12
on the pair of sustaining electrodes
11
is nearly uniform, is used, when the thickness of the dielectric layer
12
is made to be large, the luminance efficacy becomes high. However, the discharge sustaining voltage is increased. On the contrary, when the thickness of the dielectric layer
12
is made to be small, the discharge sustaining voltage can be made to be low, but the luminance efficacy becomes low.
In order to avoid the problem mentioned above, a structure is proposed.
FIG. 4
is a sectional view showing a structure of a first substrate
1
of a third conventional PDP. As shown in
FIG. 4
, the thickness of the dielectric layer
12
is not uniform at a unit discharge cell. However, in this structure, the thickness of the dielectric layer
12
must be formed precisely in the whole unit discharge cells of the PDP, and the thickness of the dielectric layer
12
is liable to be uneven. Consequently, this affects the characteristics of the PDP, and this structure makes a high quality PDP difficult.
SUMMARY OF THE INVENTION
It is therefore an object of the present invention to provide a PDP, in which a high quality image is displayed by making its luminance and its luminance efficacy high and also its power consumption is reduced.
According to a first aspect of the present invention, for achieving the object mentioned above, there is provided a PDP. The PDP provides a group of plural pairs of sustaining electrodes covered with a dielectric layer on a first glass substrate, by placing a discharge gap between the pair of sustaining electrodes, and a gas being filled up between the first glass substrate and a second glass substrate facing the first glass substrate. And an image is displayed on the PDP by irradiating ultraviolet light, which is obtained by making the group of plural pairs of the sustaining electrodes on the first glass substrate discharge by applying voltages to the group of plural pairs of the sustaining electrodes, on a fluorescent material. And a sustaining electrode in the pair of sustaining electrodes disposed on the nearly flat surface of the first glass substrate provides a discharge gap region electrode, and a main surface discharge electrode, and an aperture disposed between the discharge gap region electrode and the main surface discharge electrode. And the main surface discharge electrode is composed of plural fine patterned wires and/or opening parts where electrodes are not formed.
According to a second aspect of the present invention, in the first aspect, the area of the main surface discharge electrode is 50% or less of the area of the region where the main surface discharge electrode is formed.
According to a third aspect of the present invention, in the first aspect, the area of the main surface discharge electrode is 30% or less of the area of the region where the main surface discharge electrode is formed.
According to a fourth aspect of the present invention, in the first aspect, the width of the fine patterned wire, of which the main surface discharge electrode is composed, is twice as narrow as or less of the value of the thickness of the dielectric layer for insulating the main surface discharge electrode from a discharge space.
According to a fifth aspect of the present invention, in the first aspect, the width of the discharge gap region electrode is 20% or less of the width of the sustaining electrode, disposed on the nearly flat surface of the first glass substrate, in the direction opposing the two sustaining electrodes each other in the pair of the sustaining electrodes.
According to a sixth aspect of the present invention, in the first aspect, the width of the discharge gap region electrode is 10% or less of the width of the sustaining electrode, disposed on the nearly flat surface of the first glass substrate, in the direction opposing the two sustaining electrodes each other in the pair of the sustaining electrodes.
According to a seventh aspect of the present invention, in the first aspect, the width of the aperture, which is disposed between the discharge gap region electrode and the main surface discharge electrode, is 10% or more of the width of the sustaining electrode in the direction opposing the two sustaining electrodes each other in the pair of the sustaining electrodes.
According to an eighth aspect of the present invention, in the first aspect, the width of the aperture, which is disposed between the discharge gap region electrode and the main surface discharge electrode, is 20% or more of the width of the sustaining electrode in the direction opposing the two sustaining electrodes each other in the pair of the sustaining electrodes.
According to a ninth aspect of the present invention, at least one of connecting electrodes for connecting the discharge gap region electrode and the main surface discharge electrode is disposed at the aperture that is disposed between the discharge gap region electrode and the main surface discharge electrode.
According to a tenth aspect of the present invention, in the ninth aspect, the area of the connecting electrodes is 20% or less of the area of the aperture.
