Railway cars typically consist of a rail car that rests upon a pair of truck assemblies. The truck assemblies include a pair of side frames and wheelsets connected together via a bolster and damping system. The car rests upon the center bowl of the bolster, which acts as a point of rotation for the truck system. The car body movements are reacted through the springs and friction wedge dampers, which connect the bolster and side frames. The side frames include pedestals that each define a jaw into which a wheel assembly of a wheel set is positioned using a roller bearing adapter.
The side frames and bolsters may be formed via various casting techniques. The most common technique for producing these components is through sand casting. Sand casting offers a low cost, high production method for forming complex hollow shapes such as side frames and bolsters. In a typical sand casting operation, (1) a mold is formed by packing sand around a pattern, which generally includes the gating system; (2) The pattern is removed from the mold; (3) cores are placed into the mold, which is closed; (4) the mold is filled with hot liquid metal through the gating; (5) the metal is allowed to cool in the mold; (6) the solidified metal referred to as raw casting is removed by breaking away the mold; (7) and the casting is finished and cleaned which may include the use of grinders, welders, heat treatment, and machining.
In a sand casting operation, the mold is created using sand as a base material, mixed with a binder to retain the shape. The mold is created in two halves —cope (top) and drag (bottom) which are separated along the parting line. The sand is packed around the pattern and retains the shape of the pattern after it is extracted from the mold. Draft angles of 3 degrees or more are machined into the pattern to ensure the pattern releases from the mold during extraction. In some sand casting operations, a flask is used to support the sand during the molding process through the pouring process. Cores are inserted into the mold and the cope is placed on the drag to close the mold.
When casting a complex or hollow part, cores are used to define the hollow interior, or complex sections that cannot otherwise be created with the pattern. These cores are typically created by molding sand and binder in a box shaped as the feature being created with the core. These core boxes are either manually packed, or created using a core blower. The cores are removed from the box, and placed into the mold. The cores are located in the mold using core prints to guide the placement, and prevent the core from shifting while the metal is poured. Additionally, chaplets may be used to support or restrain the movement of cores, and fuse into the base metal during solidification.
The mold typically contains the gating system which provides a path for the molten metal, and controls the flow of metal into the cavity. This gating consists of a sprue, which controls metal flow velocity, and connects to the runners. The runners are channels for metal to flow through the gates into the cavity. The gates control flow rates into the cavity, and prevent turbulence of the liquid.
After the metal has been poured into the mold, the casting cools and shrinks as it approaches a solid state. As the metal shrinks, additional liquid metal must continue to feed the areas that contract, or voids will be present in the final part. In areas of high contraction, risers are placed in the mold to provide a secondary reservoir to be filled during pouring. These risers are the last areas to solidify, and thereby allow the contents to remain in the liquid state longer than the cavity of the part being cast. As the contents of the cavity cool, the risers feed the areas of contraction, ensuring a solid final casting is produced. Risers that are open on the top of the cope mold can also act as vents for gases to escape during pouring and cooling.
In the various casting techniques, different sand binders are used to allow the sand to retain the pattern shape. These binders have a large affect on the final product, as they control the dimensional stability, surface finish, and casting detail achievable in each specific process. The two most typical sand casting methods include (1) green sand, consisting of silica sand, organic binders and water; and (2) chemical or resin binder material consisting of silica sand and fast curing chemical binding adhesives such as phenolic urethane. Traditionally, side frames and bolsters have been created using the green sand process, due to the lower cost associated with the molding materials. While this method has been effective at producing these components for many years, there are disadvantages to this process.
Side frames and bolsters produced via the green sand operation above have several problems. First, relatively large draft angles required in the patterns result in corresponding draft angles in the cast items. In areas where flat sections are required, such as the pedestal area on the side frames, and friction shoe pockets on the bolster, cores must be used to create these features. These cores have a tendency to shift and float during pouring. This movement can result in inconsistent final product dimensions, increased finishing time, or scrapping of the component if outside specified dimensions. Other problems with these casting operations will become apparent upon reading the description below.
An object of the invention is to provide a method of manufacturing a side frame mold for casting a side frame of a railway car truck. The side frame includes forward and rearward pedestal jaws for mounting a wheel assembly from a wheel set. The method includes forming a drag and a cope portion of a mold from a casting material to define an exterior surface of a drag portion and cope portion, respectively, of the side frame. The mold includes a portion for casting a pedestal area of the side frame, including the pedestal roof, contact surfaces, outer vertical jaw, and inner vertical jaw. The drag and the cope portions are then cured.
Another object of the invention is to provide a method for manufacturing cores utilized in conjunction with a mold for casting a side frame of a railway car truck, where the side frame includes forward and rearward pedestal jaws for mounting a wheel assembly from a wheel set, and wherein each pedestal portion extends from a respective end of the side frame to a bolster opening of the side frame. The method includes forming separate drag and cope portions of at least one pedestal core. The drag and cope portions of the pedestal core define an interior region of at least one pedestal of the side frame. The method further includes attaching the drag and cope portions of the pedestal core together to form a pedestal core assembly to be inserted into the mold.
Yet another object of the invention is to provide a method of manufacturing a side frame of a railway car truck, where the side frame includes forward and rearward pedestal jaws for mounting a wheel assembly from a wheel set. The method includes providing a mold that defines an exterior surface and at least one pedestal jaw of a drag portion and cope portion, respectively, of the mold. Next, molten steel is poured into the mold and allowed to solidify. The cast side frame is removed from the mold, and consists of the final part, risers, and gating. Excess material is ground off of the cast side frame to form a finished side frame. The amount of excess material removed from the casting, in the form of core seams, parting line flash, risers, rigging, and vents, is less than 10% of the gross weight of steel originally poured into the side frame mold.
