Use of co-injection molding to produce composite parts including a molded snowboard with metal edges

Information

  • Patent Grant
  • 6309586
  • Patent Number
    6,309,586
  • Date Filed
    Tuesday, June 15, 1999
    25 years ago
  • Date Issued
    Tuesday, October 30, 2001
    23 years ago
Abstract
The present invention comprises products of and methods for producing complex shapes of composite molded articles, including snowboards, that meet or exceed the aesthetic, cost and performance requirements expected of similar non-molded composite articles. The injection molded or co-injection molded snowboard comprises a top surface and a bottom surface shaped to provide a center portion, at least one tip or tail portion and edges along the sides of the center portion, wherein the bottom surface is a substantially smooth continuous surface, the center portion is cambered away from the top surface and contains metal edges along the sides of the bottom surface center portion, the tip or tail portions are curved away from the bottom surface of the snowboard and the top surface contains binding mounts or screw threads flush mounted to secure bindings.A preferred method of constructing a snowboard comprises co-injection molding, utilizing a skin polymer with a smooth finish for exterior portions of the snowboard and a core polymer that is lighter, structurally stronger and potentially cheaper than the skin polymer for the interior of the snowboard. A mold cavity is designed for the desired shape of the snowboard. In addition to providing for the shape of the snowboard, the mold cavity is designed to accommodate inserts for side metal edges and clips to secure such edges, if necessary, and inserts for top, flush mounted binding mounts or screw threads as well as the clips to secure such mounts. An additional set of metal components may be embedded within the top surface of the snowboard to compensate for warping away from the bottom metal edges due to the polymer shrink rate. The mold cavity must be designed to accommodate inserts for securing such metal components if such components are utilized.
Description




FIELD OF THE INVENTION




The present invention relates generally to products of and methods for producing complex shapes of composite molded articles, including a snowboard with metal edges, by the process of co-injection molding.




BACKGROUND OF THE INVENTION




None of the following is admitted to be prior art to the present invention.




Injection molded, including co-injection molded, articles could be vastly improved if there was a method for producing complex shapes of composite molded articles, in a single molding operation; thus optimizing the value of injection molding and maintaining or improving the characteristics expected of similar non-molded composite articles. For example, a problem that has long plagued the art of snowboard manufacturing has been the time and cost associated with manufacturing multiple layer laminated snowboards with metal edges to meet specific aesthetic and performance requirements. Injection molding has been sought after as a means of reducing such time and costs of manufacturing, but to date, has been unable to achieve all of the aesthetic, cost and performance attributes the public has come to expect of modem laminated snowboards. What is needed is a method for producing complex shapes of composite molded articles that meet or exceed the aesthetic and performance requirements expected of similar non-molded composite articles, preferably at reduced costs.




Injection Molding




Injection molding is where thermoplastic polymers are gravity-fed from a hopper into a barrel, melted by a reciprocating screw and/or electric heat and are propelled forward by a ram (piston, plunger) or the screw (used as a plunger) into mating steel or aluminum molds, which are cooled to below the heat-distortion temperature of the resin. The injected plastic material contracts as it cools (mold shrinkage) and shrinks. When cool enough to retain its shape, the plastic part is ejected from the mold.




Typically, good part design requires adequate taper (draft) of side walls, radii at inside corners, minimal variations in wall cross-sections, use of ribs 60% or less of outer wall thickness for stiffness, strength and minimal sink marks. Thermosetting polymers can also be injection-molded. For these materials, the barrels on the injection-molding machine are heated by hot water to a point safely below cross-linking temperature; the polymer is then propelled by ram or screw feed into heated molds. After they cure, the parts can be ejected while still hot because they have already thermally set or cross-linked.




Injection molding of polymers has revolutionized many industries. Most products today contain some form of plastic molded parts in them or consist entirely of plastic molded parts. Such products include toys, automobile parts, computer covers, phones, liquid containers and many, many other articles, too numerous to recite. However, modern molding operations have not been able to produce complex shapes of composite molded articles, in a single molding operation, that meet or exceed the aesthetic and performance requirements expected of similar non-molded composite articles. For certain products, aesthetic or performance requirements dictate that non-molded components, such as metals or ceramics, be utilized. However, incorporating polymer materials and non-molding materials in the single molding step has not been able to achieve the complex geometries required of some products, including molded snowboards with metal edges. For example, round washers have been embedded into molded parts as the base legs of appliances, computers and other similar articles to lift them off of the floor. However, such components do not require the metal and molded polymer to retain a bent, curved or complex shape whereby the shape of the article presents forces that separate the polymer and non-molded component.




