None.
1. Field
The technology of the present application relates to ready mix concrete, and more specifically to ready mix concrete using recycled concrete aggregates.
2. Background
Using concrete for construction of roads, buildings, tarmacs, and the like has existed for centuries. Concrete provides a strong and formable building material. Because it is strong and formable, use of concrete in construction of roads, building, tarmacs, and the list has existed for centuries. While concrete can be formed of many materials, today's concrete typically includes a cement (most typically Portland cement in the United States), an aggregate (typically gravel and sand), and water admixture. Additional chemicals may be added depending on various features, such as hydration time, plasticizers, pigments, bonding agents, and the like.
Concrete can be mixed on-site in many applications. However, more and more frequently, project sites use what is typically known as “ready-mix concrete.” A manufacturing facility combines the cement, aggregate, and water admixture to the specifications of the job site and in accordance with American Society for Testing Materials (“ASTM”) requirements, which include international standards. The ASTM requirements define composition requirements for the concrete as well as strength and other requirements.
As one can appreciate, the ease and versatility of concrete has lead to an abundance of older structures. These structures are in various states of decay and/or in need of repair. While it is possible to tear down these structures and replace them with newer structures, the result is an abundance of concrete debris and rubble.
Thus, against this background, it would be desirable to develop a concrete that reuses or recycles used concrete debris and rubble.
Embodiments disclosed herein address the above stated needs by providing a method to make ready-mix concrete wherein at least 70% of the coarse aggregate is recycled. The method including the steps of loading raw material bins with material in predetermined mix proportions for a ready-mix concrete, the loaded raw material include at least coarse recycled aggregate. A mix proportion of raw materials is programmed in a controlling plant computer that weighs the raw materials necessary for the programmed mix proportion, the measured raw materials including a weight of coarse aggregate such that the weight of coarse aggregate comprises at least about 70% or more coarse recycled aggregate and the remaining weight comprises coarse virgin aggregate and a predetermined weight of cement and fly ash. Once weighed and measured, the raw materials are transferred to a batch mixer and mixed.
The technology of the present invention also provides mix proportions for ready-mix concrete such that at least 70% of the course aggregate comprises recycled aggregate. The mix comprising about 564 pounds of cement, about 141 pounds of fly ash, about 35.3 ounces of WRA, EUCON x15, about 1260 pounds of recycled 57 rock, about 420 pounds of virgin 57/67 rock, about 1260 pounds of sand, about 220 pounds of water, and AEA, Eucon air as need, wherein a ready-mix concrete is made having about 70% coarse recycled aggregate.
The technology of the present invention also provides mix proportions for ready-mix concrete such that at least 70% of the course aggregate comprises recycled aggregate. The mix comprising about 526 pounds of cement, about 132 pounds of fly ash, about 32.9 ounces of WRA, EUCON x15, about 1275 pounds of recycled 57 rock, about 425 pounds of virgin 57/67 rock, about 1275 pounds of sand, about 218 pounds of water, and AEA, Eucon air as need, wherein a ready-mix concrete is made having about 70% coarse recycled aggregate.
The technology of the present invention also provides mix proportions for ready-mix concrete such that at least 70% of the course aggregate comprises recycled aggregate. The mix comprising about 489 pounds of cement, about 122 pounds of fly ash, about 30.6 ounces of WRA, EUCON x15, about 1290 pounds of recycled 57 rock, about 430 pounds of virgin 57/67 rocks, about 1290 pounds of sand, about 216 pounds of water, and AEA, Eucon air as needed, wherein a ready-mix concrete is made having about 70% coarse recycled aggregate.
The technology of the present invention also provides mix proportions for ready-mix concrete such that at least 70% of the course. aggregate comprises recycled, aggregate. The mix comprising about 451 pounds of cement, about 113 pounds of fly ash, about 28.2 ounces of WRA, EUCON x15, about 1295, pounds of recycled 57 rock, about 435 pounds of virgin 57/67 rock, about 1300 pounds of sand, about 205 pounds of water, and AEA, Eucon air as needed, wherein a ready-mix concrete is made having about 70% coarse recycled aggregate.
The technology of the present application will now be explained. The technology will be explained with reference to particular composition, material, strength, and other requirements. As mentioned above, the reference is typically associated with an ASTM standard for a particular type of concrete. While a specific material may be called out, such as, for example, cement, mountain, type I/II L.A., at a particular poundage, such as, for example, 564 lbs, one of skill in the art would recognize that the particular composition called for is within a particular tolerance as defined by the ASTM standard. Thus, the present application may state the material as about 564 lbs of cement, mountain, type I/II L.A. wherein the term about, approximately, or similar term should be understood to mean within the tolerance as allowed by the existing ASTM standard as they currently exist and change from time to time. Moreover, the technology of the present invention will be explained with particular reference to exemplary embodiments and admixtures. The word “exemplary” is used herein to mean “serving as an example, instance, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments. Moreover, embodiments described herein should be construed as exemplary unless explicitly stated otherwise.
ASTM standard means any ASTM standard relating to concrete including ASTM C 94 relating to ready-mix concrete and ASTM C685 relating to concrete made by volumetric batching and continuous mixing to name but two of the numerous ASTM standards relevant to ready-mix concrete.