Yet another object of the invention is to provide a side frame of a railway car truck that includes a pair of side frame columns that define a bolster opening, and a pair of pedestals that extend away from respective side frame columns. Each pedestal defines a jaw configured to attach to a wheel assembly from a wheel set. The side frame includes a first rib positioned on an inner side of each of the side frame columns that is opposite to a bolster side of the side frame column. An opening is defined in each side frame column. The opening extends from the bolster side to the inner side of a respective side frame column. The opening extends through the first rib and is sized to receive a bolt for securing a wear plate to the bolster side of the side frame column.
Yet another object of the invention is to provide a method for manufacturing a bolster of a railway car truck. The method includes providing a drag portion and a cope portion of a mold. In a main body section of the mold, a parting line that separates the drag portion from the cope portion is substantially centered between portions of the mold that define brake window openings in sides of the bolster. The method further includes inserting one or more cores into the mold, and casting the bolster.
Yet another object of the invention is to provide a core assembly for use in manufacturing a bolster of a railway car truck. The core assembly includes a main body core that defines substantially an entire interior region of the bolster that extends from a center of the bolster towards inward gibs positioned at outboard end sections of the bolster, and that partially defines an interior end section of the bolster that extends from the inward gibs towards outboard ends of the bolster. The core assembly also includes end cores that define an interior region of the end section of the bolster that is not defined by the main body core.
Yet another object of the invention is to provide a method of manufacturing a bolster mold for casting a bolster of a railway car truck. The method includes forming a drag and a cope portion of a mold from a casting material to define an exterior surface of a drag portion and cope portion, respectively, of the bolster. A parting line that separates the drag portion from the cope portion is substantially centered between portions of the mold that define brake window openings in sides of the bolster. The method also includes curing the drag and the cope portion.
Yet another object of the invention is to provide a core assembly for use in manufacturing a bolster of a railway car truck. The core assembly includes a main body core that defines substantially an entire interior region of the bolster the extends from a center of the bolster towards inward gibs positioned at outboard end sections of the bolster, and that partially defines an interior end section of the bolster that extends from the inward gibs towards respective ends of the bolster. The assembly also includes end cores that define an interior region of the end section of the bolster that is not defined by the main body core.
Yet another object of the invention is to provide a method of manufacturing a bolster mold for casting a bolster of a railway car truck. The method includes forming a drag and a cope portion of a mold from a casting material to define an exterior surface of a drag portion and cope portion, respectively, of the bolster. A parting line that separates the drag portion from the cope portion is substantially centered between portions of the mold that define brake window openings in sides of the bolster. The method further includes curing the drag and the cope portion.
Yet another object of the invention is to provide a method of manufacturing a bolster of a railway car truck. The method includes providing a mold that includes a drag portion and a cope portion. A parting line that separates the drag portion from the cope portion is substantially centered between portions of the mold that define brake window openings in sides of the bolster. The method further includes pouring a molten steel into the mold and allowing it solidify. The cast bolster is then removed from the mold, and consists of the final bolster part, risers, and gating system. Excess material is ground off of the cast bolster to form a finished bolster. The amount of excess material removed from the casting, in the form of core seams, risers, and gating, is less than 15% of the gross weight of steel originally poured into the bolster mold.
Yet another of the invention is to provide a method for manufacturing a bolster of a railway car truck includes providing a drag portion and a cope portion of a mold. In a main body section of the mold, a parting line that separates the drag portion from the cope portion is substantially centered between portions of the mold that define brake window openings in sides of the bolster. One or more cores are inserted into the mold and a molten material is poured into the mold to thereby cast the bolster.
Yet another of the invention is to provide a method of manufacturing a side frame of a rail car, where the side frame defines an opening through which a bolster is positioned. The opening is defined by a pair of facing columns, a spring seat, and a compression member. A side frame pattern for forming a drag portion and cope portion of a mold is provide along with one or more cores that define an interior region of a cast side frame. Herein the side frame pattern and one or more cores are configured to constrain a spacing between facing columns to within a tolerance about ±0.038 inches.
Yet another of the invention is to provide a method of manufacturing a side frame of a rail car that includes providing a side frame pattern for forming a drag portion and cope portion of a mold; and providing one or more cores that define an interior region of a cast side frame, wherein at least some of the one or more cores define one or more core prints for positioning the one or more cores within the drag portion of the mold. A distance between an outside surface of the one or more core prints and a surface of the drag portion of the mold that is closest to the outside surface of the one or more core prints is less than or equal to about 0.030 inches.
Yet another of the invention is to provide a method of manufacturing a bolster of a rail car that includes a pair of shoe pockets at respective ends configured to be inserted into bolster openings of respective side frames. The method includes providing a bolster pattern for forming a drag portion and cope portion of a mold; and providing one or more cores that define an interior region of a cast bolster. The bolster pattern and one or more cores are configured to constrain shoe pocket angles within a tolerance of about ±0.5°.
Yet another of the invention is to provide a method of manufacturing a bolster of a rail car that includes a pair of shoe pockets at respective ends configured to be inserted into bolster openings of side frame. The method includes providing a bolster pattern for forming a drag portion and cope portion of a mold; and providing one or more cores that define an interior region of a cast bolster. The bolster pattern and one or more cores are configured to constrain a width between the pair of shoe pockets to within a tolerance of about ±0.063 inches.
Yet another of the invention is to provide a method of manufacturing a bolster of a rail car. The method includes providing a bolster pattern for forming a drag portion and cope portion of a mold; and providing one or more cores that define an interior region of a cast bolster. At least some of the one or more cores define one or more core prints for positioning the one or more cores within the drag portion of the mold. A distance between an outside surface of the one or more core prints and a surface of the drag portion of the mold that is closest to the outside surface of the one or more core prints is less than or equal to about 0.030 inches.
Yet another of the invention is to provide a mold for casting a side frame of a railway car truck. The side frame includes forward and rearward pedestal jaws for mounting a wheel assembly from a wheel set, the mold comprising. A drag and a cope portion are formed from a molding material to define an exterior surface of a drag portion and cope portion, respectively, of the side frame. The mold includes a portion for casting at least one pedestal jaw of the side frame.