According to an eleventh aspect of the present invention, in the first aspect, the thickness of the dielectric layer being nearly flat on the discharge gap region electrode is thinner than the thickness of the dielectric layer being nearly flat on the main surface discharge electrode.
According to a twelfth aspect of the present invention, in the first aspect, the sustaining electrode disposed on the nearly flat surface of the first glass substrate further provides a metal bus line positioned at the opposite side of the discharge gap region electrode and connected with both the discharge gap region electrode and the main surface discharge electrode, and a second aperture disposed between the main surface discharge electrode and the metal bus line. And the metal bus line makes wiring resistance of the sustaining electrode low.
According to a thirteenth aspect of the present invention, in the twelfth aspect, the width of the second aperture disposed between the main surface discharge electrode and the metal bus line is wider than the width of the aperture disposed between the discharge gap region electrode and the main surface discharge electrode.
According to a fourteenth aspect of the present invention, in the thirteenth aspect, a discharge is generated between the pair of the sustaining electrodes by applying voltages alternately to the pair of sustaining electrodes, and during a displaying discharge period by which the light emitting intensity of a light emitting display is controlled, the discharge is not spread in the region of the metal bus line beyond the second aperture.
According to a fifteenth aspect of the present invention, in the first aspect, the component of the gas generating ultraviolet light to irradiate to the fluorescent material is Xe, Kr, Ar, or nitrogen, and the partial pressure of the gas is 100 hPa or more.
BRIEF DESCRIPTION OF THE DRAWINGS
The objects and features of the present invention will become more apparent from the consideration of the following detailed description taken in conjunction with the accompanying drawings in which:
FIG. 1
is a plane view and a sectional view showing a structure of a first conventional PDP;
FIG. 2
is a perspective view showing the structure of the first conventional PDP;
FIG. 3
is a plane view and a sectional view showing a structure of a second conventional PDP;
FIG. 4
is a sectional view showing a structure of a first substrate of a third conventional PDP;
FIG. 5
is a plane view and a sectional view showing a structure of a first embodiment of a PDP of the present invention;
FIG. 6
is a diagram showing examples of structures of a main surface discharge electrode in a sustaining electrode shown in
FIG. 5
;
FIG. 7
is a plane view showing a structure of a pair of sustaining electrodes in a second embodiment of the PDP of the present invention;
FIG. 8
is a plane view showing a structure of a pair of sustaining electrodes in a third embodiment of the PDP of the present invention;
FIG. 9
is a plane view and a sectional view showing a structure of a first substrate in a fourth embodiment of the PDP of the present invention;
FIG. 10
is a plane view and a sectional view showing a structure of a pair of sustaining electrodes in a fifth embodiment of the PDP of the present invention;
FIG. 11
is a plane view and a sectional view showing a structure of a pair of sustaining electrodes in a sixth embodiment of the PDP of the present invention;
FIG. 12
is a plane view showing a distance relation in the pair of the sustaining electrodes of the PDP of the present invention; and
FIG. 13
is another plane view showing a distance relation in the pair of the sustaining electrodes of the PDP of the present invention.
DESCRIPTION OF THE PREFERRED EMBODIMENTS
Referring now to the drawings, embodiments of the present invention are explained in detail. In the embodiments of the present invention, each element, which has a nearly equal function to that in the conventional PDPs, has the same reference number.
FIG. 5
is a plane view and a sectional view showing a structure of a first embodiment of a PDP of the present invention. As shown in
FIG. 5
, a pair of sustaining electrodes
11
is formed on a nearly flat surface of a first glass substrate
10
, by placing a discharge gap
110
between the pair of the sustaining electrodes
11
at a unit discharge cell
300
. The sustaining electrode
11
is composed of a discharge gap region electrode
111
, which is positioned to the side of the discharge gap
110
, and a main surface discharge electrode
113
. An aperture
112
is disposed between the discharge gap region electrode
111
and the main surface discharge electrode
113
. This structure of the sustaining electrode
11
is different from the conventional PDPs.
