This invention relates to a novel specimen type and the associated method for testing the mechanical properties of a material, and in particular, but not exclusively for accurately obtaining creep strain data for a sample of material which is relatively small in size.
Materials such as metal can creep if they experience stress at a high enough temperature, over a long period of time. One of the primary aims of a designer of equipment operating in a creep range is to plan for the possibilities of failure by excessive deformation and avoid such failure. For example, dimensional changes with time, even of the order of a few millimetres, leading to mismatch of components or contact between moving parts, could lead to serious damage to plant, not to mention loss of human life and revenue.
Therefore there is a need for the generation of ways of predicting whether components operating in the creep range will sustain the life required of them. The useful life of a material could be terminated when deformation becomes excessive, when rupture occurs or when latent flaws or initiated cracks grow at unacceptable rates by creep or creep/fatigue.
Creep is defined as a high temperature progressive deformation at constant stress. “High temperature” is a relative term dependent upon the materials involved. Creep rates are used in evaluating materials for boilers, gas turbines, jet engines, ovens, or any application that involves high temperatures under load. Understanding high temperature behaviour of metals is useful in designing failure resistant systems.
Conventional uniaxial creep tests using cylindrical bar type specimens are usually performed for determining the creep properties. Creep occurs in three stages: Primary, or Stage I; Secondary, or Stage II: and Tertiary, or Stage III. Stage I, or Primary creep occurs at the beginning of a components life during which the strain rate reduces. Resistance to creep increases until Stage II is reached. In Stage II, or Secondary creep, the rate of creep becomes roughly steady. This stage is often referred to as steady state creep. In Stage III, or tertiary creep, the creep rate begins to accelerate as the cross sectional area of the specimen decreases due to (i) material degradation, and (ii) necking or internal voiding which decreases the effective area of the specimen. If stage III is allowed to proceed, fracture will occur.
Creep tests are usually employed to determine the minimum creep rate in Stage II. Engineers need to account for this expected deformation when designing systems. Currently there are three types of tests commonly used to determine creep strain data for a sample of material which is relatively small in size. These are the uniaxial, impression and small punch tests which are described further below.
To determine creep properties from the uniaxial creep test using small uniaxial specimen, material is subjected to prolonged constant tension or compression loading at constant temperature. Deformation is recorded at specified time intervals and a creep strain vs. time diagram is plotted. Slope of curve at any point is creep rate. If failure occurs, it terminates the test and Time for Rupture is recorded.
Impression creep testing, wherein a flat-ended cylindrical punch is used to load a small area of the specimen in compression, enables testing of small material volumes and the use of miniaturized specimens, with minimal preparation. However, under very slow creeping situations (depending on material, stress and temperature), a considerable time is necessary for the evolution of a steady-state creep zone under the punch, resulting in a prolonged period of decreasing creep rate even when the constitutive creep behaviour is strain-independent. This test-dependent transient behaviour, where the creep rate decreases slowly even at very long test times, complicates the determination of true material creep parameters. The very small creep deformations which occur under such conditions can be very difficult to accurately measure.
Small punch creep (SPC) test technique is another method used to evaluate the creep properties of materials extracted from components in a high temperature environment. The SPC uses a number of theory and test techniques for the purpose of applying the SPC test to the residual creep life assessment of plant components. However, as it is carried out in a high temperature environment using very thin miniature disc specimens, which is different from conventional uniaxial creep tests described above. The creep properties of the test specimens can be significantly influenced by surface oxidation. Moreover, when creep and oxidation occur simultaneously, it becomes difficult to unambiguously distinguish which changes are attributable to oxidation and which to fracture. When the oxide is strong and firmly adherent to the metal, it can improve creep strength, but if the oxide had low inherent strength or spalls away from the surface, creep strength can decrease.
