PROCESSING OF LOW RANK COAL

Abstract
A method of processing coal includes placing coal having a heat content between about 3,000 BTU/lb and about 9,000 BTU/lb and a moisture content between about 20 wt % and about 60 wt % in a vessel. The coal is heated by conduction. A pressure in the vessel is reduced to below atmospheric pressure, thereby reducing the coal, such that an average primary particle size of the coal is less than 1 millimeter. The reduced coal is shaped to yield a fuel composition.
Description
TECHNICAL FIELD

This disclosure relates to processing of low rank coal, such as lignite.


BACKGROUND

Low rank coal (e.g., lignite) is softer, is more CO2 intensive, and has a higher moisture content and lower fuel value than “hard” coal (e.g., bituminous, sub-bituminous, anthracite). Lignite, the lowest rank coal, typically has a moisture content in a range of 30-60 wt % and a heat content in a range of 4,000-8,300 BTU/lb. In contrast, sub-bituminous coal typically has a moisture content in a range of 10-45 wt % and an energy content in a range of 8,500-13,000 BTU/lb, and bituminous coal typically has a moisture content in a range of 2-15 wt % and a heat content in a range of 11,000-15,000 BTU/lb. Due to its high moisture content and brittle nature, processing of low rank coal typically requires significant energy input and results in the creation of fines (e.g., dust), which presents a combustion hazard and is of little use as an energy source.


SUMMARY

Certain aspects of the subject matter described can be implemented as a method for processing coal. The method includes placing coal having a heat content between about 3,000 BTU/lb and about 9,000 BTU/lb and a moisture content between about 20 wt % and about 60 wt % in a vessel. The coal is heated by conduction. A pressure in the vessel is reduced to below atmospheric pressure, thereby reducing a primary particle size of the coal, such that an average primary particle size of the coal is less than 1 millimeter. The reduced coal is shaped to yield a fuel composition.


This, and other aspects, can include one or more of the following features.


In some embodiments, heating the coal includes contacting the coal with a heated surface. In some embodiments, the heated surface includes a rotating blade. In some embodiments, the rotating blade rotates at a rate between 2 and 25 revolutions per minute.


In some embodiments, heating the coal includes heating to the coal to a temperature between 30° C. and 100° C. In some embodiments, heating the coal includes heating the coal to a temperature up to about 250° C. In some embodiments, heating the coal includes heating the coal to a temperature between 100° C. and 250° C., between 110° C. and 240° C., 120° C. and 230° C., between 130° C. and 220° C., or between 140° C. and 210° C.


In some embodiments, the coal is agitated in the vessel by contacting the coal with a rotating blade. In some embodiments, the coal is intermittently agitated in the vessel.


In some embodiments, reducing the pressure in the vessel includes intermittently reducing the pressure in the vessel. In some embodiments, reducing the pressure in the vessel includes reducing the pressure in the vessel to between 10 torr and 150 torr.


In some embodiments, the coal placed in the vessel is uncrushed. In some embodiments, the coal placed in the vessel includes lignite. In some embodiments, the coal placed in the vessel has a moisture content between 30 wt % and 60 wt %, or between 40 wt % and 50 wt %.


In some embodiments, the fuel composition has a moisture content less than 3 wt %, less than 2 wt %, or less than 1 wt %. In some embodiments, the fuel composition has a heat content between 9,000 BTU/lb and 11,000 BTU/lb, between 9,500 BTU/lb and 10,500 BTU/lb, or between 9,500 BTU/lb and 10,000 BTU/lb.


In some embodiments, the coal is not pyrolyzed in the vessel. In some embodiments, a heated fluid is not provided to the vessel. In some embodiments, the fuel composition is substantially free of fines.


In some embodiments, shaping the reduced coal includes extruding the reduced coal to yield an extruded fuel product. In some embodiments, shaping the reduced coal includes cutting, shredding, or milling the extruded fuel product to form discrete portions of the fuel composition.







DETAILED DESCRIPTION

“Low rank coal” is a coal typically having a heat content (for example, higher heating value (HHV)) between about 4,000 BTU/lb and about 8,300 BTU/lb and a moisture content between about 20 wt % and about 60 wt % or between about 40 wt % and about 50 wt %. In some embodiments, low rank coal has a fixed carbon content between about 30 wt % and about 70 wt %. In some embodiments, low rank coal has an ash content of less than about 10 wt %. In some embodiments, low rank coal has a volatiles content between about 5 wt % and about 50 wt %. One example of low rank coal is lignite.