Yet another of the invention is to provide a bolster of a railway car truck formed from a mold. The bolster includes a drag portion and a cope portion. A parting line that defines the drag portion and the cope portion is configured such that in a main body section of the bolster the parting line is substantially centered between brake window openings in sides of the bolster.
Yet another of the invention is to provide a mold for manufacturing a bolster of a railway car truck. The mold includes a drag portion and a cope portion. A parting line that separates the drag portion and the cope portion is configured such that the parting line is substantially centered between portions of the mold that define brake window openings in sides of the bolster.
Yet another of the invention is to provide a bolster of a railway car truck formed from a mold. The bolster includes a drag portion and a cope portion. A parting line that defines the drag portion and the cope portion is configured such that at outboard end sections are substantially defined by the drag portion.
Yet another of the invention is to provide a mold for manufacturing a bolster of a railway car truck. The mold includes a drag portion and a cope portion. Respective mating surfaces of the drag and cope portions have a non-planar complementary shape.
Other features and advantages will be, or will become, apparent to one with skill in the art upon examination of the following figures and detailed description. It is intended that all such additional features and advantages included within this description be within the scope of the claims, and be protected by the following claims.
The accompanying drawings are included to provide a further understanding of the claims, are incorporated in, and constitute a part of this specification. The detailed description and illustrated embodiments described serve to explain the principles defined by the claims.
The bolster opening 110 is defined by a pair of side frame columns 120, a compression member 125, and a spring seat 127. The bolster opening 110 is sized to receive an outboard end section 705 (
A pair of wear plates 135 are positioned between shoe pockets 710 of the outboard end sections 705 of the bolster 700 and the side frame columns 120. A single exemplary wear plate 135 is illustrated in
In operation, pressure is produced against the wear plates 135 by the movement of the bolster 700 within the bolster opening 110. In known side frames, the side frame columns 120 tend to elastically deform under these wedge pressures. As a result, the fasteners securing the wear plates 135 to the side frame columns 120 become loose. To overcome these problems, an embodiment of the side frame 100 of the application includes column stiffeners 205 (
Returning to
At block 400, a mold 500 for manufacturing the side frame 100 may be formed. Referring to
The respective portions may be formed by first providing first and second patterns (not shown) that define an outside perimeter of the drag side 102 and cope side 103, respectively, of the side frame 100. The patterns may partially define one or more feed paths 540 for distribution of molten material within the mold 500. The one or more feed paths 540 are advantageously positioned in a center region of the mold 500, which results in an even distribution of the molten material throughout the mold 500. For example, the feed paths 540 may be positioned in an area of the mold 500 that defines the bolster opening 110 of the side frame 100.
The patterns (not shown) also define a pedestal jaw portion 520 that defines the pedestal jaw 140 of the side frame 100. In known forming methods, the patterns do not define the details of the pedestal jaw 140. Instead, a core having the general shape of the inner area of the pedestal jaw 140 is inserted into the mold prior to casting. The cores tend to move during the casting process resulting in inaccurate dimensions, large core seams that have to be removed.
The pattern above and a group of risers 535 may then be inserted into respective flasks 525 and 526 for holding a molding material 527. The risers 535 may inserted in the cope portion 510. The risers 535 correspond to hollow cylindrical structures into which molten material fills during casting operations. The risers 535 are positioned at areas of the mold that correspond to thicker areas of the side frame that cool more slowly than other areas of the side frame. The risers 535 function as reservoirs of molten material that compensate for contraction that occurs in the molten material as the molten material cools, and thus prevent shrinkage, or hot tearing of the cast side frame in the thicker areas that might otherwise occur. Exemplary risers 550 for the side frame 100 are illustrated in
In known casting operations, the precise locations requiring accurate feeding are not generally known. Therefore, relatively large risers (e.g., 6 inches or more) that cover larger areas are utilized. By contrast, in the disclosed embodiments, the precise locations requiring accurate feeding have been determined via various analytical techniques, as described below. As a result, risers 435 that are considerably smaller in diameter (e.g., about 4 inches or smaller) may be utilized, which improve the yield of the casting. The riser heights may be between about 4 and 6 inches. In one embodiment, less than 10% of the gross weight of the casting material poured into the mold ends up in the risers. This leads to more efficient use of the casting material.
The flasks 525 and 527 are generally sized to follow the shape of the pattern, which is different than flasks utilized in known casting operations. These flasks are generally sized to accommodate the largest cast item in a casting operation. For example, in known casting operations, the flask may be sized to accommodate a bolster or an even larger item. By contrast, as illustrated in
A molding material 527 is then packed into the flask 525 and over and around the pattern until the flasks 525 are filled. The molding material 527 is then screeded or leveled off with the flask, and then cured to harden the molding material 527. The patterns are removed once the molding material 527 cures.
The molding material 527 may correspond to a chemical or resin binder material such as phenolic urethane, rather than green-sand products utilized in known casting operations. The chemical binder material product enables forming molds with greater precision and finer details.
To facilitate removal of the patterns (not shown), sides of the respective cavities in the drag and cope portions of the mold 500 are formed with a draft angle D 515 of 1°, ¾°, or even less to prevent damage to the mold 500 when removing the pattern. The draft angle of the mold forms a corresponding draft angle D 305 along sides of the side frame 100. The draft angle formed on most surfaces of the side frame 100 may be of little consequence. However, in certain regions, such as the contact surfaces 115 of the pedestal jaws 140 draft angles of greater than 1° may not be tolerated. The chemical or resin binder material such as phenolic urethane facilitates forming sides with draft angles of 1° or less versus green-sand products, for which draft angles of 3° or greater are required to prevent damaging the mold. In the pedestal jaws 140 green-sand products require additional cores to create these features to maintain flatness requirements. These cores create large seams and dimensional variation among castings.