The advantage that the small punch test method has relative to the impression creep test method is that it involves tertiary creep and fracture, whereas the impression creep test method only gives information on secondary creep behaviour and some indication about primary creep. However, so far the small punch test method does not have a fully verified and universal route for interpreting the primary, secondary and tertiary contributions to the overall displacement versus time curve.
For practical small specimen dimensions, the “test section” area for all three specimen types can be made large enough to enable “bulk” creep properties to be obtained (as opposed to single grains, or a few grain boundary properties being determined, which can be the case if the sample is very small). Similarly, all three have relatively small equivalent gauge length (EGLs), i.e. 2 to 10 mm for practical dimensions. The term EGL is defined as the length by which the measured deformation must be divided to give the equivalent strain to that which would be obtained from a corresponding uniaxial test.
The term “gauge length” is used in mechanical testing, it is the length, usually marked on a portion of a tensile test piece over which the elongation is measured.
In order to obtain results in reasonably short timescales (tests are usually carried out for times in the range 500 h to 3000 h), and in order to get easily measureable deformations with high accuracy, tests are often conducted at relatively high “stress” levels and/or temperatures, as compared with typical values of stress and temperature that a component would be designed to endure. All three specimen types currently being used are relatively “stiff” and so there is little scope for significantly increasing the EGL.
Any discussion of documents, acts or knowledge in this specification is included to explain the context of the invention. It should not be taken as an admission that any of the material forms part of the prior art base or the common general knowledge in the relevant art.
According to a first aspect, the present invention provides a method for testing the mechanical properties of a specimen having a first contact surface and a second contact surface spaced apart and opposing the first contact surface, the method comprising: applying forces to the contact surfaces of the specimen to deform the specimen over a period of time and determining the response of the specimen to the forces over time; and defining a spatial distance between the contact surfaces such that the equivalent gauge length of the specimen is greater than the distance between the contact surfaces.
The method may further comprise obtaining a sample of material from an object to be tested and forming the specimen from the sample or operating on the sample with machine tools to form the specimen or forming a ring-like shaped specimen from the sample. The first contact surface may be either a concave surface or convex surface, and wherein the second contact surface is also either a concave surface or a convex surface. The specimen may be symmetrical about a line joining the contact surfaces. The specimen may comprise an elliptical shape or a circular shape. The specimen may have a flattened elliptical shape having two opposed generally parallel sides and at least one, and preferably two, curved regions linking the parallel sides. The forces that may be applied to the contact surfaces forces the surfaces toward each other. The forces that may be applied to the contact surfaces forces the surfaces away from each other. The forces applied to the contact surfaces may be a diametric force which causes the contact surfaces to deform diametrically as a result of the forces being applied to at least a point on the contact surfaces. The diametric force may be either a tension force or a compression force applied to the contact surfaces. The equivalent gauge length of the specimen may be significantly greater than the distance between the contact surfaces. The equivalent gauge length of the specimen may be greater than or equal to 20 mm. The equivalent gauge length of the specimen may be at least two times or four times the distance between the contact surfaces. The method may further comprise heating the specimen to a temperature which may be substantially the same as the operating temperature which the sample made from the material would operate at. The specimen may be formed from a sample by a sample scooping technique or any other specimen retrieval technique. A force may be applied to either the first contact surface or the second contact surface and the other contact surface which does not have the force applied to it is secured to an apparatus for testing the mechanical properties of the specimen, wherein when the force is applied to the first surface or the second contact surface an equal and opposite reactive force is applied to the other contact surface. The first contact surface and/or the second contact surface may be shaped so as to self-align or self-centre a specimen within the apparatus for testing the mechanical properties of the specimen. The first contact surface and/or the second contact surface may be shaped so as to self-align or self-centre a specimen within the apparatus for testing the mechanical properties of the specimen. The method may further comprises hanging a weight from either the first contact surface or the second contact surface and using the other contact surface which does not have the weight applied to it to react to the force of the weight. Testing the mechanical properties of the specimen may comprise creep testing the specimen.