Co-Injection Molding




Co-injection molding takes advantage of a characteristic of injection molding called fountain flow. That is, as the cavity is filled, the plastic at the melt front moves from the center line of the stream to the cavity walls. Because the walls are below the transition temperature (freeze temperature) of the melt, the material that touches the walls cools rapidly and freezes in place. This provides insulating layers on each wall, through which new melt makes its way to the melt front.




Sequential co-injection processes have two barrels and one nozzle in an injection molding machine. The skin polymer is injected into the mold first, then the core polymer is injected. The skin polymer is the material that is expected to be deposited on the cavity wall over the entire surface of the part. The core polymer displaces the skin polymer at the hot core, pushing it to fill the rest of the cavity. The end product is a sandwich-like structure, with the core polymer in the middle and the skin polymer on the surfaces of the part.




As two materials are processed, two hopper/screw/barrel assemblies are required for co-injection. A special co-injection nozzle allows the operator to alternate between the two materials with the speed, timing and accuracy necessary to optimize the co-injection application.




The advantages of this process are: the combination of two material properties into one part, and the maximization of the overall performance/cost ratio. One good example of co-injection is the use of polymer re-grind as the core material, while maintaining surface finish quality by using virgin polymer as the skin material. Other applications include using thermally more stable polymer as the core material to increase the thermal resistance of a part, or using a high melt-flow index polymer as the core material, to reduce the overall clamp force. Still other applications include using a core material that is lighter and exhibits more flexibility than the skin material to combine strength and flexibility to the desired part, while keeping the weight down. One combination may include a fiberglass loaded core material to provide a structural component to the part and a different skin material to maintain a smooth, consistent surface.




Numerous articles on the co-injection process have been authored. Some articles include,


Co


-


Injection Molding ′


95


: Market Outlook


, by Thomas W. Betts of Battlefield of America, Inc;


Molded


-


In Shielding Using the Coinjection Process


, by Thomas W. Nash and Ralph J. McDonald, IBM Application Business Systems, Rochester, Minn. 55901


; Coinjection Molding with Automotive Polyolefins


, by Bruce R. Denison, D & S Plastics International;


Recycling—Why Not Use Co


-


Injection Molding


?, by Joseph McRoskey of Co-Mack Technology, Inc. and Thomas W. Nash of Thomas W. Nash & Associates; and


Co-Injection Molding: Current Applications


, by Joseph McRoskey of Co-Mack Technology, Inc. (May 31-Jun. 2, 1998). The foregoing articles are incorporated herein by reference, including any drawings.




Injection and co-injection molding operations that incorporate additional non-molded components, such as metal edges, comprise additional technical hurdles to overcome, especially when such non-molded components are incorporated into a single molding operation step. Such hurdles include the need to adjust for shrinkage of the polymer as it cools in the mold; securing the non-molded components within the mold and eliminating or minimizing surface lines from inserting components into the mold. Previous attempts to address such technical matters have not succeeded in producing a snowboard that meet the expectations of an industry dominated by laminated snowboards.




To date, efforts to produce molded snowboards have focused on producing low cost snowboards, causing quality, performance and aesthetics to suffer. For example, a molded snowboard is available under the name ESP and is distributed by the EMSCO Group of Girard, Pennsylvania, USA. The board is a low grade plastic material with metal edges. The snowboard lacks smooth continuous curves and surfaces, lacks a proper camber, is warped, contains bumps and surface irregularities from inserting plugs into holes made for binding fasteners and possibly from the shrinkage of inconsistent material densities, lacks a smooth finish and color, and contains exposed metal points from holding the edges in place during the molding process. Identity Snowboards, in Montana, produces an injection molded snowboard whereby the plastic sides and top are molded with space for metal edges and binding fasteners to be inserted and glued to the injection molded section of the snowboard as a secondary process. Such additional process steps are time consuming and expensive and this method produces a snowboard that suffers from some of the same de-lamination issues as traditional laminated snowboards.




Laminated Snowboards




Most modem snowboards are produced by laminating several materials together. Such snowboards are produced by companies such as Ride Snowboards, K2, Saloman, Burton and Morrow, to name a few. Examples of modem laminated snowboards can be found on web sites operated by these companies, including http://www.ridesnowboards.com, http://www. burton. com, http://www.k2snowboards .com, http://www.salomonsports.com/northamerica/snowboarding/connect/pub.html, and http://www.morrowsnowboards.com. This list is not an exhaustive list as there are hundreds of snowboard companies in business, owning to the popularity of the sport. Further examples may be found in U.S. Pat. Nos. 5,769,445; 5,782,482; 5,823,562; 5,851,331; 5,855,389; and 5,871,224.