At block 405, a core assembly 545 that defines the interior region of the side frame 100 is formed. Referring to
The pedestal core 605 may define one or more core prints that form openings in the cast side frame. For example, a first set of core prints 630 may form openings at the ends of the pedestal that correspond to ends of the side frame. A second core print 632 may form openings in the diagonal tension members 141 (
For example, a mold that includes a cope and drag portion that defines a given core may be formed. Molding sand may be inserted into the core box and cured. The core box is then removed to reveal the cured core. The respective cores may be formed individually, integrally, or in some combination thereof. The respective cores may be formed as two portions. For example, each core (i.e., pedestal core, bolster core, etc.) may include a cope portion and a drag portion formed separately in separate core boxes (i.e., a cope mold and drag mold). After curing, the formed portions may be attached. For example, the cope and drag portions of a given core may be glued together to form the core.
At block 410, the core assembly 545 is inserted in the mold and the side frame 100 is cast. For example, the core assembly 545 may be inserted into the drag portion 505 of the mold 500. The cope portion 510 may be placed over the drag portion 505 and secured to the drag portion 505 via clamps, straps, and the like. In this regard, locating features may be formed in the drag portion 505 and the cope portion 510 to ensure precise alignment of the respective portions.
After securing the respective portions, molten material, such as molten steel, is poured into the mold 500 via an opening in the cope portion 510. The molten material then flows through the gating 540 and throughout the mold 500 in the space between the mold 500 and the core assembly 545.
At block 415, the mold 500 is removed from the side frame 100 and the side frame 100 is finished. For example, the contact surfaces 115 are machined to remove portions of the residual draft angle D 305 produced as a result of the draft angle D 515 of the mold. Other material may be removed. For example, riser material formed in the risers 535 is removed. In some implementations, the mold 500 is configured so that a wedge or recess is formed in riser material just beyond the side of the side frame 100. The wedge or recess enables hammering the riser material off, rather than more time consuming flame cutting utilized in known casting operations.
As shown by the various operations, the side frames 100 may be produced with a minimum of wasted material and time. For example, the flask configurations minimize the amount of casting material needed to form the mold 500. Smaller risers result in the removal of less material (i.e., solidified steel) during finishing. The precision of the mold enables, for example, producing dimensionally accurate pedestal jaws. These improvements result in removal of less than 10% of the material during finishing.
In addition to these advantages, other advantages are realized. For example, as noted above, the flasks 525 and 526 are not required when casting the side frame 100. Therefore, the flasks 525 and 526 may be utilized to form new molds while a given side frame 100 is being cast.
As noted above, various analytic techniques may be utilized to precisely determine various dimensions. To achieve tolerances narrower than normally achievable for green sand, or chemical or resin binder material such as phenolic urethane molding, an iterative process of casting and three-dimensional scanning to measure critical dimensions and variability is utilized. This approach may be utilized throughout the manufacturing of the core boxes, patterns, manufacturing cores, manufacturing cope and drag mold portions, and casting the final part. By accurately measuring each step of the process, the exact shrink rates are known in all three directions (i.e., vertical, longitudinal, lateral) as well as how well the cores and mold collapse during solidification.
In one implementation, the scanning may be performed with a 3D point cloud scanner, such as a Z Scanner, Faro Laser Scanner, or a similar device. 3D point cloud data may be analyzed in software such as Geomagic®, Cam2®, and Solidworks® to measure and compare the tooling, cores, and final parts. These comparisons may be utilized to calculate actual casting shrink, which is usually expressed as a percentage. For example, typical pattern maker shrink allowance for a carbon steel casting may be about 1.56%. This typical shrink allowance is not exact, and varies depending on the complexity of the shape being cast. In some cases, shrink allowance may be as much as 2%. For large castings, such as a side frame or bolster, this range of shrink allowance may create casting differences of up to 0.5″, and therefore out of tolerance. In the described embodiments, the actual shrinkage rates in vertical, longitudinal, and lateral directions were determined using this process, and is reflected in the tooling dimensions.
In addition to calculating the shrink of the casting as it cools, it is important to understand how the cores and mold collapse during solidification. Controlling the collapsibility of the cores and mold can control the range of tolerances achieved. This can be achieved through a combination of molding materials, and geometry of the core and mold. For critical side frame dimensions, such as column spacing A 170 (
In addition to determining the range of manufacturing variance achieved of the molds and cores for calculating shrink and collapse, core print sizes may be reduced. Reducing the clearance between the interface between the core print in the mold and core protrusion reduces core movement during pouring. Less core movement creates more accurate wall thicknesses and part tolerances. In addition to the accuracy of the mold and tooling tolerances, a controlled amount of mold wash has been achieved to minimize the variance of core print dimensions. The clearance used in this process was 0.030″, wherein the mold was 0.030″ larger than the inserting protrusion created in the core, as illustrated by dimension F 561, which illustrates a cross section taken along section 555 (
Another advantage of these operations is that the surface finish of the cast side frame is smoother than in known casting operations. The smoother the surface, the greater the fatigue life of the part. The operations above facilitate manufacturing side frames with a surface finish less than about 750 micro-inches RMS, and with a pedestal surface finish that is less than about 500 micro-inches RMS.
Each outboard end section 705 includes a pair of friction shoe pockets 710. The surfaces of the respective shoe pockets 710 are known to be a critical area of the bolster 700 from a finishing perspective as the shoe pockets 705 are configured to abut the wear plates 135 and cooperate with the wear plates 135 to function as shock absorbers, as described above. There are wedges which are assembled into the shoe pockets, and the wedges wear against the column guide wear plates.
As described above, the main body section 715 of the bolster 700 defines a pair of brake window openings 725 configured to enable the use of brake rigging. These windows also act as core prints to support the main body core in the mold.
The bolster 700 may be formed in a manner similar to that of the side frame 100. For example, cope and drag sections of a mold may be formed from a casting material, such as a chemical or resin binder material such as phenolic urethane. Patterns that define the exterior of the respective cope and drag sections of the bolster 700 may be utilized to form respective cavities in the cope and drag sections of the mold. The draft angles of the sides of the patterns may be 1° or less. As in the side frame, flasks for forming the mold may be sized to follow the shape of a pattern that defines the bolster. A flask configured in this manner minimizes the amount of molding material needed to cast a bolster. For example, in some embodiments, the ratio of the molding sand to the molten material poured into the mold in subsequent operations may be less than 3:1. This is an important consideration given that the mold may only be used a single time when casting.