FIG. 6
is a diagram showing examples of structures of the main surface discharge electrode
113
in the sustaining electrode
11
shown in FIG.
5
. As shown in
FIG. 6
, the main surface discharge electrode
113
has various shapes, and occupies a part or full of a main surface discharge electrode area
120
. That is, the main surface discharge electrode
113
is formed at the main surface discharge electrode area
120
. And the discharge gap region electrodes
111
, the apertures
112
, and the main surface discharge electrodes
113
are positioned symmetrically by placing the discharge gap
110
as their center axis in the pair of sustaining electrodes
11
.
FIG. 7
is a plane view showing a structure of a pair of sustaining electrodes
11
in a second embodiment of the PDP of the present invention.
FIG. 8
is a plane view showing a structure of a pair of sustaining electrodes
11
in a third embodiment of the PDP of the present invention. And
FIG. 9
is a plane view and a sectional view showing a structure of the first substrate
1
in a fourth embodiment of the PDP of the present invention.
As shown in FIG.
7
(
a
), the discharge gap region electrode
111
and the main surface discharge electrode
113
are connected with a connecting electrode
114
occupying a part of the aperture
112
. And in FIG.
7
(
b
), the discharge gap region electrode
111
and the main surface discharge electrode
113
are connected with two connecting electrodes
114
occupying a part of the aperture
112
. Further, as shown in
FIG. 8
, the discharge gap region electrode
111
is divided and the divided discharge gap region electrode
111
is disposed in the unit discharge cell
300
. The divided discharge gap region electrode
111
is connected to the main surface discharge electrode
113
with the connecting electrode
114
in FIG.
8
(
a
), and with the connecting electrodes
114
in FIG.
8
(
b
). The thickness of a dielectric layer
12
(not shown), which is formed on the pair of the sustaining electrodes
11
, is nearly uniform.
In the fourth embodiment of the present invention shown in
FIG. 9
, however, the thickness of the dielectric layer
12
on the discharge gap region electrode
111
is different from that on the main surface discharge electrode
113
. This level difference is formed nearly on the aperture
112
, which separates these two electrodes
111
and
113
. As shown in
FIG. 9
, this level difference rises at the edge part of the main surface discharge electrode
113
, and increases continuously on the aperture
112
. On the discharging electrodes
111
, there is no level difference. And this level difference falls continuously on the next aperture
112
, and the surface of the dielectric layer
12
becomes again the original surface level on the next main surface discharge electrode
113
. The shape of this level difference is not limited to a specific shape, and is possible to be steps, concave, or convex. In the fourth embodiment, the connecting electrode(s)
114
, which is used in the second and third embodiments, can be used between the discharge gap region electrode
111
and the main surface discharge electrode
113
.
In the second and third embodiments shown in
FIGS. 7 and 8
, the discharge gap region electrode
111
and the main surface discharge electrode
113
are connected so that their electric potential becomes almost equal. This is the same in the fourth embodiment in case that the fourth embodiment has the connecting electrode(s)
114
.
FIG. 10
is a plane view and a sectional view showing a structure of a pair of sustaining electrodes
11
in a fifth embodiment of the PDP of the present invention. As shown in
FIG. 10
, in the fifth embodiment, the sustaining electrode
11
provides a metal bus line
115
, in addition to the discharge gap region electrode
111
and the main surface discharge electrode
113
. This metal bus line
115
, positioned almost in parallel with the electrodes
111
and
113
, is disposed by placing a second aperture
117
between the main surface discharge electrode
113
and the metal bus line
115
.