The modern snowboard laminating technique consists of sandwiching multiple layers together with resins and industrial adhesives. Such layers typically include a wood or foam core, fiber reinforcement layer, thermoplastic layers, metal edge material, base material and a monocoque envelope. Other features may include the use of reinforcing materials in the end portions of the snowboard as an attempt to prevent delamination. Graphics may be applied below the top surface or monocoque envelope or to the top of it. In the sandwiched layers a set of screw threads or binding fasteners are inserted for securing bindings to the snowboard. Laminated boards have set the standard for the snowboard industry in terms of aesthetics and performance. The boards are strong enough to withstand the pressures applied by snowboard riders and flexible enough to absorb the shocks applied through maneuvers.




Notwithstanding the above, laminated boards experience several disadvantages. The laminated layers are held together by adhesives. The layers separate over prolonged use. Moreover, ice and snow can penetrate into the cracks between adhered layers and destroy the structural integrity of the snowboards, thereby delaminating the layers and the metal edges. The inserted screw threads for securing bindings depend on the strength of the adhesives. The screw threads may sometimes loosen and spin within the boards. As well, modern laminating techniques are time consuming, environmentally harmful and expensive to operate, requiring hours of labor for adhering layers, inserting screw threads and shaping the product.




What is needed is a method for producing complex shapes of composite molded articles, including snowboards, that meet or exceed the aesthetic and performance requirements expected of similar non-molded composite articles, preferably at reduced costs and using recyclable materials.




SUMMARY OF THE INVENTION




The present invention comprises products of and methods for producing complex shapes of composite molded articles, including snowboards, that meet or exceed the aesthetic, cost and performance requirements expected of similar non-molded composite articles. The injection molded or co-injection molded snowboard comprises a top surface and a bottom surface shaped to provide a center portion, at least one tip or tail portion and edges along the sides of the center portion, wherein the bottom surface is a substantially smooth continuous surface, the center portion is cambered away from the top surface and contains metal edges along the sides of the bottom surface center portion, the tip or tail portions are curved away from the bottom surface of the snowboard and the top surface contains binding mounts or screw threads flush mounted to secure bindings.




A preferred method of constructing a snowboard comprises co-injection molding, utilizing a skin polymer with a smooth finish for exterior portions of the snowboard and a core polymer that is lighter, structurally stronger and potentially cheaper than the skin polymer for the interior of the snowboard. A mold cavity is designed for the desired shape of the snowboard. In addition to providing for the shape of the snowboard, the mold cavity is designed to accommodate inserts for side metal edges and clips to secure such edges, if necessary, and inserts for top, flush mounted binding mounts or screw threads as well as the clips to secure such mounts. An additional set of metal components may be embedded within the top surface of the snowboard to compensate for warping away from the bottom metal edges due to the polymer shrink rate. The mold cavity must be designed to accommodate inserts for securing such metal components if such components are utilized.




As the polymer in the mold cools, it shrinks and the shrinkage rate depends on the polymer material selected. The metal edge material that is secured into the molten polymer does not shrink and therefore the shrinking polymer tends to “pull” the embedded metal component with it. This shrinkage and pulling action warps or bends the metal edge. The bottom surface metal edges contour to the final cure form of the majority polymer component, which for a snowboard is upward toward the top surface of the snowboard.




Several methods to adjust for the shrinkage rate of a particular polymer material may be employed. One method is to adjust the curvature of the snowboard mold cavity so that the warping will provide the desired curvature when cooling is completed. Another method is to adjust the composition of the polymer material, through additives or glass loading, to control the warping to provide the desired curvature when cooling is completed. Since the metal edges along the bottom surface of the snowboard are designed to be at a set camber after cooling, the exact adjustment necessary to achieve the desired camber after cooling involves an iterative process depending on the polymer material selection.




Another method to adjust for the shrinkage rate of a particular polymer material is to embed additional metal components similar to the bottom edge materials, into the top surface of the mold. Therefore, as the polymer material cools and shrinks, it will pull away from both the top and bottom portions in substantially equal proportions, thereby counteracting each other and producing the desired shape. Care must be taken to embed the top metal edges into the top surface so that they do not stick out of the top surface and so that they are not embedded so deep as to have no effect. The preferred depth is in the range of 0.015 to 0.060 inches (0.038 to 0.152 cm) for a snowboard that is approximately 0.5 inches (1.27 cm) thick. Proper placement involves an iterative process depending on the polymer material selection.