Risers 805 (
In known casting operations, the entire parting line forms a plane that cuts through the bolster. For example, the parting line may extend between the end sections and may be centered within the end sections such that the parting line bisects the shoe pockets and passes through the upper portions of the brake windows. In green sand, pockets are created with cores, because the operation cannot create this shape.
Configuring the parting line according to the disclosed embodiments has several advantages over known parting line configurations. For example, the upper and lower portions of the respective brake windows are known to be regions of high stress. Placement of the parting line near such locations, as is the case in known configurations, renders the bolster more susceptible to higher stresses. By contrast, in the disclosed embodiments, the parting line 905 is positioned in the middle of the brake window openings 720 where the stress is lower. The parting line of the mold is also in the same location as the parting line of the cores. This allows for uniform wall thicknesses of the side walls, thereby promoting even cooling of the casting.
No finishing of the shoe pockets 710 is required because the parting line does not pass through the shoe pockets 710. In known parting line configurations, the parting line may be a straight line that bi-sects the bolster and passes through a middle region of the shoe pockets. This may necessitate finishing of the core seams surrounding the shoe pockets. However, the disclosed parting line is configured to be above the shoe pockets 710. That is, the shoe pockets 710 are formed entirely in either the cope or the drag portion of the mold. As noted earlier, the shoe pockets 710 are a more critical region of the bolster 700. Therefore, elimination of a finishing operation is advantageous.
The cross-sectional thickness of the bolster is more symmetrical about the parting line 905. As noted above, patterns are utilized to form cavities in the drag and cope portions of the mold. The patterns are formed with draft angles to enable removal of the patterns from the mold. Core boxes are used to create the cores defining the inside of the bolster. The two halves of the core boxes meet at a parting line, from which draft angles also extend to allow the removal of the core. Where the parting lines of a core, and parting line of a mold do not match, non-uniform wall thicknesses occur. Placing the parting line towards the top of the bolster, as is the case in known parting line configurations, results in a non-uniform thickness in the cross-section of the bolster. The non-uniform thickness results in the utilization of excess material in casting the bolster. This non-uniform thickness also prevents uniform cooling, and may allow shrinkage and voids to be present. To prevent shrinkage and voids from occurring, large risers to feed the critical sections must be used. By contrast, positioning the parting line 905 as disclosed enables the formation of a bolster 700 with a symmetrical side wall thickness about the parting line 905 as illustrated by thicknesses T1 1005 and T2 1010 in
Another advantage of the disclosed parting line 905 configuration is that it enables easy alignment of the drag and cope portions of the mold. In known molding operations, locating features, such as pins and openings, are arranged within the drag and cope flask portions to align the two portions. Any amount of misalignment in the locating features results in misalignment between the drag portion and cope portion of the bolsters. The described parting line 405, however, is keyed by virtue of the geometry of the parting line 405 and the drag portion and cope portion essentially interlock with one another in such a manner that the two portions self-align. As a result, pins and bushings known in art are not necessary to maintain alignment of the drag and cope portions.
After forming the drag and cope portions, one or more cores 1100 that define an interior of the bolster 700 are formed. Referring to
The techniques described above with respect to a side frame for constraining the tolerance of various dimensions may be applied to the bolster. For critical bolster dimensions such as shoe pocket angles N 1020 (
The distance H 950 (
Another advantage of these operations is that the surface finish of the cast bolster is smoother than in known casting operations. The smoother the surface, the greater the fatigue life of the part. The operations above facilitate manufacturing bolsters with a surface finish less than about 750 micro-inches RMS, and with shoe pockets with a surface finish less than about 500 micro-inches RMS.
While various embodiments of the embodiments have been described, it will be apparent to those of ordinary skill in the art that many more embodiments and implementations are possible that are within the scope of the claims. The various dimensions described above are merely exemplary and may be changed as necessary. Accordingly, it will be apparent to those of ordinary skill in the art that many more embodiments and implementations are possible that are within the scope of the claims. Therefore, the embodiments described are only provided to aid in understanding the claims and do not limit the scope of the claims.