FIG. 11
is a plane view and a sectional view showing a structure of a pair of sustaining electrodes
11
in a sixth embodiment of the PDP of the present invention. As shown in
FIG. 11
, the metal bus line
115
, the discharge gap region electrode
111
, and the main surface discharge electrode
113
are connected with connecting metals
116
. These connecting metals
116
are formed on upper surfaces of barrier ribs
23
, which are the upper surfaces of the barrier ribs
26
formed on a second substrate
2
and contacts with the first substrate
1
. With this, the pair of the sustaining electrodes
11
is sustained in a low resistance value, and the discharge gap region electrode
111
, the main surface discharge electrode
113
, and the metal bus line
115
are sustained in the same electric potential. In the fifth and sixth embodiments shown in
FIGS. 10 and 11
, the discharge gap region electrode
111
, the main surface discharge electrode
113
, and the metal bus line
115
are positioned symmetrically as that the discharge gap
110
is their center axis. And the aperture
112
is disposed between the discharge gap region electrode
111
and the main surface discharge electrode
113
, and the second aperture
117
is disposed between the main surface discharge electrode
113
and the metal bus line
115
.
In the embodiments of the PDP of the present invention, a gas, which mainly generates ultraviolet light, is filled up and sealed in a discharge space between the first substrate
1
and the second substrate
2
. This gas is xenon (Xe), krypton (Kr), argon (Ar), or nitrogen, and its partial pressure is 100 hPa or more. Helium (He) or neon (Ne) can be included in this gas.
In the embodiments of the present invention, the total gas pressure is several 10 hPa to 1 atm. (1013.25 hPa), and 100 hPa to 1 atm. is acceptable. Furthermore, preferably, the range of the total gas pressure is 300 hPa to less than 1 atm. At a high place whose pressure is 1 atm. or less, the gas pressure can be set to be up to the pressure at the place, for example, about 800 hPa. It is desirable that the total pressure is about 300 to 800 hPa. And also it is desirable that the partial pressure of the gas being ultraviolet light source is several 10 to 500 hPa.
Next, referring to the drawings, a manufacturing method of the PDP of the present invention is explained. In the first embodiment shown in
FIG. 5
, first, the pair of the sustaining electrodes
11
made of a transparent conductive material thin film, whose main component is tin oxide or indium oxide, is formed on the first glass substrate
10
by etching or a lift-off method. The sustaining electrode
11
provides at least two electrodes
111
and
113
and the aperture
112
between the electrodes
111
and
113
, as shown in FIG.
5
. In this, in case that the width of fine patterned wires, of which the main surface discharge electrode
113
is composed, is 30 μm or less, and the area of the main surface discharge electrode
113
is 30% or less of the main surface discharge electrode area
120
as shown in
FIG. 6
, a conductive material being different from the transparent conductive material thin film can be used for the main surface discharge electrode
113
. This conductive material is a metal thin film or a conductive material containing metal fine particles whose reflection factor for its discharge space side is 50% or more.
In the embodiments of the present invention, as mentioned above, the etching or the lift-off method was used to form the pair of the sustaining electrodes
11
. However, this forming method is not limited to the methods mentioned above, and other film forming methods and patterning methods can be used.
Next, the dielectric layer
12
being transparent made of such as low-melting glass is formed with almost flat surface by covering the pair of the sustaining electrodes
11
. It is desirable that the width of the fine patterned wires, of which the main surface discharge electrode
113
is formed, is twice as narrow as or less of the value of the thickness of the dielectric layer
12
.
Last, a magnesium oxide layer
13
, which is a protection layer, is formed on the surface, which contacts with the discharge space, of the dielectric layer
12
. With the processes mentioned above, the first substrate
1
is formed.
In the second substrate
2
facing the first substrate
1
, a data electrode
22
and a white dielectric layer
24
covering the data electrode
22
are formed on the second glass substrate
21
. Barrier ribs
26
, which decide the discharge space, is formed on the white dielectric layer
24
, and a fluorescent material layer
25
is formed on the white dielectric layer
24
decided by the barrier ribs
26
.
Next, comparing with the conventional PDP shown in
FIGS. 1
to
4
, the present invention is explained. The PDP of the present invention realized the high luminance efficacy by reducing the discharge current density without lowering the luminance.
Further, at the present invention, a remarkable good effect was realized by changing the area ratio between the area of the main surface discharge electrode
113
and the main surface discharge electrode area
120
. In this, the area ratio is that the area of
113
is divided by the area of
120
. When the area ratio was 50% or less, or preferably 30%, the remarkable good effect was recognized. The reason, why the remarkable good effect was realized, is that the discharge current at the main surface discharge electrode
113
being a main discharge region was reduced.