According to a further aspect, the present invention provides a specimen for testing the mechanical properties of a material, the specimen comprising: a first contact surface; a second contact surface; wherein the second contact surface opposes the first contact surface and defines an opening in between each surface; and wherein the specimen defines a spatial distance between the contact surfaces such that the equivalent gauge length of the specimen is greater than the distance between the contact surfaces.
The first contact surface may be either a concave surface or convex surface, and wherein the second contact surface is also either a concave surface or a convex surface. The specimen may be symmetrical about a line joining the contact surfaces. The specimen may comprise a ring-like shape. The specimen may comprise an elliptical shape, or a flattened elliptical shape, or a circular shape, or a split-ring shape, or a C-shape, or the like. The specimen may be formed from a sample of the material by a sample scooping technique or any other specimen retrieval technique. The equivalent gauge length of the specimen may be significantly greater than the distance between the contact surfaces. The equivalent gauge length of the specimen may be greater than or equal to 20 mm. The equivalent gauge length of the specimen may be at least two times or four times the distance between the contact surfaces. A force may be applied to either the first contact surface or the second contact surface and the other contact surface which does not have the force applied to it is secured to an apparatus for testing the mechanical properties of the specimen, wherein when the force is applied to the first surface or the second contact surface an equal and opposite reactive force is applied to the other contact surface. The first contact surface and/or the second contact surface may be shaped so as to self-align or self-centre a specimen within the apparatus for testing the mechanical properties of the specimen. The specimen may further comprise hanging a weight from either the first contact surface or the second contact surface and using the other contact surface which does not have the weight applied to it to react to the force of the weight. Testing the mechanical properties of the specimen may comprise creep testing the specimen.
According to a still further aspect, the present invention provides an apparatus for testing the mechanical properties of a material to determine a creep characteristic of a sample taken from the material, the sample comprising a first contact surface, a second contact surface spaced apart and opposing the first contact surface, applying forces to the contact surfaces of the sample to deform the sample over a period of time, and the sample defines a gap between the contact surfaces such that the effective gauge length of the sample is greater than the distance between the control surfaces, the apparatus comprising: an apparatus to apply the forces to the contact surfaces to deform the sample over a period of time; a heating device to heat the sample; and a processor to calculate a steady state time dependent deformation rate to determine a creep strain rate.
According to a still further aspect, the present invention provides a method of forming a sample from a material, the sample being used for testing the mechanical properties of the material, the method comprising: extracting the sample from the material; forming the sample into a test specimen having a first contact surface, a second contact surface spaced apart and opposing the first contact surface; applying forces to the contact surfaces of the specimen to deform the specimen over a period of time and determining the response of the specimen to the forces over time; and defining a spatial distance between the contact surfaces such that the equivalent gauge length of the specimen is greater than the distance between the contact surfaces.
According to a still further aspect, the present invention provides a process for producing a product from a production plant comprising: operating the plant to produce the product; checking the expected operational life of a component of the plant by: (i) obtaining a sample of the material of a component of the plant, and forming from the sample a specimen in accordance with any one of claims 21 to 29; (ii) performing a creep test on the specimen using the method according to any one of claims 1 to 20; determining that the component has a remaining safe operational life; and continuing to produce more product, using the component in the future.
The product may be electricity and the plant may be an electricity generating plant.
The present invention overcomes or reduces the problems associated with the prior art by producing a specimen type which makes the specimen relatively “flexible” and hence relatively larger deformations are measured and used to produce relatively low creep strain data equivalent to relatively low equivalent uniaxial data related to stress levels. It is of course easier to measure larger deformations, and the test can be performed faster at lower temperatures.
The most important aspect of the small sample design concept within this invention is the high EGL values which can be achieved. This allows easily measureable deformations to be obtained related to relatively small strains. Hence, apart from the ease with which the experiments can be performed, stresses and temperatures can be chosen to be much closer to practical operating values; most small specimen creep testing which is carried out is performed at elevated stress and/or temperature.