Number | Name | Date | Kind |
---|---|---|---|
1746301 | Bettendorf | Feb 1930 | A |
1750344 | Bettendorf | Mar 1930 | A |
1990095 | Rohlfing | Feb 1935 | A |
2014224 | Campbell | Sep 1935 | A |
3218989 | Kreiner et al. | Nov 1965 | A |
3254613 | Weber | Jun 1966 | A |
3320904 | Weber | May 1967 | A |
3339498 | Weber | Sep 1967 | A |
3446265 | Buck, Jr. | May 1969 | A |
3461814 | Weber et al. | Aug 1969 | A |
3461815 | Gedris et al. | Aug 1969 | A |
3517620 | Weber | Jun 1970 | A |
3559589 | Williams | Feb 1971 | A |
3575117 | Tack | Apr 1971 | A |
3595350 | Wiebe | Jul 1971 | A |
3599574 | Robertson | Aug 1971 | A |
3603265 | Barber | Sep 1971 | A |
3626864 | Wiebe | Dec 1971 | A |
3670660 | Weber et al. | Jun 1972 | A |
3687086 | Barber | Aug 1972 | A |
3699897 | Sherrick | Oct 1972 | A |
3707927 | Geyer et al. | Jan 1973 | A |
3712247 | Young | Jan 1973 | A |
3716903 | Tack | Feb 1973 | A |
3736978 | Taccone | Jun 1973 | A |
3748001 | Neumann et al. | Jul 1973 | A |
3762339 | Dwyer | Oct 1973 | A |
3772995 | Wright | Nov 1973 | A |
3799067 | Neumann et al. | Mar 1974 | A |
3802353 | Korpics | Apr 1974 | A |
3805707 | Neumann et al. | Apr 1974 | A |
3837293 | Neumann et al. | Sep 1974 | A |
3845725 | Gierlach | Nov 1974 | A |
3855942 | Mulcahy | Dec 1974 | A |
3857341 | Neumann | Dec 1974 | A |
3868912 | Wagner et al. | Mar 1975 | A |
3872795 | Tack | Mar 1975 | A |
3897737 | Davis | Aug 1975 | A |
3901163 | Neumann | Aug 1975 | A |
3910655 | Willison et al. | Oct 1975 | A |
3961584 | Paton et al. | Jun 1976 | A |
3965825 | Sherrick | Jun 1976 | A |
3977332 | Bullock | Aug 1976 | A |
3995720 | Wiebe | Dec 1976 | A |
4000931 | Geyer | Jan 1977 | A |
4003318 | Bullock et al. | Jan 1977 | A |
4004525 | Wiebe et al. | Jan 1977 | A |
4034681 | Neumann et al. | Jul 1977 | A |
4040362 | Oppenheim et al. | Aug 1977 | A |
4067262 | Scheffel | Jan 1978 | A |
4072112 | Wiebe | Feb 1978 | A |
4077496 | Wiebe | Mar 1978 | A |
4080016 | Wiebe | Mar 1978 | A |
4082043 | Hammonds et al. | Apr 1978 | A |
4084513 | Bullock | Apr 1978 | A |
4084514 | Bullock | Apr 1978 | A |
4090750 | Wiebe | May 1978 | A |
4103623 | Radwill | Aug 1978 | A |
4109585 | Brose | Aug 1978 | A |
4111131 | Bullock | Sep 1978 | A |
4114540 | Strugielski et al. | Sep 1978 | A |
4130066 | Mulcahy | Dec 1978 | A |
4131152 | Ruddle et al. | Dec 1978 | A |
4132176 | Wiebe | Jan 1979 | A |
4135833 | MacDonnell et al. | Jan 1979 | A |
4167907 | Mulcahy et al. | Sep 1979 | A |
4179995 | Day | Dec 1979 | A |
4192240 | Korpics | Mar 1980 | A |
4196672 | Bullock | Apr 1980 | A |
4198911 | Wiebe | Apr 1980 | A |
4203371 | Tack | May 1980 | A |
4224876 | Larsen | Sep 1980 | A |
4230047 | Wiebe | Oct 1980 | A |
4236457 | Cope | Dec 1980 | A |
4239007 | Kleykamp et al. | Dec 1980 | A |
4242966 | Holt et al. | Jan 1981 | A |
4245564 | Eulenfeld | Jan 1981 | A |
4254712 | O'Neil | Mar 1981 | A |
4254713 | Clafford | Mar 1981 | A |
4256041 | Kemper et al. | Mar 1981 | A |
4265182 | Neff et al. | May 1981 | A |
4274340 | Neumann et al. | Jun 1981 | A |
4276833 | Bullock | Jul 1981 | A |
4278030 | Ahlbron et al. | Jul 1981 | A |
4295429 | Wiebe | Oct 1981 | A |
4311098 | Irwin | Jan 1982 | A |
4313384 | Holden et al. | Feb 1982 | A |
4316417 | Martin | Feb 1982 | A |
4322981 | Radwill | Apr 1982 | A |
4330498 | Kleykamp et al. | May 1982 | A |
4333403 | Tack et al. | Jun 1982 | A |
4333404 | Kleykamp | Jun 1982 | A |
4342266 | Cooley | Aug 1982 | A |
4351242 | Irwin | Sep 1982 | A |
4356774 | Wear et al. | Nov 1982 | A |
4357880 | Weber | Nov 1982 | A |
4363276 | Neumann | Dec 1982 | A |
4363278 | Mulcahy | Dec 1982 | A |
4370933 | Mulcahy | Feb 1983 | A |
4373446 | Cope | Feb 1983 | A |
4380199 | Thomson et al. | Apr 1983 | A |
4408810 | Geyer | Oct 1983 | A |
4413569 | Mulcahy | Nov 1983 | A |
4416203 | Sherrick | Nov 1983 | A |
4426934 | Geyer | Jan 1984 | A |
4428303 | Tack | Jan 1984 | A |
4434720 | Mulcahy et al. | Mar 1984 | A |
4458604 | Cope | Jul 1984 | A |
4478154 | Holden et al. | Oct 1984 | A |
4480553 | Scheffel | Nov 1984 | A |
4483253 | List | Nov 1984 | A |
RE31784 | Wiebe | Jan 1985 | E |
4491075 | Neumann | Jan 1985 | A |
4512261 | Horger | Apr 1985 | A |
4537138 | Bullock | Aug 1985 | A |
RE31988 | Wiebe | Sep 1985 | E |
4552074 | Mulcahy et al. | Nov 1985 | A |
4574708 | Solomon | Mar 1986 | A |
4637319 | Moehling et al. | Jan 1987 | A |
4674412 | Mulcahy et al. | Jun 1987 | A |
4729325 | Henkel | Mar 1988 | A |