Transportation of unprocessed low rank coal can be considered inefficient due to its high moisture content. In effect, paying to transport unprocessed low rank coal can be considered wastefully paying for transport of a resource that can be about half water by weight. Thus, it can be beneficial to remove moisture content from low rank coal before transportation. Methods to remove the moisture in lignite have been employed but entail specific challenges. One such challenge is that lignite must often be crushed or pulverized as a separate step, prior to effective moisture removal. For example, in order to remove moisture content from low rank coal, the low rank coal needs to be reduced in size (e.g., pulverized) so that the water trapped in the low rank coal can escape. However, pulverizing the low rank coal in order to reduce moisture content can produce coal dust and can pose handling, logistics and transport challenges, including due to the creation of dust. For example, pulverizing the low rank coal in order to reduce moisture content can produce coal dust and can convert the low rank coal into a non-transportable form (e.g., a hazardous powder). Therefore, after reducing the moisture content of the low rank coal, the low rank coal needs to be re-packaged and/or processed into a transportable form.


The methods described in this disclosure can be implemented to complete the steps of removing moisture content from low rank coal and re-packaging the low rank coal with reduced moisture content into a transportable form in a single batch process. One example advantage of the methods described herein is that the energy content of the coal is increased on a per weight basis, while also displacing a certain percentage of coal with a waste material that otherwise would not be beneficially used, thus allowing for a near-term reduction of the amount of coal needed by the operator due to the higher energy content and reducing the negative environmental impact of coal combustion emissions and the total demand for coal. As described in this disclosure, low rank coal can be processed to yield a processed coal having moisture content of less than 3 wt %, less than 2 wt %, or less than 1 wt %, and to a heat content of at least about 1.5 to at least about 1.9 times the heat content of the unprocessed coal.


Processing low rank coal includes placing coal having a heat content between about 4,000 BTU/lb and about 8,300 BTU/lb in a vessel. The coal can be uncrushed (e.g., straight from a mine) or crushed. The vessel can be sealed. The coal is heated by conduction. Heating the coal by conduction includes contacting the coal with a heated surface. Heating the coal can occur without providing heated gas (e.g., air) to the vessel. In one example, the heated surface includes one or more blades configured to rotate in the vessel. The coal can be heated to a temperature up to about 250° C. In some examples, the coal is heated to a temperature between 100° C. and 250° C., between 110° C. and 240° C., between 120° C. and 230° C., between 130° C. and 220° C., or between 140° C. and 210° C. The heat provided is insufficient to pyrolyze the coal. Moreover, in some embodiments, heated fluid (e.g., in the form of steam or air) is not provided to the vessel.


When the coal is heated by a blade configured to rotate in the vessel, the blade(s) can be rotated at a speed between about 1 and about 10 rotations per minute. The blade(s) can be rotated intermittently, such that the blade is stationary at times and in motion at other times. The intermittent rotation can occur in a pattern (e.g., periodically) or occur randomly. The coal can be agitated (e.g., by rotation of the blade(s)). The agitation can occur intermittently (e.g., during rotation of the blade(s)). In some embodiments, the agitation is intermittently performed in intervals of about 1 minute separated by pauses in agitation of about 1 minute to about 3 minutes. In some embodiments, the blade(s) protrude radially outward from and are coupled to a central rod. In some embodiments, the central rod is rotated, for example, by a motor, to rotate the blade(s), resulting in agitation of the coal within the vessel. While the methods provided herein can produce fines and/or dust during processing, the fines and/or dust are largely stabilized once the processing has been completed to significantly reduce the amount of fines and/or dust by-product that are produced by the system. For example, during processing, the fines and/or dust can be stabilized by densifying (for example, through extrusion) the fines and/or dust into a solid fuel product. The pattern, duration, and extent of agitation can be selected to reduce or minimize pulverization of the coal, and thereby reduce or minimize the amount of fines and/or dust by-product produced from the coal.