The mold cavity is split in two halves, an “A” half and a “B” half, with the A half representing the top of the snowboard article being manufactured and the B half representing the bottom of the snowboard article being manufactured. Loaded into each side of the B half is a B side rail insert comprising a metal rail with locator clips attached to the metal rails at about 3.5 inches (8.9 centimeters) apart center to center from adjacent clips whereby the locator clips are in molded cavities of the B side rail insert. Loaded into the A half is (i) parallel to, but not flush with, each side of the A half is an A side rail insert comprising a metal rail with locator clips attached to the metal rails at about 3.5 inches (8.9 cm) apart center to center from adjacent clips whereby the locator clips are in molded cavities of the A side rail insert and (ii) two A side nut inserts, each nut insert comprising six (6) nuts secured in place on the nut insert by six millimeter (6 mm) screws from the back of the nut insert. The distance between locator clips depends on the size of the snowboard. The goal is to allow the A side metal rail to “float” a bit within the mold, so proper placement and location of clips is an iterative process depending on the size of the snowboard. The inserted nuts comprise a base that is wider than the threading such that the wider base is embedded within the molded polymer. In order to resist spinning within the molded part, as determined by screw-retention strength standards of binding mounts for alpine skis, in compliance with ASTM Standard Nos. F474-98 and F475-77 (1992), the wider base is preferably a polygon or other non-rounded shape such as a hexagon.




The locator clips for the A side rails are designed to be a specific size in order to embed the top metal rails into the top surface of the snowboard so that the metal rails do not stick out of the top surface and so that the metal rails are not embedded so deep as to have no effect on the curvature of the board as described above. Proper placement involves an iterative process depending on the polymer material selection. A depth change of just five thousandths of an inch (0.005 inches or 0.013 centimeters) causes a difference in the shape of the snowboard product.




Once all of the inserts have been located within the A and B side cavities of the mold, the mold is closed and the co-injection molding cycle is operated. The mold is then opened and the snowboard is removed from the B side of the mold. The locator clips on the B side of the mold break off, producing small plastic nubs. The screw threads holding the inserts for the binding nuts are removed. The A side locator clips are cut off and milled down.











BRIEF DESCRIPTION OF THE DRAWINGS





FIG. 1

depicts an open snowboard mold cavity with inserts in accordance with the present invention.





FIG. 2



a


depicts a metal rail and locator clip for the bottom of a snowboard in accordance with the present invention.





FIG. 2



b


depicts a mold insert incorporating a metal rail with locator clips for the bottom of a snowboard in accordance with the present invention.





FIG. 3



a


depicts a metal rail and locator clip for the top of a snowboard in accordance with the present invention.





FIG. 3



b


depicts a mold insert incorporating a metal rail with locator clips for the top of a snowboard in accordance with the present invention.





FIG. 4

depicts a mold insert incorporating a nut with a screw for incorporation into the top of a snowboard in accordance with the present invention.





FIG. 5

depicts a cross-sectional view of a closed snowboard mold of the present invention.





FIG. 6

depicts a metal rail for the bottom of a snowboard in accordance with the present invention.





FIG. 7

depicts a snowboard produced in accordance with the present invention.











DESCRIPTION OF THE PREFERRED EMBODIMENTS




The following description includes the best presently contemplated mode of carrying out the invention. This description is made for the purpose of illustrating the general principles of the inventions and should not be taken in a limiting sense.




Injection molded parts, especially snowboards, having curved portions incorporating non-resin materials such as metal components, require innovative methods for incorporating such non-resin components while maintaining the required shape for aesthetic and performance purposes. Moreover, ensuring that the final molded product requires minimum processing after the molding operation, while incorporating such non-resin materials, is a desired benefit of the present invention. The methods described herein produce snowboards having metal edges, a cambered bottom surface, ends curved away from the bottom surface and smooth finishes at costs and production times lower than conventional laminating methods.




DEFINITIONS




“A ” Side and Top Surface




The terms “A side” and “top surface” are used interchangeably throughout to refer to the top surface of the snowboard product as viewed by a typical snowboard rider. The “A side” is that portion of the mold cavity that results in the top surface of the final molded snowboard product.




“B” Side and Bottom Surface




The terms “B side” and “bottom surface” are used interchangeably throughout to refer to the bottom surface of the snowboard product as viewed by a typical snowboard rider. The “B side” is that portion of the mold cavity that results in the bottom surface of the final molded snowboard product.




