Abstract
A process for electrochemical stripping of components is disclosed. An operating point of the electrochemical stripping is determined under actual process conditions prior to the actual electrochemical stripping and is determined anew continuously, i.e., monitored and optionally adjusted during the electrochemical stripping.
Description
BACKGROUND AND SUMMARY OF THE INVENTION

The invention relates to a process for electrochemical stripping of components.


Components of a gas turbine such as the rotor blades are provided with special coatings to provide oxidation resistance, corrosion resistance or also erosion resistance on the surfaces. The components of gas turbines are subject to wear during operation of same and may be damaged in other ways. To repair damage, it is usually necessary to partially or completely remove and/or deplate the coating in the area of the component to be repaired. The removal and/or deplation of coatings is also referred to as stripping of coatings.


Referring to stripping methods, a distinction is made as to whether stripping is performed by mechanical means, chemical means or electrochemical means. Electrochemical stripping is based on the principle of electrolysis. In electrochemical stripping processes, a distinction is made among those that operate with the help of a 2-electrode system, a 3-electrode system or a 4-electrode system. The present invention relates to an electrochemical stripping process, preferably using a 2-electrode system.


U.S. Pat. No. 6,165,345 discloses an electrochemical process for stripping coatings from gas turbine blades based on a 2-electrode system. According to the method disclosed there, a turbine blade to be stripped is connected to the positive terminal of a voltage source, whereby a specially adapted electrode is connected to the negative terminal of same. The shape of this electrode corresponds essentially to the shape of the turbine blades to be stripped and/or the shape of the area of the turbine blade to be stripped. The electrode, and at least the area of the turbine blade to be stripped, are immersed in a working medium, a direct voltage of 1V to 3V being applied per component to provide a current flow between 5 A and 10 A. The operating range of electrochemical stripping as defined by the applied direct voltage is constant during the entire stripping process according to U.S. Pat. No. 6,165,345.


The object of the present invention is to create a novel process for electrochemical stripping of components.


According to the invention, an operating point of the electrochemical process of stripping is determined under actual process conditions prior to the actual electrochemical stripping process and is determined anew, i.e., monitored continuously, during electrochemical stripping and optionally adjusted.


Within the meaning of the present invention, the operating point of electrochemical stripping is determined in situ, i.e., under actual process conditions of electrochemical stripping—and is monitored continuously during electrochemical stripping and optionally adjusted. It is possible in this way to adjust the operating point to variable process conditions and thus always work at an optimum stripping rate and/or deplating rate. The time required for stripping is thus reduced significantly. Due to the continuous monitoring and optional adjustment of the operating point during electrochemical stripping, the operating point is also adjusted with respect to the component to be stripped, and is in particular adapted to the degree of stripping already performed and thus to the associated change in chemical composition of same. The inventive process is thus characterized by a high selectivity in stripping, so that there is a low risk of damage to the components during stripping.


According to an advantageous development of the invention, a direct voltage potential is applied, whereby the direct voltage potential is increased until a measured polarization current reaches a maximum as a function of the direct voltage potential, whereby this maximum determines the operating point of the stripping process. During stripping, an alternating voltage is superimposed on the direct voltage potential, and a change in the polarization current or the polarization conductance, which is due to the superimposed alternating voltage, is measured, whereby the direct voltage potential is adjusted as a function thereof so that the polarization current remains at the maximum.


Preferred embodiments of the present invention are derived from the following description.





BRIEF DESCRIPTION OF THE DRAWINGS

An exemplary embodiment of the present invention is explained in greater detail on the basis of the drawing, without being restricted thereto.



FIG. 1 illustrates a blade of a gas turbine that is to be stripped.





DETAILED DESCRIPTION OF THE DRAWINGS

Hereinafter, the inventive method is described by using the example of a gas turbine blade to be stripped. FIG. 1 illustrates such a blade 10 of a gas turbine comprising a blade vane 11 and a blade footing 12. In the exemplary embodiment shown here, the entire blade 10, i.e., the entire surface area of the blade vane 11 and the blade footing 12, is provided with a coating 13. This coating 13 may be an oxidation-resistant, corrosion-resistant and erosion-resistant coating.


Within the meaning of the present invention, a method is now proposed for deplating and/or removing the coating 13 from the surface of the blade pan 11 and the blade footing 12, for example, to repair the blade 10. Within the meaning of the present invention, this is performed by an electrochemical process using a 2-electrode system.


For electrochemical stripping of the blade 10, the latter is connected to the positive terminal of a voltage source, whereas the control electrode and/or counter-electrode is connected to the negative terminal of the voltage source. The control electrode and/or counter-electrode and the blade 10 to be stripped are immersed in a working medium—in an electrolyte solution.