The various features of novelty which characterize the present invention are pointed out with particularity in the claims annexed to and forming part of this disclosure. For a better understanding of the present invention, its operation, advantages and specific objects attained by its use, reference should be had to the accompanying drawings and descriptive matter in which preferred embodiments of the invention are illustrated and described.
The present invention will be discussed hereinafter in detail in terms of the preferred embodiment of a novel specimen type and associated method of testing a sample from an object to determine the mechanical properties and in particular for testing and obtaining creep strain data. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present invention. It will be obvious, however, to those skilled in the art that the present invention may be practiced without these specific details.
Many components and structures in, for example, power plant or an electricity generating plant, chemical plant, aero engines, super-plastic forming dies etc, operate at temperatures high enough for creep to occur. In order to predict the creep behaviour of these components, “bulk material creep properties” are required. Typical, “bulk property” creep curves are shown in
In order to produce a sample a technique known as scooping using a hemispherical shaped toothed saw type cutter powered by an air motor is used. The cutting surface is lubricated and cooled using a water mist system with a high temperature lubricant. The cooling system prevents sparks, allowing the device to cut the small samples from such equipment as power plant, chemical plant, aero engines, super-plastic forming dies etc, which operate at temperatures high enough for creep to occur. Obviously other techniques for producing the sample can be used without departing from the scope of the invention. The present invention can be used to obtain data corresponding to that shown in
Specimens such as those shown in
a) shows small diameter specimens, typically 1.5 to 3 mm in diameter which may be electron beam welded into conventional end pieces. Tests were carried out in inert atmospheres and specialised loading frames were used to accommodate the low loads required. Data were obtained for four materials (0.5Cr0.5Mo0.25V, 1Cr0.5Mo, 1.25Cr0.5Mo and 2.25Cr1Mo) and results were compared with those of conventional creep tests. Provided grain sizes are not too large, specimen diameters as small as 1 mm can be used to produce “bulk” material creep properties. Small gauge lengths (<10 mm) can significantly reduce strain measurement sensitivities compared to conventional creep test specimens and can make strain measurements sensitive to relatively small temperature variations. The effects of specimen misalignment are greater when specimen diameters are small. In addition specimen manufacture is more complicated and more expensive than for conventional “full size” specimens.
b) shows a typical small specimen used in an impression creep test. In this case the dimensions of the block are; width=bi is approximately 10 mm with a height of approximately 2.5 mm and having an impression width=di of approximately 1 mm. The technique has been used for a wide range of materials (e.g. low alloy ferritic CrMoV steels, stainless steels, high chromium martensitic steels such as P91 and T91). A typical set of data obtained from such tests is shown in
The η and β values for the recommended specimen geometry (10 mm×10 mm×2.5 mm) are η=0.430 and β=2.18. These are independent of material properties and do not vary with impression depth provided Δc is relatively small compared to the specimen thickness, h.
The area of contact (10 mm×1.0 mm) will generally be large compared to metallurgical features and hence the test is capable of producing “bulk” material creep properties. The quantity “βdi” in equation (2), is divided into the measured displacement, Δc, to obtain the creep strain. Hence, βdi can be thought of as being the equivalent gauge length (EGL) for the corresponding uniaxial creep test carried out at a stress level of η
c) shows a typical small specimen used in the small punch creep (SPC) test. Typical specimen dimensions measure approximately 8 mm in diameter and 0.5 mm in thickness. The small punch test involves large deformations relative to the specimen thickness. Test data obtained from this type of test is shown in
The failure location in small punch creep tests is near the edge of contact between the punch and the specimen. Based on the Chakrabarty membrane theory, expressions have been determined relating the strain at the edge of contact position to the displacement. Similarly, the ratio of the force to membrane stress, P/σ, and the displacement have been determined. For the case of ap=2.0 mm and Rs=1.25 mm, the P/σ ratio and edge of contact strain, ε, for Δ>0.8 mm, are given by:—
P/σ=1.72476Δ−0.05638Δ2−0.17688Δ3 (3a)
ε=0.17959Δ+0.09357Δ2+0.00440Δ3 (3b)
The maximum P/σ value, based on the Chakrabarty membrane theory is 1.89, when Δ=1.6 mm. When Δ>1.6 mm, P/σ decreases because of the thickness reduction which occurs.