In some embodiments, the blade(s) are rotated at a speed that is less than 25 revolutions per minute (rpm), less than 20 rpm, less than 15 rpm, less than 10 rpm, or less than 5 rpm. In some embodiments, the blade(s) are rotated at a speed between 2 rpm and 25 rpm. In some embodiments, the speed at which the blade(s) are rotated is varied. In some embodiments, the speed at which the blade(s) are rotated is varied between 1 rpm and 25 rpm. In some embodiments, the blade(s) are not rotated at all or not rotated for a desired time duration (e.g., 1 min to 5 min). In some embodiments, the speed at which the blade(s) are rotated alternates between gradually decreasing and gradually increasing. In some embodiments, the time duration(s) of no rotation of the blade(s) is between 1 minute and 3 minutes. In some embodiments, the blade(s) are rotated around a longitudinal axis defined by the central rod, such that an outermost tip of the blade(s) has a maximum tangential velocity of about 20 inches per second (in/s) or about 15 in/s. In some embodiments, the blade(s) are rotated around the longitudinal axis defined by the central rod, such that the outermost tip of the blade(s) has a tangential velocity between 5 in/s and 15 in/s.


The pressure in the vessel can be reduced to below atmospheric pressure (vacuum). As used in this disclosure, the term “vacuum” can encompass any pressure that is less than atmospheric pressure (1 atmosphere). Reducing the pressure in the vessel can occur intermittently. The intermittent pressure reduction can occur in a pattern (e.g., periodically) or occur randomly. That is, the pressure may be reduced, then allowed to increase (e.g., to atmospheric pressure), and then reduced again. The pressure in the vessel can be reduced to a pressure between 10 torr and 150 torr, between 50 torr and 150 torr, or between 50 torr and 100 torr. With reduced pressure in the vessel, the coal may be heated to a temperature between about 30° C. and about 100° C. Reducing the pressure in the vessel (e.g., to about 50 torr) and heating to a lower temperature (e.g., 40° C.) may yield the same results as heating at a greater pressure (e.g., atmospheric pressure) and a greater temperature (e.g., 140° C.). Reducing the pressure promotes thermal transformation, removal of moisture (e.g., in the form of water vapor), and also promotes removal of oxygen, thereby mitigating and/or preventing ignition of the coal.


Pressure reduction in the vessel can be carried out by using, for example, a vacuum pump. Reducing pressure in the vessel can involve using the vacuum pump to evacuate vapor from an interior of the vessel. For example, an outlet of a vapor space of the vessel is connected to the vacuum pump, and during operation, the vacuum pump pulls vapor from the vapor space of the vessel. The outlet of the vapor space of the vessel that is connected to the vacuum pump is located a predetermined distance away from a processing zone of the vessel that includes the rotating blade(s). In some embodiments, the outlet is located at least one radius away from an outermost tip of the rotating blade(s), in which the radius is defined as the distance between the central rod and the outermost tip of the rotating blade(s). For example, for mixing blade(s) that radially protrude twelve inches from the central rod, the radius is twelve inches, and the outlet is located at least twelve inches away from the outermost tip of the rotating blade(s). In this example, this also means that the outlet is located at least 24 inches away from the central rod. In some embodiments, the outlet is located at least one radius away from the outermost tip of the rotating blade(s) and also above the rotating blade(s) with respect to gravity. The orientation of the outlet and the distance away from the processing zone (the rotating blade(s)) can mitigate and/or prevent coal dust from being evacuated with the vapor by the vacuum pump. The intermittent agitation can also mitigate and/or prevent coal dust from being evacuated with the vapor by the vacuum pump. For example, by pausing the agitation intermittently, coal dust can be allowed to settle via gravity to mitigate and/or prevent coal dust from being evacuated with the vapor by the vacuum pump.


In some embodiments, a knockout pot is included between the outlet and the vacuum pump for collecting water. In some embodiments, a filter is included between the outlet and the vacuum pump for mitigating and/or preventing particulates from reaching the vacuum pump. In some embodiments, the filter is downstream of the knockout pot. In some embodiments, the filter is a single stage filter. In some embodiments, the filter is a multi-stage filter, such as a dual stage filter or a 3-stage filter. For example, the filter is a multi-stage filter having a 1st stage filter defining openings with a maximum dimension between 30 micrometers and 50 micrometers, a 2nd stage filter defining openings with a maximum dimension between 10 micrometers and 20 micrometers, and a 3rd stage filter defining openings with a maximum dimension between 2 micrometers and 10 micrometers.