Different from a 3-electrode system, the 2-electrode system used here employs a sturdy metal electrode as the control electrode instead of a combined measuring electrode and control electrode. Such a sturdy metal electrode as the control electrode is much less sensitive to the stripping process and to environmental influences such as electromagnetic waves. The electrochemical stripping process thus becomes less susceptible to interferences and is thus more overall more stable.


It is within the meaning of the present invention to determine the operating point of the 2-electrode system, i.e., the operating point of electrochemical stripping, in situ prior to the actual electrochemical stripping and to determine the operating point anew continuously during the stripping process, i.e., to monitor it and optionally adjust it. The term in situ is to be understood to mean that the operating point of electrochemical stripping is determined under actual process conditions, i.e., specifically in 2-electrode system. A measured polarization current and/or a measured polarization conductance is used as the control signal, i.e., criterion for determining the operating point of the electrochemical stripping. To do so, the procedure is as follows:


To determine the operating point of electrochemical stripping, a potentiostatic circuit for the working potential and/or for the control potential of the electrochemical stripping is created on the 2-electrode system, which means that a direct voltage potential is applied to the 2-electrode system. This direct voltage potential is then raised continuously or incrementally to determine the operating point for electrochemical stripping. The measured polarization current and/or the measured polarization conductance changes as a function of the applied direct voltage. Thus, in this way, a polarization-current/control-potential characteristic and/or a polarization-conductance/control-potential characteristic is determined.


The direct voltage is then increased until the first derivation of the polarization current as a function of the direct voltage potential, starting from positive values, assumes a value of zero and subsequently becomes negative, which means that the polarization current has reached a maximum and the polarization conductance assumes a value of zero. This value of the direct voltage potential, at which the polarization current assumes a maximum and/or at which the polarization conductance assumes a value of zero, serves as the operating point for electrochemical stripping. At this direct voltage potential, the electrochemical stripping proceeds at a maximum deplating rate or stripping rate. This determination of the operating point is system-specific, i.e., the ohmic resistance of the working medium, i.e., the electrolyte solution, is taken into account.


According to an advantageous development of the present invention, an alternating voltage is superimposed on the direct voltage potential determined during the electrochemical stripping. The alternating voltage preferably has a low voltage amplitude of preferably ±5 mV. The change in the polarization current or the polarization conductance due to the superimposed alternating voltage is measured, and the direct voltage potential is modified as a function thereof, so that the polarization current remains at the maximum and/or the polarization conductance retains a value of zero. At a negative polarization conductance, the control potential and/or the direct voltage potential is reduced; at a positive polarization conductance, the direct voltage potential is increased accordingly. This ensures that stripping is always performed at the maximum rate of removal, and that stripping is avoided within the range of the so-called breakdown potential. In this way, an optimal deplating rate can be achieved during the entire stripping process, and gentle stripping of the gas turbine blade to be stripped is always achieved.


It is also within the meaning of the present invention to use the values measured for the polarization current and/or the polarization conductance during the stripping process for definition of a termination criterion for electrochemical stripping. The measured values of the polarization current thus also contain information about the degree of stripping of the stripped component that has already taken place and/or about the structure of the coating to be deplated with the help of electrochemical stripping. The termination criterion for the electrochemical stripping is obtained from the relationship between the initial value and the values currently measured for the polarization current. This calculation is performed without stopping during the stripping and is thus performed continuously. If the polarization current assumes a value obtained from this calculation, the stripping process can be terminated as a function thereof.


The inventive process for electrochemical stripping is preferably used for stripping gas turbine blades. It is also suitable for stripping gas turbine blades having internal channels such as cooling channels. For stripping such gas turbine blades, as described above, the operating point of the electrochemical stripping is determined and monitored continuously during stripping and optionally adjusted. The stripping of the blade surfaces is performed in this way. If it is found on the basis of the continuously detected values for the polarization current that the stripping process on the surface of the gas turbine blade has been terminated, then according to this invention, the control potential is increased into a passive range for the blade surface. Because of the small diameters of the channels arranged inside the gas turbine blade, there is a shift in the control potential for the channels to an active range, so that stripping can also be performed within the channels in this way. During stripping of the blade surfaces, there is no stripping of the channels.


The present inventive process for electrochemical stripping of components is characterized by a high selectivity of the stripping process. The operating point of electrochemical stripping is adjusted continuously and thus the electrochemical stripping can always be performed at the optimal deplating rate. The inventive process is more rapid and less expensive than the stripping processes known from prior art. Due to its high selectivity, there is a minimal risk of damage to the components during stripping.


Referring to the inventive electrochemical stripping process, highly diluted acids are used as the electrolyte solution, i.e., the working medium. To this extent, only a minimum of safety measures and a minimum of time and energy are required for disposal of the working medium.


The inventive stripping process can be integrated in line production. The inventive process is also insensitive to so-called local elements on the surface of the component to be stripped, which elements can develop due to significant differences in wear and/or damage to the coating on the surface of the component to be stripped.