The variation of the maximum P/σ, with ap, Rs, and to, for Δ>0.8 mm, has been obtained and this leads to an expression for a of the form:—
where P is the small punch load and ap, Rs, and to are the radius of the disc between the supports, radius of the punch and initial thickness of the disc, respectively; K, is a correlation factor, which is determined empirically for the particular material.
By using equation (3b) the deflection versus time curves obtained experimentally can be converted to strain versus time curves. Similarly, the variation of P/σ (and hence σ) can be obtained by using equation (3a). Hence, the stationary strain rates can be obtained from the secondary stages of the creep tests.
The sample 10 which is machined (or otherwise extracted) from the blank has two contact surfaces, a first contact surface 20 and a second contact surface 30. The second contact surface 30 being spaced apart and opposing the first contact surface 20 and defining an opening 40 between the two contact surfaces. The contact surfaces 20, 30 may be either concave surfaces or convex surfaces. The contact surfaces 20, 30 may also be symmetrical about a line 80 joining the contact surfaces. For example the sample 10 may be a ring like object (or similar flexible specimen such as a spring), either a circular ring 100 or an elliptical ring 90. However, any ring like (or similarly flexible) shape may be used without departing from the scope of the present invention. The sample 10 used for determining creep in an object or solid material may be for example a small sample 10 which may be defined as a sample, typically 10 mm in diameter (ie b=10 mm) with a radial thickness, d, of approximately 0.5 mm and a length in the z direction of 2 mm which is capable of being deformed.
In order to test a sample 10 from an object to determine the mechanical properties and in particular for testing and obtaining creep strain data, the sample 10 requires a force to be applied to the contact surfaces 20, 30 of the sample 10 to deform the sample over a period of time.
A computer 60 or similar processor controls the uniaxial tension device 70 and is also used to calculate a steady state time dependent deformation rate to determine a creep strain rate, the creep strain rate is dependent upon the relationship of the deformation and an effective gauge length of the sample 10. The apparatus also includes a heating device (not shown) for example a heating element or furnace controlled by a thermocouple or similar device. The sample 10 is heated to a temperature substantially the same as the operating temperature of the object from which the sample 10 is taken.
The object of the uniaxial creep test is to find the steel properties equivalent to those which would be obtained from a test case out in a state of pure tensile stress. The device 70 loads a test specimen 10 and records the load vs. deflection. The compressive loading may also be used in which the sample 10 is compressed rather than stretched. In this embodiment the ring like shape is used. The ring like shape has a force applied to the contact surfaces which may either force the contact surfaces towards each other or away from each other depending on whether a tension or compression test is used. Due to the shape of the ring like sample a diametric force may be applied which causes the contact surfaces to deform diametrically. Further the diametric force may be either a tension or compression force applied to the contact surfaces. In this embodiment the diametrically loaded sample, in this case an elliptical ring 90, as shown in
Another aspect of the sample design concept is the high equivalent gauge length (EGL) values which can be achieved. This allows easily measureable deformations to be obtained related to relatively small strains. Hence, apart from the ease with which the experiments can be performed, stresses and temperatures can be chosen to be much closer to practical operating values. As stated above the term “gauge length” is used in the mechanical testing of materials, it is the length marked on a portion of a tensile test piece 10 over which the elongation is measured. Therefore, the EGL means the length which must be divided into the measured deformation of the specimen 10 in order to obtain the strain equivalent to that which would be obtained in a creep uniaxial tensile test.