Heat and/or vacuum exposure within the vessel can cause the coal to be reduced in size without requiring a time and/or energy-intensive process of mechanically reducing the coal (for example, by smashing or rigorous agitation using substantial force, and/or investing several hours of time to process). In some cases, the coal is pulverized into fines and/or dust within a short time (e.g., between 5-30 minutes) of being exposure to heat and vacuum within the vessel. In some embodiments, the coal is reduced to having an average primary particle size of less than 1 millimeter within a predetermined time. As used herein, a “primary particle size” refers to the longest linear dimension, e.g., a maximum length or a maximum diameter, of a primary particle. As used herein, a “primary particle” is an individual single particle, not an agglomeration of two or more particles. In some embodiments, a primary particle can be visually identified by microscopy and distinguished from agglomerations of two or more primary particles based on size, shape, or both.


In some embodiments, the coal is reduced to having an average primary particle size between 1 micrometer and 1 millimeter, between 1 micrometer and 500 micrometers, or between 1 micrometer and 100 micrometers. In some embodiments, the coal is reduced to having an average primary particle size of about or less than 100 micrometers (e.g., or about or less than 90 micrometers, 80 micrometers, 70 micrometers, 60 micrometers, 50 micrometers, 40 micrometers, 30 micrometers, 20 micrometers, 10 micrometers, 9 micrometers, 8 micrometers, 7 micrometers, 6 micrometers, 5 micrometers, 3 micrometers, or 1 micrometer).


In some embodiments, the predetermined time for achieving the desired average primary particle size is about or no more than 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 1 hour, 2 hours, or about or no more than 3 hours of being exposed to heat and/or vacuum within the vessel. The processed coal (fuel composition) can be mechanically forced through an extrusion die to yield a shaped fuel composition. The shaped fuel composition can be cut, shredded, or milled to form discrete portions of the fuel composition. In some cases, the discrete portions can include pellets or briquettes.


Thus, the coal is introduced to a single vessel, and processed by a low speed, mid to high torque mechanical blending while being exposed to heat. The coal can be processed in an uncrushed state. The processed coal typically has a moisture content of less than 3 wt %, less than 2 wt %, or less than 1 wt %, and a heat content between 9,000 BTU/lb and 11,000 BTU/lb, between 9,500 BTU/lb and 10,500 BTU/lb, or between 9,500 BTU/lb and 10,000 BTU/lb. In some embodiments, the fuel composition has a fixed carbon content between about 40 wt % and about 70 wt % or between about 50 wt % and about 60 wt %. In some embodiments, the fuel composition has an ash content between about 5 wt % and 20 wt % or between about 10 wt % and about 20 wt %. In some embodiments, the fuel composition has a volatiles content between about 40 wt % and about 70 wt %, between about 40 wt % and about 60 wt %, or between about 40 wt % and about 50 wt %.


In some embodiments, after the fuel composition has been formed, it is substantially free of coal dust (for example, the fuel composition is substantially free of coal particulates having an average size of 75 micrometers or smaller). The term “substantially free” can refer to the fuel composition containing less than 1 wt % (e.g., less than 0.5 wt %, less than 0.1 wt %, less than 0.01 wt %, or less than 0.001 wt %) of a material, such as coal dust. In some embodiments, after the fuel composition has been formed, it comprises less than 20 wt % coal dust, less than 15 wt % coal dust, less than 10 wt % coal dust, less than 5 wt % coal dust, less than 4 wt % coal dust, less than 3 wt % coal dust, less than 2 wt % coal dust, less than 1 wt % coal dust, less than 0.5 wt % coal dust, or less than 0.1 wt % coal dust. In some embodiments, after the fuel composition has been formed, it is substantially free of coal dust. In some embodiments, after the fuel composition has been formed, it releases less than 20 wt % coal dust, less than 15 wt % coal dust, less than 10 wt % coal dust, less than 5 wt % coal dust, less than 4 wt % coal dust, less than 3 wt % coal dust, less than 2 wt % coal dust, less than 1 wt % coal dust, less than 0.5 wt % coal dust, or less than 0.1 wt % coal dust.


The methods described herein can be implemented to convert unprocessed, uncrushed low rank coal into the fuel composition provided herein within 1 hour, within 55 minutes, within 50 minutes, within 45 minutes, within 40 minutes, within 35 minutes, within 30 minutes, within 25 minutes, or within 20 minutes.


Example

Uncrushed lignite coal taken directly from a Mississippi mine showed typical characteristics: 43.22 wt % moisture, 26.4 wt % volatiles, HHV of 5922 BTU/lb, 0.012 wt % sulfur, and 6.63 wt % ash. The composition of the uncrushed and unprocessed lignite coal is provided in Table 1.