FIG. 12
is a plane view showing a distance relation in the pair of the sustaining electrodes
11
of the PDP of the present invention. As shown in
FIG. 12
, the width of the sustaining electrode
11
is defined as Wel, and the width of the discharge gap region electrode
111
is defined as Wfe. When the width ratio (Wfe/Wel) becomes 20% or less, preferably 10% or less, the high luminance efficacy can be realized by reducing the discharge current density.
FIG. 13
is another plane view showing a distance relation in the pair of the sustaining electrodes
11
of the PDP of the present invention. As shown in
FIG. 13
, in case that the width of the aperture
112
is defined as Wopn, when the width ratio (Wopn/Wel) is 10% or more, preferably, 20% or more, the high luminance efficacy can be realized by reducing the discharge current density. This is, when a large discharge generated at the discharge gap
110
transfers to the main discharge region, discharge factors relating to the discharge efficiency such as the electronic temperature are controlled to be higher efficiency.
Referring to
FIGS. 7 and 8
, the second and third embodiments of the present invention are explained in more detail. As mentioned above, the connecting electrode(s)
114
is provided at a part of the aperture
112
, disposed between the discharge gap region electrode
111
and the main surface discharge electrode
113
. This connecting electrode
114
works to help to transfer the discharge generated at the discharge gap
110
to the main surface discharge electrode
113
, in which the main discharge is formed, in a degree that does not decrease the effect of the aperture
112
mentioned above. With the structures mentioned above, the high luminance efficacy was realized by reducing the discharge current density without lowering the luminance.
In order to confirm the size of the connecting electrode
114
without decreasing the effect of the aperture
112
, the ratio of the area of the connecting electrode
114
to an area
130
of the aperture
112
was evaluated. In case that this ratio (the area of
114
/the area of
130
) is 20% or less, the luminance efficacy of the PDP of the present invention was especially increased. The connecting electrodes
114
are not necessary to be a pair as shown in FIGS.
7
(
a
) and
8
(
a
), but plural pairs of the connecting electrodes
114
can be disposed as shown in FIGS.
7
(
b
) and
8
(
b
). That is, the size and the number of the connecting electrodes
114
are not limited to the embodiments mentioned above, they are acceptable as far as the ratio is 20% or less.
In the second embodiment shown in
FIG. 7
, a pair of the discharge gap region electrodes
111
are disposed symmetrically as the discharge gap
110
is their center axis.
In the third embodiment shown in
FIG. 8
, in addition to the structure mentioned in the second embodiment, the pair of the discharge gap region electrodes
111
are divided and the divided pair of discharge gap region electrodes is disposed in the unit discharge cell
300
. In
FIG. 8
, the electric potential of the divided discharge gap region electrodes
111
is preferably equal to that of the main surface discharge electrode
113
. However, the electric potential of the part of the discharge gap region electrode
111
, which is positioned between the upper surfaces of barrier ribs
23
, can be controlled to be a little higher or lower than that of the main surface discharge electrode
113
. As mentioned above, the electric potential of the discharge gap region electrode
111
can be set arbitrary. In
FIGS. 7 and 8
, the number of the connecting electrodes
114
is one or two, however, the number is not limited to the number mentioned above.
Next, referring to
FIG. 9
, the fourth embodiment of the present invention is explained in more detail. In the fourth embodiment, the shape of the main surface discharge electrode
113
can be changed applying the first embodiment shown in FIG.
6
. In the fourth embodiment, the thickness of the dielectric layer
12
on the pair of the sustaining electrodes
11
is changed. In order to form the dielectric layer
12
having level difference parts, the level difference parts are formed by using low-melting glass, and are burned at a temperature near the glass softening point, and this non-flat dielectric layer
12
is formed. With this structure, the current density of the main discharge was reduced largely, and the luminance efficacy was improved.