In this embodiment the sample defines a gap 40 between the contact surfaces 20, 30 such that the equivalent gauge length of the sample 10 is greater than the distance between the contact surfaces 20, 30. This embodiment of the present invention overcomes the problems associated with the prior art by producing a sample which is relatively “flexible” and hence larger deformations are measured and used to produce relatively low creep strain data related to relatively low equivalent uniaxial stress levels. The equivalent gauge length may be very large by comparison with the specimen dimensions (in particular the distance between the points between which the deformation is measured). Typically the equivalent gauge length can be of the order of at least four times the distance between the points between which the deformation is measured. It is relatively easy to have an EGL of at least 50 mm for a sample according to the present invention. By way of example, from table 1 below, for a circular ring with R=6 mm, β=0.448 and d=1 mm and using the formula for effective gauge length;
An equivalent gauge length of approximately 65 mm may be achieved.
An advantage obtained using the present invention is that it allows easily measureable deformations to be obtained related to relatively small equivalent strains when related to the corresponding uniaxial test. Hence, apart from the ease with which the experiments can be performed, stresses and temperatures can be chosen to be much closer to practical operating values. It is also noted that the deformations do not significantly affect the parameters η and β, which enables accurate secondary creep properties to be easily obtained.
A diametric force is applied to the sample 10 in order to deform the sample 10 over a period of time. Preferably or optionally the diametric force applied to the sample 10 is a single deformation mechanism which does not, to any significant extent locally deform the sample 10 at the point of application of the diametric force 50. As shown in
Creep is defined as a high temperature progressive deformation at constant stress. “High temperature” is a relative term dependent upon the materials involved. The prior art states that in order to evaluate the creep in a material using the known specimen samples means that rather higher temperatures or stresses than those expected under operating conditions are required. In accordance with the present invention the use of the sample in this case the elliptical ring 90, allows stresses and temperatures to be chosen to be much closer to practical operating values of the materials from which the sample 10 was taken.
As will be shown in the following calculations a steady state time dependent deformation rate is calculated to determine a minimum creep strain rate. The minimum creep strain rate is dependent upon the relationship of the deformation of the sample 10 and the equivalent gauge length of the flexible small sample 10. The gauge length also allows easily measureable deformations to be obtained related to relatively small strains.
The following calculations for a sample 10 in this case the elliptical ring 90 show that the results obtained are comparable with those of known prior art small specimens. However, the sample 10 of the present invention (either the elliptical ring 90 or the circular ring 100) are easy to manufacture, compared with conventional samples 10. Also, because the samples 10 are designed to obtain creep strain rate data, i.e. not creep rupture data, the surface finish is not too critical and samples 10 may be made using, for example, a water jet cutting machine; such a machine is highly versatile and capable of being programmed to make much more complicated shapes than the elliptical rings 90 or circular rings 100 described above. It will be appreciated that the ring-like shape of the specimen could also be a closed ring or not. It could be a split ring, or a C-shape for example.
The loading system, experimental setup and alignment procedures used for the sample 10 are simple to operate. Temperature control is no more difficult than for other small sample 10 test types and because creep deformations are relatively large, the sensitivity is not significantly affected by the small thermal strains which occur due to the unavoidable temperature variations which occur within the test furnace. Elliptical geometries with a/b>1, and other similarly shaped specimens, such as that shown in
It will be appreciated that a very simple creep test is to hang a weight off one of the contact surfaces and support the specimen (and the weight) off the other contact surface. One contact surface would then be a weight bearing surface (or an applied force surface) and the other contact surface is a reaction force surface. If the surfaces are concave in shape on the inside of the areas where the weight is contacted with the specimen and where a reaction support contacts the specimen, then the sample, weight, and reaction surface could all be self-aligning or self-centering: in that gravity could automatically line up the points at which the weight force is applied to the ring-like specimen and the point at which the force of the weight is reacted. This makes the creep test easy to use.