TABLE 1







Composition of uncrushed lignite coal










Component
Amount (wt %)














Moisture
43.22



Carbon
34.96



Hydrogen
2.71



Nitrogen
0.65



Sulfur
0.012



Ash
6.63



Oxygen
11.82










The coal was exposed to heat ranging from 140-208° C. for a duration of approximately 60 minutes. The mechanism of heat transfer was conduction. Slow speed (up to 25 rpm), high torque mechanical blades were used to promote intermittent contact with the lignite, and a careful balance was maintained to reduce creation of coal dust. The mechanical blades were rotated intermittently, and the rotation speed varied between 0 rpm and 25 rpm with gradual increases and decreases. The rotation of the mechanical blades was paused (that is, no rotation) for time durations of between 1 minute and 2 minutes. The coal was kept in a vessel at all times, with intermittent exposure to vacuum. The vacuum was introduced (1) to remove oxygen and, thus, reduces the likelihood of ignition of the coal, (2) to promote thermal transformation, and (3) remove moisture from the coal. The pressure within the processing chamber, at various points during processing, was kept at 150 torr or less. The combination of heat and slow speed intermittent mechanical processing facilitated a natural breakdown of the coal.


Some of the processed lignite was removed from the heated chamber in a manner representative of rotating a drum/vessel/chamber and relying on gravity. Some of the processed lignite was mechanically removed from the chamber using a screw. Processing of the lignite resulted in a moisture reduction from 43.22 wt % to less than 1 wt % (0.84 wt % and 0.52 wt % for Samples 1 and 2, respectively) and an increase in energy content from 5922 BTU/lb to 9880 BTU/lb (HHV) and to 9941 BTU/lb (HHV) for Samples 1 and 2, respectively. Volatiles increased, as well as the sulfur portion. These changes are expected to result in improved combustion characteristics, ranging from better fuel burnout to lower CO2 emissions on a per GJ basis. The sulfur remained <1 wt % in Samples 1 and 2. The compositions of Samples 1 and 2 are provided in Table 2.









TABLE 2







Composition of Samples 1 and 2










Sample 1
Sample 2











Component
Amount (wt %)















Moisture
0.84
0.52



Carbon
57.45
58.68



Hydrogen
4.54
4.41



Nitrogen
1.11
1.16



Sulfur
0.055
0.492



Ash
16.11
16.36



Oxygen
19.90
18.38










As used in this disclosure, the terms “a,” “an,” or “the” are used to include one or more than one unless the context clearly dictates otherwise. The term “or” is used to refer to a nonexclusive “or” unless otherwise indicated. The statement “at least one of A and B” has the same meaning as “A, B, or A and B.” In addition, it is to be understood that the phraseology or terminology employed in this disclosure, and not otherwise defined, is for the purpose of description only and not of limitation. Any use of section headings is intended to aid reading of the document and is not to be interpreted as limiting; information that is relevant to a section heading may occur within or outside of that particular section.


As used in this disclosure, the term “about” or “approximately” can allow for a degree of variability in a value or range, for example, within 10%, within 5%, or within 1% of a stated value or of a stated limit of a range.


As used in this disclosure, the term “substantially” refers to a majority of, or mostly, as in at least about 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.99%, or at least about 99.999% or more.


Values expressed in a range format should be interpreted in a flexible manner to include not only the numerical values explicitly recited as the limits of the range, but also to include all the individual numerical values or sub-ranges encompassed within that range as if each numerical value and sub-range is explicitly recited. For example, a range of “between 0.1% and about 5%” or “between 0.1% and 5%” should be interpreted to include about 0.1% to about 5%, as well as the individual values (for example, 1%, 2%, 3%, and 4%) and the sub-ranges (for example, between 0.1% and 0.5%, between 1.1% and 2.2%, and between 3.3% and 4.4%) within the indicated range. The statements “X to Y” and “between X and Y” have the same meanings as “about X to about Y” and “between about X and about Y”, unless indicated otherwise. Likewise, the statement “X, Y, or Z” has the same meaning as “about X, about Y, or about Z,” unless indicated otherwise.


The details of one or more embodiments of the subject matter of this disclosure are set forth in the accompanying drawings and the description. Other features, aspects, and advantages of the subject matter will become apparent from the description, the drawings, and the claims.