At the fourth embodiment, even if the discharge gap region electrode
111
and the main surface discharge electrode
113
are formed almost continuously, without disposing the aperture
112
, the luminance efficacy can be improved a little. However, in a structure, in which the aperture
112
does not exist or the area of the aperture
12
is small (not enough), in case that the level difference parts of the pair of the sustaining electrodes
11
are not symmetry for the center axis of the discharge gap
110
, the dispersion of the discharge characteristics becomes large. On the contrary, in a structure having the aperture
112
, even when the level difference parts of the pair of the sustaining electrodes
11
are positioned not symmetrically a little for the center axis of the discharge gap
110
, that is, even when the level difference parts are not positioned symmetrically, the dispersion of the characteristics is small, and the luminance efficacy can be improved.
At the C part in
FIG. 9
, the dielectric layer
12
is formed between the upper level and the electrode level under the main surface discharge electrode
113
, and is formed between the lower level and the electrode level under the discharge gap
110
and the discharge gap region electrodes
111
. The aperture
112
can be disposed between the lower and electrode levels of the dielectric layer
12
. At the range of the discharge gap
110
, the dielectric layer
12
is preferably provided up to the lower level, however, can be provided up to near the substrate level of the first glass substrate
10
. As mentioned above, the dielectric layer
12
can be formed with the level difference on the first glass substrate
10
, by not forming with the same thickness.
Next, referring to
FIGS. 10 and 11
, the fifth and sixth embodiments of the present invention are explained in more detail. As mentioned above, in
FIG. 10
, the metal bus line
115
, made of a metal thin film, metal particles, or low-melting glass containing metal particles, which makes wiring resistance of the pair of the sustaining electrodes
11
low, is formed in parallel with the discharge gap region electrode
111
and the main surface discharge electrode
113
. The second aperture
117
is disposed between the metal bus line
115
and the main surface discharge electrode
113
. In
FIG. 11
, in order to make the electric potential of the discharge gap region electrode
111
and the main surface discharge electrode
113
equal, the connecting metals
116
are provided at the part corresponding to the upper surfaces of the barrier ribs
23
. With this structure, the luminance efficacy can be improved. In this case, it is desirable that a discharge, transferred to the main surface discharge electrode
113
from the discharge gap region electrode
111
, is not transferred to the metal bus line
115
. In order to achieve this, the width of the second aperture
117
, which is disposed between the main surface discharge electrode
113
and the metal bus line
115
, is made to be wider than that of the aperture
112
, which is disposed between the discharge gap region electrode
111
and the main surface discharge electrode
113
.
As mentioned above, in the embodiments of the present invention, it is desirable that each electrode in the pair of the sustaining electrodes
11
is positioned symmetrically as the discharge gap
110
is their center axis. That is, it is ideal that the shape and area of the same electrodes and the interval among the electrodes are almost equal. However, the degree of the symmetry is not strict, and it is desirable that the order positioning the electrodes and apertures is symmetry for the discharge gap
110
. However, it is enough that the shape and area of the same electrodes and the interval among the electrodes are almost equal. And the small difference in the intervals and the areas is acceptable. Cases, in which the symmetry is not satisfied completely, are included in the present invention, as far as the effects of the present invention are realized.
As mentioned above, according to the present invention, a PDP, in which a high quality image is displayed by making its luminance and its luminance efficacy high and its power consumption is reduced, can be realized.
As mentioned above, a PDP of the present invention provides a group of plural pairs of sustaining electrodes covered with a dielectric layer on a first glass substrate by placing a discharge gap between the pair of sustaining electrodes, and a gas is filled up between the first glass substrate and a second glass substrate facing the first glass substrate. And an image is displayed on the PDP by irradiating ultraviolet light, which is obtained by making the group of plural pairs of the sustaining electrodes on the first glass substrate discharge by applying voltages to the group of plural pairs of the sustaining electrodes, on a fluorescent material. And a sustaining electrode in the pair of sustaining electrodes disposed on the nearly flat surface of the first glass substrate provides a discharge gap region electrode, a main surface discharge electrode, and an aperture disposed between the discharge gap region electrode and the main surface discharge electrode. And the main surface discharge electrode is composed of plural fine patterned wires and/or opening parts where electrodes are not formed.