As will be shown the deformations do not significantly affect the parameters η and β, which enables accurate secondary creep properties to be easily obtained.
The stationary state solution for the deformation of a structure made from a nonlinear material obeying a time-dependent model of the Norton form
{dot over (ε)}c=B|σ|nsign(σ) (5)
is of exactly the same form as that for a time-independent nonlinear material obeying a constitutive equation of the form
ε=B|σ|nsign(σ) (6)
The only difference in the two solutions is that the expression obtained for displacement using a material model described by equation (6) would be replaced by an expression for displacement rate using a material model described by equation (5).
In further calculations, shown below, the derived relationship between the bending moment and stress in a beam is, i.e.
Using the principles of virtual complimentary work and stationary complimentary energy, it can be shown that
where ui are the displacements at the point of application and in the directions of a set of “k” loads, Pi (i=1, 2 . . . k). For the case of a beam in bending, U* is given by:
When M=0, θ=θ′, say, where
Using equation (7),
Using equations (8) with (11) and 12(a) gives
Equation (13) can be solved numerically to obtain θ′ for any particular value of n and a/b, see
Using equations (8) with (11) and 12(b) gives
The term inside the { . . . } brackets in equation (14) is a function of n and a/b; this is defined as Int2 (n, a/b).
Therefore, equation (14) can be simplified and converted to a stationary state creep solution as:—
In particular, for a rectangular cross-section beam, i.e.
Using MacKenzie's method for determining reference stresses,
Choosing the value of α(=η) which makes
independent of n leads to
where β is constant for a given a/b,
Re-arranging equation (18) gives
Equations (19) and (20) give the equivalent uniaxial stress and EGL for an elliptical specimen.
For the special case of a circular ring, i.e. a=b=Rs, equation (20) becomes:—
The variations of η and β-values with a/b are shown in
For some typical dimensions, it can be seen (Table 1) that the test section area (beam cross-section) is about 5-10 mm2 which is good by comparison with the other specimens. The EGL for the circular ring is approximately 32 mm for R=6 mm and d=2 mm or 64 mm for R=6 mm and d=1 mm. For an elliptical ring with a/b=2 and with a=8 mm, b=4 mm and d=1 mm, say, the EGL is about 90 mm. It is clear that these EGL values are significantly larger than the equivalent gauge length values applicable to commonly used small specimen types. The dimension range of the specimens can be chosen to match the load capacity of the test machines to be used and the EGL required. In order to make the specimens “small”, 2R≦10 mm, d≈1 mm and bo≈2 mm may be used.
An approximate reference stress can be obtained from knowledge of the limit load of a structure. Using this approach it can be shown that
An approximate limit load for a circular ring is derived, i.e.
Hence, using equations (23) and (25),
The accurate theoretical solution gives
Hence, the approximate, limit load, reference stress is about 10% higher than the more accurate value. Also, using the approximate reference stress, equation (26), in equation (24), together with the elastic solution for a diametrally loaded circular ring, i.e.
gives:—
The accurate theoretical solution (Equation (20)) gives
Hence, the approximate EGL value is about 0.5% lower than the more accurate value.
The data shown in
The same material was used to manufacture circular rings (a/b=1) with R/d=5. These specimens were tested in diametrical tension, at 650° C., with loads corresponding to uniaxial stresses (obtained using Equation (22)) of 55, 60 and 65 MPa; the displacement versus time data for these tests are shown in
In order to further improve the accuracy of the results obtained from the ring test data the slight ellipticity which develops during testing can be corrected for by using the instantaneous a and b values and deformation rates in equations (19) and (20). These slight ellipticity errors which develop during testing of circular rings (as a result of creep deformation) can be practically eliminated by starting with an elliptical specimen (a/b=2, say) for which the loadline displacement is accompanied by a relatively small transverse reduction of the major axis of the elliptical ring, compared with that which occurs for a circular ring.