Although this disclosure contains many specific embodiment details, these should not be construed as limitations on the scope of the subject matter or on the scope of what may be claimed, but rather as descriptions of features that may be specific to particular embodiments. Certain features that are described in this disclosure in the context of separate embodiments can also be implemented, in combination, in a single embodiment. Conversely, various features that are described in the context of a single embodiment can also be implemented in multiple embodiments, separately, or in any suitable sub-combination. Moreover, although previously described features may be described as acting in certain combinations and even initially claimed as such, one or more features from a claimed combination can, in some cases, be excised from the combination, and the claimed combination may be directed to a sub-combination or variation of a sub-combination.


Particular embodiments of the subject matter have been described. Other embodiments, alterations, and permutations of the described embodiments are within the scope of the following claims as will be apparent to those skilled in the art. While operations are depicted in the drawings or claims in a particular order, this should not be understood as requiring that such operations be performed in the particular order shown or in sequential order, or that all illustrated operations be performed (some operations may be considered optional), to achieve desirable results.


Accordingly, the previously described example embodiments do not define or constrain this disclosure. Other changes, substitutions, and alterations are also possible without departing from the spirit and scope of this disclosure.

Claims
  • 1. A method of processing coal, the method comprising: placing coal having a heat content between about 3,000 BTU/lb and about 9,000 BTU/lb and a moisture content between about 20 wt % and about 60 wt % in a vessel;heating the coal by conduction; andreducing a pressure in the vessel to below atmospheric pressure, thereby reducing the coal, such that an average primary particle size of the coal is less than 1 millimeter; andshaping the reduced coal to yield a fuel composition.
  • 2. The method of claim 1, wherein heating the coal comprises contacting the coal with a heated surface.
  • 3. The method of claim 2, wherein the heated surface comprises a rotating blade.
  • 4. The method of claim 3, wherein the rotating blade rotates at a rate between 2 and 25 revolutions per minute.
  • 5. The method of claim 1, wherein heating the coal comprises heating the coal to a temperature between 30° C. and 100° C.
  • 6. The method of claim 1, wherein heating the coal comprises heating the coal to a temperature up to about 250° C.
  • 7. The method of claim 1, wherein heating the coal comprises heating the coal to a temperature between 100° C. and 250° C., between 110° C. and 240° C., 120° C. and 230° C., between 130° C. and 220° C., or between 140° C. and 210° C.
  • 8. The method of claim 1, further comprising agitating the coal in the vessel by contacting the coal with a rotating blade.
  • 9. The method of claim 1, further comprising intermittently agitating the coal in the vessel.
  • 10. The method of claim 1, wherein reducing the pressure in the vessel comprises intermittently reducing the pressure in the vessel.
  • 11. The method of claim 1, wherein reducing the pressure in the vessel comprises reducing the pressure in the vessel to between 10 torr and 150 torr.
  • 12. The method of claim 1, wherein the coal placed in the vessel is uncrushed.
  • 13. The method of claim 1, wherein the coal placed in the vessel comprises lignite.
  • 14. The method of claim 1, wherein the coal placed in the vessel has a moisture content between 30 wt % and 60 wt %, or between 40 wt % and 50 wt %.
  • 15. The method of claim 1, wherein the fuel composition has a moisture content less than 3 wt %, less than 2 wt %, or less than 1 wt %.
  • 16. The method of claim 1, wherein the fuel composition has a heat content between 9,000 BTU/lb and 11,000 BTU/lb, between 9,500 BTU/lb and 10,500 BTU/lb, or between 9,500 BTU/lb and 10,000 BTU/lb.
  • 17. The method of claim 1, wherein the coal is not pyrolyzed in the vessel.
  • 18. The method of claim 1, wherein a heated fluid is not provided to the vessel.
  • 19. The method of claim 1, wherein the fuel composition is substantially free of fines.
  • 20. The method of claim 1, wherein shaping the reduced coal comprises: extruding the reduced coal to yield an extruded fuel product; andcutting, shredding, or milling the extruded fuel product to form discrete portions of the fuel composition.
CROSS-REFERENCE TO RELATED APPLICATIONS

This application claims the benefit of priority to U.S. Provisional Application No. 62/961,540 filed on Jan. 15, 2020, and entitled “PROCESSING OF LOW RANK COAL,” the contents of which are hereby incorporated by reference.

Provisional Applications (1)
Number Date Country
62961540 Jan 2020 US