Finally, it should be pointed out that for the most accurate possible adjustment and/or control of the operating point for electrochemical stripping, the control potential, i.e., the direct voltage potential, should not be tapped directly on the current carrying lines but, instead, should be tapped via a separate line. Voltage losses by the current-carrying lines can be eliminated in this way. The operating point can be determined and adjusted more accurately.

Claims
  • 1-8. (canceled)
  • 9. A method for electrochemical stripping of components, in particular for stripping aluminum-coated components of a gas turbine, wherein an operating point of the electrochemical stripping is determined under actual process conditions prior to actual stripping, wherein the operating point of maximum stripping is determined as a function of a measured polarization current or a measured polarization conductance and is determined anew continuously during the electrochemical stripping, and wherein an applied direct voltage potential is adjusted accordingly.
  • 10. The method according to claim 9, wherein the stripping is performed using a two-electrode system.
  • 11. The method according to claim 9, wherein the direct voltage potential is increased to a value where the polarization conductance or a first derivation of the polarization current as a function of the direct voltage potential is approximately zero, and wherein the value of the direct voltage potential determines the operating point of stripping.
  • 12. The method according to claim 9, wherein the direct voltage potential is increased until the polarization current reaches a maximum as a function of the direct voltage potential, and wherein the maximum determines the operating point of the stripping.
  • 13. The method according to claim 9, wherein an alternating voltage is superimposed on the direct voltage potential during the stripping, wherein a change in the polarization current or the polarization conductance due to the superimposed alternating voltage is measured, and wherein the direct voltage potential is adjusted as a function thereof, so that the polarization current remains at a maximum.
  • 14. The method according to claim 13, wherein the alternating voltage has a low amplitude.
  • 15. The method according to claim 14, wherein the alternating voltage is ±5 mV.
  • 16. The method according to claim 9, wherein a value of the measured polarization current or the polarization conductance during the stripping is used to determine a termination criterion for the electrochemical stripping.
  • 17. The method according to claim 9, wherein a blade of a gas turbine having channels, in particular cooling channels, integrated into the blade is stripped, wherein the operating point is determined as a function of the measured polarization current or polarization conductance for stripping a surface of the blade, and wherein, after stripping the blade surface, a control potential is increased, so that the stripping of the blade surface comes to a standstill and stripping of the channels is performed.
  • 18. A method for electrochemical stripping of a component of a gas turbine engine, comprising the steps of: determining a value of an applied direct voltage potential for a maximum stripping rate of the electrochemical stripping process prior to commencing the stripping process;commencing the electrochemical stripping process at the value of the direct voltage potential; andcontinuously monitoring the value during the electrochemical stripping process.
  • 19. The method according to claim 18, wherein the step of determining the value includes the steps of determining when a measured value of a polarization current is at a maximum or a measured value of a polarization conductance is zero.
  • 20. The method according to claim 19, further comprising the step of adjusting the value during the electrochemical stripping process such that the measured value of the polarization current remains at the maximum or the measured value of the polarization conductance remains at zero.
  • 21. The method according to claim 20, wherein the step of adjusting the value includes the step of superimposing an alternating voltage on the direct voltage potential.
  • 22. The method according to claim 20, wherein the step of adjusting the value includes the step of reducing the direct voltage potential.
  • 23. The method according to claim 20, wherein the step of adjusting the value includes the step of increasing the direct voltage potential.
  • 24. The method according to claim 18, further comprising the step of terminating the electrochemical stripping process.
  • 25. The method according to claim 24, wherein the step of terminating the electrochemical stripping process includes the step of defining a termination criterion for the electrochemical stripping process.
  • 26. The method according to claim 25, wherein the step of defining the termination criterion includes the steps of measuring a value of a polarization current applied to the component at a commencement of the electrochemical stripping process and measuring a value of the polarization current applied to the component after commencement of the electrochemical stripping process.
  • 27. The method according to claim 18, further comprising the steps of: terminating the electrochemical stripping process on a surface of the component; andcommencing the electrochemical stripping process within a channel of the component.
  • 28. The method according to claim 27, wherein the steps of terminating the electrochemical stripping process on the surface of the component and commencing the electrochemical stripping process within the channel of the component includes the step of adjusting the value of the applied direct voltage potential.
Priority Claims (1)
Number Date Country Kind
102004002763.3 Jan 2004 DE national
Parent Case Info

This application claims the priority of International Application No. PCT/DE2004/002799, filed Dec. 22, 2004, and German Patent Document No. 10 2004 002 763.3, filed Jan. 20, 2004, the disclosures of which are expressly incorporated by reference herein.

PCT Information
Filing Document Filing Date Country Kind 371c Date
PCT/DE2004/002799 12/22/2004 WO 00 8/4/2008