In order to further verify the technique, FE analyses (under plane stress conditions) were performed for a circular ring, with R=10 and bo=1, for a number of R/d values. The variations of FE steady-state load-line deformation rates with R/d, for a specific load magnitude and material property values, are compared with predictions obtained from the corresponding analytical solutions, in
The axial strain and the bending moment of a beam under pure bending conditions are:—
where Ro is the radius of curvature. Assume a non-linear power law material behaviour model as follows: —
ε=B|σ|nsign(σ) (A1-3)
which leads to
A non-linear power law material behaviour model is given by
ε=B|σ|nSign(σ) (A1-3)
The complimentary strain energy density (
Therefore, for the ring, assumed to be comprised of beam-type structures (four quadrants), the total complimentary strain energy of the structure is given by:—
The geometry and loading are shown in
For an ellipse,
x=a cos θ
y=b sin θ
(ds)2=(dx)2+(dy)2, therefore,
ds=√{square root over (a2 sin2 θ+b2 cos2 θdθ)} (A3-1)
The bending moments in the ring,
For the case of pure bending, for a material obeying a power relationship of the form given by equation A1-3, the complimentary strain energy density is
given by:—
Therefore, for a beam with uniform cross-sectional area,
For the elliptical ring,
Using equations 12(a) and 11, the following relationship is obtained:—
from which the θ′-value, which is dependent on n and a/b, can be obtained, see
Also, using equations 12(b) and 11, the load point deformation rate can be obtained:—
The term inside the { . . . } brackets in equation. (A3-8) is a function of n and a/b; see
Work done by PL (the limit load) is dissipated in the formation of the plastic “hinges” at A, B, C and D, therefore,
From equations (A4-2) and (A4-1),
For a rectangular cross-sectional beam,
For a conventional uniaxial creep test, the creep strain at a time is usually measured from the deformation of the gauge length (GL). If the gauge length elongation is A and the elastic portion is neglected,
For non-conventional small creep test specimens, an equivalent gauge length (EGL) could be defined, if the measured creep deformation can be related to an equivalent uniaxial creep strain, in the same form as that of Equation (A5-1), i.e.
The EGL is related to the dimensions of the specimen and in some cases may be related to the time-dependent deformation of the test specimen. The creep strain and creep deformation given in Equation (A5-2) may be presented in a form of the reference stress, σR, i.e.
Δc≈Dεc(σR) (A5-3)
In which D is the reference multiplier, which is in fact the EGL for the test. In some cases, the geometric changes, due to the specimen creep deformation with time, are small (e.g. for impression creep test), and in such cases, the effects of geometric changes on D (EGL) can be neglected for simplicity.
For some specimen types, such as the ring or elliptical specimens, creep deformation Δc can be obtained from analytical solutions, for example, using the principles of virtual complimentary work and stationary total complimentary energy. Therefore, if a reference stress approach is used, analytical solutions for the reference stress, σR, and the reference multiplier, D, may be obtained. In more general situations when Δc cannot be obtained analytically, a numerical procedure, using, for example, the finite element analysis, can be used to determine the reference stress, σR, which is related to the applied load, and the reference multiplier, D (EGL), which is a function of specimen dimensions.
Although the present invention has been illustrated and described with respect to exemplary embodiment thereof, it should be understood by those skilled in the art that the foregoing and various other changes, omission and additions may be made therein and thereto, without departing from the scope of the invention. Therefore the present invention should not be understood as limited to the specific embodiment set out above but to include all possible embodiments which can be embodied within a scope encompassed and equivalent thereof with respect to the features set out in the appended claims.
| Number | Date | Country | Kind |
|---|---|---|---|
| 0821168.2 | Nov 2008 | GB | national |
| Filing Document | Filing Date | Country | Kind | 371c Date |
|---|---|---|---|---|
| PCT/GB2009/051560 | 11/18/2009 | WO | 00 | 7/27/2011 |