Abstract
The invention refers to the non-ferrous metallurgy, i.e. to the creation of the modern titanium alloys, having the high genericity. Titanium-base alloy contains aluminum, vanadium, molybdenum, chromium, iron, zirconium, oxygen and nitrogen. Herewith the components of the alloy have the following ratio by weight %; aluminun—4.0-6.0; vanadium—4.5-6.0; molybdenum—4.5-6.0; chromium—2.0-3.6; iron—0.2-0.5; zirconium—0.1-less than 0.7; oxygen—0.2 max; nitrogen—0.05 max; titanium—balance. Technical result—creation of the titanium alloy with the required strength and plastic properties. The alloy may be used to produce the wide range of the products including the large-size forgings and die-forgings as well as semiproducts of small section, such as bars and plates up to 75 mm thick.
Description
FIELD OF THE INVENTION

The invention refers to the field of the non-ferrous metallurgy, i.e. to creation of the universal titanium alloys, used for manufacture of the wide range of products, including the large die-forgings and forgings as well as semiproducts of fine section, such as bars, plates up to 75 mm thick, which are widely used for manufacture of the different parts of the aeronautical engineering.


PRIOR STATE OF THE ART

The known titanium-base alloy of the following composition, weight %:

















Aluminum
4.0-6.3



Vanadium
4.5-5.9



Molybdenum
4.5-5.9



Chromium
2.0-3.6



Iron
0.2-0.8



Zirconium
0.01-0.08



Carbon
0.01-0.25



Oxygen
0.03-0.25



Titanium
balance









(Patent RF #2122040, cl. C22C 14/00, 1998)


This alloy is characterized by a combination of the strength and plastic properties in large-size parts up to 150-200 mm thick, water and air-quenched. The alloy can be perfectly strained when hot and welded by any type of welding.


However, the alloy has no sufficient strength for manufacture of the large heavy parts with the thickness up to 200 mm and air-quenched.


The closest in technical substance and the result achieved to the invention pending is the titanium-base alloy containing following weight %:

















Aluminum
4.0-6.0



Vanadium
4.5-6.0



Molybdenum
4.5-6.0



Chromium
2.0-3.6



Iron
0.2-0.5



Zirconium
0.7-2.0



Oxygen
max 0.2



Nitrogen
 max 0.05



Titanium
balance









(Patent RF No 2169782, cl. C22C 14/00, issue of 2001)—prior art.


The disadvantage of the prior art is the low plasticity and tend to cracking when cold upsetting to more than 40%, which limits its use in fasteners.


DISCLOSURE OF THE INVENTION

The task to be solved by this invention is the creation of the universal titanium alloy with the required strength and plasticity characteristics, structure and producibility of the large range of products.


The technical result achieved when exercising this invention is in regulation of the optimum combination of α- and β-stabilizers in the alloy.


The specified result is achieved by the following combination in weight % of elements in titanium-base alloy, containing aluminum, vanadium, molybdenum, chromium, iron, zirconium, oxygen and nitrogen,

















Aluminum
4.0-6.0



Vanadium
4.5-6.0



Molybdenum
4.5-6.0



Chromium
2.0-3.6



Iron
0.2-0.5



Zirconium
0.1-less than 0.7



Oxygen
max 0.2



Nitrogen
 max 0.05



Titanium
balance









β-phase contributes mainly to the high strength of the alloy due to wide range of the β-stabilizers (V, Mo, Cr, Fe), their amount and effect on maintaining the metastable phase in the course of the slow cooling (for example, in the air) of die-forgings large sections. Though β-phase drives the hardening process in the alloy, the strength may be increased only due to the increased strength of the α-phase, the general fraction of which for this alloy is 60-70%. For this purpose the alloy is alloyed with the α-stabilizer zirconium. Zirconium forms a wide range of the solid solutions with α-titanium, is relatively close to it in melting temperature and density and increases the corrosion resistance. Alloying with zirconium in the range of 0.1—less than 0.7% ensures the combination of the high strength and plasticity for large forgings and die-forgings as well as semiproducts of fine section, such as bars, plates up to 75 mm thick, allows to perform the hot and cold deformation with the upset ratio up to 60%.







EMBODIMENT OF THE INVENTION

To investigate the properties of the applied alloy the trial ingots were produced with the diameter of 190 mm with the averaged chemistry (data is given in Table 1).










TABLE 1








Chemical Composition, wt. %
















Alloy
Al
Mo
V
Cr
Zr
Fe
O
N
Ti



















1
5.45
5.3
5.35
3.1
0.65
0.4
0.145
0.006
Bal


2
5.1
5.22
5.1
2.9
0.3
0.41
0.12
0.005
Bal


3
4.9
4.8
5.0
2.8
0.5
0.3
0.10
0.006
Bal


4
5.3
5.3
5.2
3.1
0.2
0.4
0.12
0.006
Bal


5
5.1
4.9
5.3
3.1
1.2
0.35
0.12
0.006
Bal


Prior art









The ingots were forged in succession in β-, α+β-, β-, α+β-fields with the final deformation in α+β-field within 45-50% for the cylindrical stock(billet) 40 mm in diameter.


The forgings were subsequently heat-treated:

    • a) Solution heat-treatment:
    • heating up to 790° C., 3 h holding, air cooling.
    • b) Ageing:
    • heating up to 560° C., 8 h holding, air cooling.


Forgings mechanical properties (averaged data in the longitudinal direction) are under Table 2.














TABLE 2






σ02 (VTS),
σB (UTS),


K1C,


Alloy
MPa
MPa
δ (A), %
Ψ (Ra), %
MPa/{square root over (m)}




















1
1230
1300
10
21
63


2
1200
1290
15
28
69


3
1110
1190
14
26
71


4
1160
1270
16
32
72


5
1255
1350
10.5
27
51.5


Prior art









As the forgings mechanical test results state, microalloying with zirconium in the claimed ranges 0.1—less than 0.7 weight % in combination with quenching allows to keep the high strength, providing for the fine alloy plasticity.


COMMERCIAL PRACTICABILITY

The applied titanium alloy as compared to the known alloys may be used for manufacture of the wide range of products of the critical application, including the large-size forgings and die-forgoings as well as semiproducts of small section, such as bars, plates up to 75 mm thick, which are widely used for aerotechnical parts including fasteners.

Claims
  • 1. Titanium-base alloy containing aluminum, vanadium, molybdenum, chromium, iron, zirconium, oxygen and nitrogen, and differing in the following selected composition, weight %:
  • 2. The alloy of claim 1 wherein the alloy has a fracture toughness of 69 MPa √m to 72 MPa √m.
Priority Claims (1)
Number Date Country Kind
2005114842 May 2005 RU national
PCT Information
Filing Document Filing Date Country Kind 371c Date
PCT/RU2006/000234 5/6/2006 WO 00 11/7/2007
Publishing Document Publishing Date Country Kind
WO2006/123968 11/23/2006 WO A
US Referenced Citations (4)
Number Name Date Kind
3615378 Bomberger et al. Oct 1971 A
4745977 Love et al. May 1988 A
5264055 Champin et al. Nov 1993 A
20030116233 Tetyukhin et al. Jun 2003 A1
Foreign Referenced Citations (6)
Number Date Country
62267438 Nov 1987 JP
2004010963 Jan 2004 JP
1132567 Oct 1994 RU
2169782 Jun 2001 RU
03095690 Nov 2003 WO
WO 2005123976 Dec 2005 WO
Related Publications (1)
Number Date Country
20080210345 A1 Sep 2008 US