4744308 | Long et al. | May 1988 | A |
4753174 | Berg et al. | Jun 1988 | A |
4765251 | Guins | Aug 1988 | A |
4785740 | Grandy | Nov 1988 | A |
4825775 | Stein et al. | May 1989 | A |
4825776 | Spencer | May 1989 | A |
4825777 | Cummins | May 1989 | A |
4838174 | Moehling | Jun 1989 | A |
4915031 | Wiebe | Apr 1990 | A |
4936226 | Wiebe | Jun 1990 | A |
4938152 | List | Jul 1990 | A |
4953471 | Wronkiewicz et al. | Sep 1990 | A |
4964346 | Kirilloff et al. | Oct 1990 | A |
4974521 | Eungard | Dec 1990 | A |
4977835 | Altherr | Dec 1990 | A |
4986192 | Wiebe | Jan 1991 | A |
5027716 | Weber et al. | Jul 1991 | A |
5046431 | Wagner | Sep 1991 | A |
5046866 | Mulcahy | Sep 1991 | A |
5072673 | Lienard | Dec 1991 | A |
5081935 | Pavlick | Jan 1992 | A |
5086707 | Spencer et al. | Feb 1992 | A |
5086708 | McKeown, Jr. et al. | Feb 1992 | A |
5095823 | McKeown, Jr. | Mar 1992 | A |
5111753 | Zigler et al. | May 1992 | A |
5138954 | Mulcahy | Aug 1992 | A |
5150658 | Grandy | Sep 1992 | A |
RE34129 | Wright | Nov 1992 | E |
5176083 | Bullock | Jan 1993 | A |
5226369 | Weber | Jul 1993 | A |
5239932 | Weber | Aug 1993 | A |
5241913 | Weber | Sep 1993 | A |
5261332 | Grandy | Nov 1993 | A |
5305694 | Wronkiewicz et al. | Apr 1994 | A |
5315934 | List et al. | May 1994 | A |
5327837 | Weber | Jul 1994 | A |
5404826 | Rudibaugh et al. | Apr 1995 | A |
5410968 | Hawthorne et al. | May 1995 | A |
RE34963 | Eungard | Jun 1995 | E |
5438934 | Goding | Aug 1995 | A |
5450799 | Goding | Sep 1995 | A |
5452665 | Wronkiewicz et al. | Sep 1995 | A |
5461987 | Nassar | Oct 1995 | A |
5463964 | Long et al. | Nov 1995 | A |
5481986 | Spencer et al. | Jan 1996 | A |
5482675 | Shotwell et al. | Jan 1996 | A |
5509358 | Hawthorne et al. | Apr 1996 | A |
5511489 | Bullock | Apr 1996 | A |
5524551 | Hawthorne et al. | Jun 1996 | A |
5544591 | Taillon | Aug 1996 | A |
5546869 | Nassar | Aug 1996 | A |
5551351 | Hardin | Sep 1996 | A |
5555818 | Bullock | Sep 1996 | A |
5562045 | Rudibaugh et al. | Oct 1996 | A |
5572931 | Lazar et al. | Nov 1996 | A |
5718177 | Wronkiewicz et al. | Feb 1998 | A |
5722327 | Hawthorne et al. | Mar 1998 | A |
5735216 | Bullock et al. | Apr 1998 | A |
5746137 | Hawthorne et al. | May 1998 | A |
5752564 | Callahan et al. | May 1998 | A |
5794538 | Pitchford | Aug 1998 | A |
5799582 | Rudibaugh et al. | Sep 1998 | A |
5802982 | Weber | Sep 1998 | A |
5832838 | Shaw | Nov 1998 | A |
5850795 | Taillon | Dec 1998 | A |
5875721 | Wright et al. | Mar 1999 | A |
5904203 | Mai | May 1999 | A |
5918547 | Bullock et al. | Jul 1999 | A |
5921186 | Hawthorne et al. | Jul 1999 | A |
5924366 | Trainer et al. | Jul 1999 | A |
5954114 | Bauer et al. | Sep 1999 | A |
5967053 | Toussaint et al. | Oct 1999 | A |
6089166 | Callahan et al. | Jul 2000 | A |
6125767 | Hawthorne et al. | Oct 2000 | A |
6142081 | Long et al. | Nov 2000 | A |
6173655 | Hawthorne | Jan 2001 | B1 |
6186075 | Spencer | Feb 2001 | B1 |
6196134 | Stecker | Mar 2001 | B1 |
6227122 | Spencer | May 2001 | B1 |
6259752 | Domino et al. | Jul 2001 | B1 |
6269752 | Taillon | Aug 2001 | B1 |
6276283 | Weber | Aug 2001 | B1 |
6324995 | Kaufhold et al. | Dec 2001 | B1 |
6354226 | Stecker | Mar 2002 | B2 |
6371033 | Smith et al. | Apr 2002 | B1 |
6425334 | Wronkiewicz et al. | Jul 2002 | B1 |
6439130 | Scheffel | Aug 2002 | B1 |
6543367 | Stecker et al. | Apr 2003 | B1 |
6622776 | Bauer et al. | Sep 2003 | B2 |
6659016 | Forbes | Dec 2003 | B2 |
6662853 | Bauer et al. | Dec 2003 | B2 |
6672224 | Weber et al. | Jan 2004 | B2 |
6688236 | Taillon | Feb 2004 | B2 |
6871688 | Yamazaki et al. | Mar 2005 | B2 |
6874426 | Forbes | Apr 2005 | B2 |
6895866 | Forbes | May 2005 | B2 |
6920828 | Forbes | Jul 2005 | B2 |
7004079 | Forbes | Feb 2006 | B2 |
7017498 | Berg et al. | Mar 2006 | B2 |
7143700 | Forbes et al. | Dec 2006 | B2 |
7174837 | Berg et al. | Feb 2007 | B2 |
7255048 | Forbes | Aug 2007 | B2 |
7263930 | Pershwitz et al. | Sep 2007 | B2 |
7263931 | Forbes | Sep 2007 | B2 |
7267059 | Forbes | Sep 2007 | B2 |
7302994 | Mautino et al. | Dec 2007 | B2 |
7308855 | Van Auken | Dec 2007 | B2 |
7328659 | Forbes | Feb 2008 | B2 |
7337826 | Mautino et al. | Mar 2008 | B2 |
7353759 | Gray | Apr 2008 | B2 |
7387074 | Myers | Jun 2008 | B2 |
7469641 | Berg et al. | Dec 2008 | B2 |
7497169 | Forbes et al. | Mar 2009 | B2 |
7543626 | Pinkstock et al. | Jun 2009 | B1 |
7571684 | Forbes | Aug 2009 | B2 |