And when the area of the main surface discharge electrode is 50% or less, or 30% or less of the area of the region where the main surface discharge electrode is formed, the effect of the present invention can be realized. Further, when the width of the fine patterned wire, of which the main surface discharge electrode is composed, is twice as narrow as or less of the value of the thickness of the dielectric layer for insulating the main surface discharge electrode from a discharge space, the effect of the present invention can be realized. And when the width of the discharge gap region electrode is 20% or less, or 10% or less of the width of the sustaining electrode, disposed on the nearly flat surface of the first glass substrate, in the direction opposing the tow sustaining electrodes each other in the pair of the sustaining electrodes, the effect of the present invention can be realized. And when the width of the aperture, which is disposed between the discharge gap region electrode and the main surface discharge electrode, is 10% or more, or 20% or more of the width of the sustaining electrode in the direction opposing the tow sustaining electrodes each other in the pair of the sustaining electrodes, the effect of the present invention can be realized. And at least one of connecting electrodes for connecting the discharge gap region electrode and the main surface discharge electrode is disposed at the aperture that is disposed between the discharge gap region electrode and the main surface discharge electrode, and when the area of the connecting electrodes is 20% or less of the area of the aperture, the effect of the present invention can be realized. And when the thickness of the dielectric layer being nearly flat on the discharge gap region electrode is thinner than the thickness of the dielectric layer being nearly flat on the main surface discharge electrode, the effect of the present invention can be realized.
Further, the sustaining electrode disposed on the nearly flat surface of the first glass substrate further provides a metal bus line positioned at the opposite side of the discharge gap region electrode, and a second aperture disposed between the main surface discharge electrode and the metal bus line. And the metal bus line makes wiring resistance of the sustaining electrode low.
And the width of the second aperture disposed between the main surface discharge electrode and the metal bus line is wider than the width of the aperture disposed between the discharge gap region electrode and the main surface discharge electrode. Therefore, when a discharge is generated between the pair of the sustaining electrodes by applying voltages alternately to the pair of sustaining electrodes, and during a displaying discharge period in which the light emitting intensity of a light emitting display is changed, the discharge is not generated at the metal bus line beyond the second aperture.
And the component of the gas generating ultraviolet light to irradiate to the fluorescent material is Xe, Kr, Ar, or nitrogen, and the partial pressure of the gas is 100 hPa or more.
According to the structure of the PDP of the present invention, the electric current density at the surface discharge can be reduced, with sustaining the electric field strength largely in the discharge space near the discharge gap region electrodes facing each other, which affects largely the way of discharge between the pair of sustaining electrodes formed on an almost flat surface. Further, the intense discharge generated at the discharge gap is not sustained on the sustaining electrodes as it is, and can be transferred to the surface discharge by that the intense discharge is made to be low. Therefore, the high luminance efficacy can be realized with that the voltage sustaining the discharge is made to be low. With this, a PDP with high image quality and low power consumption having such as high luminance, high luminance efficacy, and high contrast can be realized.
While the present invention has been described with reference to the particular illustrative embodiments, it is not to be restricted by those embodiments but only by the appended claims. It is to be appreciated that those skilled in the art can change or modify the embodiments without departing from the scope and spirit of the present invention.
Claims
- 1. A plasma display panel (PDP), comprising:a group of plural pairs of sustaining electrodes covered with a dielectric layer on a first glass substrate by placing a discharge gap between said pair of sustaining electrodes; and a gas being filled up between said first glass substrate and a second glass substrate facing said first glass substrate, wherein: an image is displayed on said PDP by irradiating ultraviolet light, which is obtained by making said group of plural pairs of said sustaining electrodes on said first glass substrate discharge by applying voltages to said group of plural pairs of said sustaining electrodes, on a fluorescent material, wherein: a sustaining electrode in said pair of sustaining electrodes disposed on the nearly flat surface of said first glass substrate, comprising: a discharge gap region electrode; a main surface discharge electrode; and an aperture disposed between said discharge gap region electrode and said main surface discharge electrode, wherein: said main surface discharge electrode is composed of plural fine patterned wires and/or opening parts where electrodes are not formed.