Generally speaking, concrete comprising, among other things, recycled material has been frowned upon in the industry because of many detrimental effects. Typically, using recycled material reduces, for example, the strength of the concrete. Additionally, the ready-mix concrete manufacturers have shunned using recycled material because of the abundance of virgin materials available to most ready-mix facilities.
Particularly shunned in the past was the recycling of aggregate material, i.e., sand and rock. It has been found, however, that in proper combinations recycling aggregate materials provides unexpected benefits to the ready-mix concrete. For example, using recycled sand not only reduces the need for virgin materials, which provides an environmental benefit, but also provides recycled cement that can be used for the gravel or rock portion of the aggregate. The recycled cement results from the crushing and screening operations to extract the recyclable sand.
Recycling concrete into the gravel or stone for ready-mix concrete also provides unexpected benefit to the ready-mix concrete. Generally, recycled concrete that has been crushed, screened and filtered to the appropriate size generally provides a lighter mixture per volume than non-recycled gravel or stone. Also, crushed concrete typically is a fractured face material that typically increases the strength of concrete using a similar recipe. Reducing the weight and increasing the strength allows for the carrying of a larger payload and allows less material for a similar cubic volume, which reduces overall resources.
While both recycled sand and recycled gravel or stone provide increased benefits, it has been found that particular combinations of materials work well. In one particular embodiment, it has been found combining about 30% recycled gravel or stone with 70% virgin stone provides a satisfactory admixture. Some sample embodiments suing this combination include the following ready-mix concretes:
Example 1 is a 30% coarse recycled aggregate ready-mix concrete comprising, in combination:
The above and below combinations (for both 30% coarse recycled aggregate and 70% coarse recycled aggregate) are based on pre-mix weights (with are allowed to be within a tolerance, such tolerance will be designated as about or approximately), in other words, the mix proportions are largely saturated, surface dry condition based weights and amounts. The AEA, Eucon Air 40 for both the 30% and 70% coarse recycled aggregate described above and below would be supplied consistent with conventional techniques for adding air to the mix and as it is well within the ordinary skill of the art for someone making ready-mix concrete, it will not be explained herein.
Using the above ready-mix concrete, the final product will generally provide satisfactory results for ASTM testing standards. For example, one batch provided a unit weight of concrete under ASTM C 138 as 143.4 pcf. A yield under ASTM C 138 of 27.27 ft cubed. A slump under ASTM C 143 of 3¼ inches. An air content under ASTM C 231 of 5.4% and a water/cementitious ration of 0.43 at 74° F.
A second embodiment of 30% coarse recycled aggregate ready-mix concrete includes, in combination:
A third embodiment of 30% coarse recycled aggregate ready-mix concrete includes, in combination:
A fourth embodiment of 30% coarse recycled aggregate ready-mix concrete includes, in combination:
A fifth embodiment of 30% coarse recycled aggregate ready-mix concrete includes, in combination:
A sixth embodiment of 30% coarse recycled aggregate ready-mix concrete includes, in combination:
While the above six embodiments are provided, one of ordinary skill in the art will recognize and understand other combinations resulting in other mix proportions are possible.
Another combination that has been discovered to work particularly well includes a combination of about 70% recycled gravel or stone with 30% virgin stone. Some particular admixtures include the following ready-mix concretes.
A first embodiment of a 70% coarse recycled aggregate ready-mix concrete includes, in combination:
A second embodiment of a 70% coarse recycled aggregate ready-mix concrete includes, in combination:
A third embodiment of a 70% coarse recycled aggregate ready-mix concrete includes, in combination:
A fourth embodiment of a 70% coarse recycled aggregate ready-mix concrete includes, in combination:
While the above ready-mix concretes were made using 100% virgin sands, it is believed any amount of recycled sand from 0% to 20% could be used in place of or in combination with virgin sand.
Referring now to
Next, the raw materials are loaded into storage bins, step 104. A mix proportion is set in a controlling plant computer, step 106. While described in relation to preparing a single mix of ready-mix concrete, one of ordinary skill in the art will recognize on reading the disclosure that a plant typically batch loads mix proportions into the controlling plant computer to run numerous mixes automatically. Optionally, once the mix proportions are set, the controlling plant computer may check the appropriate raw materials are loaded in the bins, step 108. A delivery vehicle, typically a truck, is located at the plant outlet to receive the ready-mix concrete once the batch is prepared, step 110. Next, the controlling plant computer operates bin valves or gates to cause each bin to unload material onto an associated scale until an appropriate amount of material is measured, step 112. Once measured, the raw material is transferred to the truck, step 114. The truck mixes the raw material, typically 120 revolutions of the truck holder, step 116. Optionally, after the revolutions, the batch of ready-mix concrete is checked for quality, step 118, and delivered to the appropriate site, step 118.
The previous description of the disclosed embodiments is provided to enable any person skilled in the art to make or use the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the generic principles defined herein may be applied to other embodiments without departing from the spirit or scope of the invention. Thus, the present invention is not intended to be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
The present application claims priority to the pending United States provisional patent application Ser. No. 60/971,800, titled READY-MIX CONCRETE USING RECYCLED CONCRETE AGGREGATE, filed Sep. 12, 2007, the specification of which is incorporated herein as if set out in full.
Number | Date | Country | |
---|---|---|---|