7603954 | Forbes | Oct 2009 | B2 |
7610862 | Forbes | Nov 2009 | B2 |
7631603 | Forbes et al. | Dec 2009 | B2 |
7654204 | Forbes | Feb 2010 | B2 |
7681506 | Forbes et al. | Mar 2010 | B2 |
7699008 | Forbes | Apr 2010 | B2 |
7775163 | Forbes et al. | Aug 2010 | B2 |
7823513 | Forbes et al. | Nov 2010 | B2 |
7845288 | Forbes et al. | Dec 2010 | B2 |
7926428 | Schorr et al. | Apr 2011 | B2 |
7946229 | Forbes et al. | May 2011 | B2 |
8011306 | Forbes | Sep 2011 | B2 |
8104409 | Wolinski et al. | Jan 2012 | B2 |
8113126 | Forbes et al. | Feb 2012 | B2 |
20010000571 | Bauer et al. | May 2001 | A1 |
20010008108 | Stecker | Jul 2001 | A1 |
20030136542 | Bauer et al. | Jul 2003 | A1 |
20030221811 | Smith et al. | Dec 2003 | A1 |
20040031413 | Smith | Feb 2004 | A1 |
20040211543 | Wick et al. | Oct 2004 | A1 |
20050223936 | Forbes | Oct 2005 | A1 |
20060021727 | Rizzo | Feb 2006 | A1 |
20060117985 | Forbes et al. | Jun 2006 | A1 |
20060137565 | Forbes et al. | Jun 2006 | A1 |
20070051270 | Forbes et al. | Mar 2007 | A1 |
20070137516 | Gray | Jun 2007 | A1 |
20070181033 | Forbes et al. | Aug 2007 | A1 |
20070209546 | Forbes | Sep 2007 | A1 |
20080017065 | Berg et al. | Jan 2008 | A1 |
20080066641 | Forbes et al. | Mar 2008 | A1 |
20080271633 | Forbes et al. | Nov 2008 | A1 |
20090126599 | Forbes et al. | May 2009 | A1 |
20100037797 | Forbes | Feb 2010 | A1 |
20100095864 | Forbes | Apr 2010 | A1 |
20100139521 | Forbes | Jun 2010 | A1 |
20100154672 | Forbes et al. | Jun 2010 | A1 |
20110068077 | Smyth | Mar 2011 | A1 |
20110073002 | Forbes et al. | Mar 2011 | A1 |
20110126392 | Forbes | Jun 2011 | A1 |
20110168655 | Nibouar et al. | Jul 2011 | A1 |
20110185939 | Forbes et al. | Aug 2011 | A1 |
Number | Date | Country |
---|---|---|
2009293193 | Mar 2010 | AU |
1163805 | Nov 1997 | CN |
1777484 | May 2006 | CN |
101066554 | Nov 2007 | CN |
101443143 | May 2009 | CN |
101733365 | Jun 2010 | CN |
101848779 | Sep 2010 | CN |
9315991 | Feb 1994 | DE |
2022580 | Feb 2009 | EP |
2149413 | Feb 2010 | EP |
2008154712 | Dec 2008 | WO |
WO 2010033694 | Mar 2010 | WO |
Entry |
---|
“Design for Economical Sand Molding,” Casting Design and Performance, ASM International, Materials Park, Ohio, 2009, pp. 81-87. |
International Search Report and Written Opinion dated Aug. 23, 2012 for International Application No. PCT/US2012/037946, 17 pages. |
International Search Report and Written Opinion dated Aug. 30, 2012 for International Application No. PCT/US2012/037880, 12 pages. |
Clark, Tom. The Sand Process, McCann Sales, Inc., Internet Archive Dated at least Oct. 10, 2008,retrieved at “www.mccannsales.com:book:sandcasting.pdf”. |
International Search Report for PCT:US2012:037905, mailed Aug. 14, 2012. |
Written Opinion for PCT:US2012:037905, mailed Aug. 14, 2012. |
International Search Report for PCT:US2012:037984, mailed Aug. 22, 2012. |
Written Opinion for PCT:US2012:037984, mailed Aug. 22, 2012. |
International Search Report for PCT:US2012:037947, mailed Oct. 25, 2012. |
Written Opinion for PCT:US2012:037947, mailed Oct. 25, 2012. |
Oct. 10, 2008—“The Sand Process” by Tom Clark, McCann Sales, Inc., Internet Archive ww.mccannsales.com:Book:Sandcasting.pdf. |
Aug. 8, 2012—(WO) International Search Report and Written Opinion—App. PCT/US2012/037880. |
Oct. 25, 2012—(WO) International Search Report and Written Opinion—App. PCT/US2012/037947. |
Jun. 4, 2014—(CN) Office Action—App. 201280001875.2. |
Feb. 5, 2015—(MX) Office Action—App. MX/A/2013/000184. |
Feb. 6, 2015—(AU) Office Action—App. 2012255890. |
Feb. 9, 2015—(AU) Office Action—App. 2012255926. |
Feb. 12, 2015—(AU) Office Action in App. 2012255958. |
Feb. 16, 2015—(CN) Office Action—App. 201280001875.2. |
Feb. 26, 2015—(MX) Office Action—App. MX/X/2013/000187. |
Jun. 3, 2015—(CN) Office Action—App. 201280001865.9. |
Mar. 3, 2015—(MX) Office Action—App. MX/A/2013/000186. |
Mar. 5, 2015—(MX) Office Action—App. MX/A/2013/000185. |
Mar. 10, 2015—(CN) Office Action—App. 201280001871.4. |
Mar. 11, 2015—(CN) Office Action—App. 201280001874.8. |
Mar. 17, 2015—(CN) Office Action—App. 201280001865.9. |
Rajput, R. K., A Textbook of Manufacturing Technology: Manufacturing Processes, Oct. 1, 2007, Firewall Media, pp. 74-78. |
“Optimising Sand Use in Foundries”, Environmental Technology Best Practice Programme, Mar. 1998, GG119. |
Feb. 9, 2015—(AU) Office Action—App. 2012255940. |
Number | Date | Country | |
---|---|---|---|
20120291662 A1 | Nov 2012 | US |