- 2. A PDP in accordance with claim 1, wherein:the area of said main surface discharge electrode is 50% or less of the area of the region where said main surface discharge electrode is formed.
- 3. A PDP in accordance with claim 1, wherein:the area of said main surface discharge electrode is 30% or less of the area of the region where said main surface discharge electrode is formed.
- 4. A PDP in accordance with claim 1, wherein:the width of said fine patterned wire, of which said main surface discharge electrode is composed, is twice as narrow as or less of the value of the thickness of said dielectric layer for insulating said main surface discharge electrode from a discharge space.
- 5. A PDP in accordance with claim 1, wherein:the width of said discharge gap region electrode is 20% or less of the width of said sustaining electrode, disposed on said nearly flat surface of said first glass substrate, in the direction opposing the two sustaining electrodes each other in said pair of said sustaining electrodes.
- 6. A PDP in accordance with claim 1, wherein:the width of said discharge gap region electrode is 10% or less of the width of said sustaining electrode, disposed on said nearly flat surface of said first glass substrate, in the direction opposing the two sustaining electrodes each other in said pair of said sustaining electrodes.
- 7. A PDP in accordance with claim 1, wherein:the width of said aperture, which is disposed between said discharge gap region electrode and said main surface discharge electrode, is 10% or more of the width of said sustaining electrode in the direction opposing the two sustaining electrodes each other in said pair of said sustaining electrodes.
- 8. A PDP in accordance with claim 1, wherein:the width of said aperture, which is disposed between said discharge gap region electrode and said main surface discharge electrode, is 20% or more of the width of said sustaining electrode in the direction opposing the two sustaining electrodes each other in said pair of said sustaining electrodes.
- 9. A PDP in accordance with claim 1, wherein:the thickness of said dielectric layer being nearly flat on said discharge gap region electrode is thinner than the thickness of said dielectric layer being nearly flat on said main surface discharge electrode.
- 10. A PDP in accordance with claim 1, wherein:the component of said gas generating ultraviolet light to irradiate to said fluorescent material is Xe, Kr, Ar, or nitrogen, and the partial pressure of said gas is 100 hPa or more.
- 11. A PDP in accordance with claim 1, wherein:at least one of connecting electrodes for connecting said discharge gap region electrode and said main surface discharge electrode is disposed at said aperture that is disposed between said discharge gap region electrode and said main surface discharge electrode.
- 12. A PDP in accordance with claim 11, wherein:the area of said connecting electrodes is 20% or less of the area of said aperture.
- 13. A PDP in accordance with claim 1, wherein:said sustaining electrode disposed on the nearly flat surface of said first glass substrate, further comprising: a metal bus line positioned at the opposite side of said discharge gap region electrode and connected with both said discharge gap region electrode and said main surface discharge electrode; and a second aperture disposed between said main surface discharge electrode and said metal bus line, wherein: said metal bus line makes wiring resistance of said sustaining electrode low.
- 14. A PDP in accordance with claim 13, wherein:the width of said second aperture disposed between said main surface discharge electrode and said metal bus line is wider than the width of said aperture disposed between said discharge gap region electrode and said main surface discharge electrode.
- 15. A PDP in accordance with claim 14, wherein:a discharge is generated between said pair of said sustaining electrodes by applying voltages alternately to said pair of sustaining electrodes, and during a displaying discharge period by which the light emitting intensity of a light emitting display is controlled, said discharge is not spread in the region of said metal bus line beyond said second aperture.
Priority Claims (1)
Number |
Date |
Country |
Kind |
2000-400586 |
Dec 2000 |
JP |
|
US Referenced Citations (2)
Number |
Name |
Date |
Kind |
6384531 |
Park et al. |
May 2002 |
B1 |
20020195939 |
Okigawa et al. |
Dec 2002 |
A1 |