Composite Molded Articles and Complex Shapes




The term “composite molded article,” refers to injection or co-injection molded parts that comprise an additional non-molded component part, in a single molding operation step, so that the final article resembles a homogeneous article. The term “complex shape” refers to a composite molded article whereby the shape of the article produces forces inherent in the molding operation that tend to separate the polymer and non-molded component and whereby the separation forces are not counteracted in the molding operation, but rather, are compensated for and utilized to shape the composite molded article. An example of a composite molded article of a complex shape includes, but is not limited to, a plastic molded snowboard comprising metal edges and metal binding fasteners, where the metal edges maintain a cambered shape. Many molded articles that comprise a non-molded component that is not embedded within, surrounded by, or in sufficient quantity to counteract the molding material forces of the molding polymer will fall into this category. Some examples include, but are not limited to, airplane food trays with metal edges for fastening, flashlights, boat accessories, sporting goods, toys and many other articles where it is important to maintain a homogeneous appearance of a complex shaped article.




Co-Injection Molding




The term “co-injection molding” or “co-injected molds” as used interchangeable herein, refers to a process of injection molding whereby a skin polymer is injected into the mold first, then the core polymer is injected within the skin polymer. The skin polymer, surrounding the core polymer, is the material that is deposited on the cavity wall over the entire surface of the part.




CO-INJECTION MOLDED SNOWBOARD





FIG. 1

depicts an open snowboard mold cavity, split in two halves, “A” half or “upper” half cavity


20


and “B” half or “lower” half cavity


10


, with cavity


20


representing the top of snowboard article


60


being manufactured and cavity


10


representing the bottom of snowboard article


60


being manufactured. Snowboard article


60


is shown for illustration purposes only. Loaded into each side of cavity


10


is insert


30


(one shown) comprising a metal rail with locator clips attached to the metal rails (shown in

FIG. 2



a


). Loaded into cavity


20


is (i) insert


40


(one shown) parallel to, but not flush with, each side of cavity


20


, comprising a metal rail with locator clips attached to the metal rails (shown in

FIG. 3



a


) and (ii) two inserts


50


(one shown) comprising six (6) nuts secured in place on insert


50


(shown in FIG.


4


). More or less nuts may be utilized if desired.





FIG. 2



a


shows metal rail


35


with locator clips


33


attached to metal rail


35


. Such locator clips


33


are usually placed at about 3.5 inches (8.9 centimeters) apart center to center from adjacent clips, along the length of metal rail


35


.

FIG. 2



b


shows metal rail


35


, secured by locator clips


33


, attached to insert


30


via locator clips


33


in mold cavities


37


.





FIG. 3



a


shows metal rail


45


with locator clips


43


attached to metal rail


45


. Such locator clips


43


are usually placed at about 3.5 inches (8.9 cm) apart center to center from adjacent clips, along the length of metal rail


45


.

FIG. 3



b


shows metal rail


45


, secured by locator clips


43


, attached to insert


40


via locator clips


43


in mold cavities.




Locator clips


43


attached to metal rails


45


are designed to be a specific size in order to embed metal rails


45


into the top surface of the snowboard so that metal rails


45


do not stick out of the top surface and so that metal rails


45


are not embedded so deep as to have no effect on the curvature of the board. Proper placement involves an iterative process depending on the polymer material selection A depth change of just five thousandths of an inch (0.005 inches or 0.013 centimeters) causes a difference in the shape of the snowboard product. A depth of 0.025 inches (0.064 cm) is preferred for a snowboard article having a center width from top surface to bottom surface of about 0.50 inches (1.27 cm).





FIG. 4

shows six nuts


55


secured by six millimeter (6 mm) screws


53


(one shown) attached to insert


50


via screws


53


in mold cavities


57


. Nuts


55


are preferably polygon in shape, such as a hexagon, so that the nuts do not slip in the snowboard, to meet or exceed ASTM Standard No. F474-98.




Referring to

FIG. 1

, once inserts


30


,


40


and


50


have been located within cavities


10


and


20


of the mold, the mold is closed and the co-injection molding cycle is operated according to standard co-injection operating procedures.

FIG. 5

illustrates a cross-section of the closed mold depicting the middle of a snowboard, width wise, oriented so that the top of the figure is the top of the snowboard article being produced in the mold.

FIG. 5

shows inserts


30


,


40


and


50


; locator clips


33


and


43


; metal rails


35


and


45


; screws


53


and nuts


55


and a molded snowboard


60


. Referring to

FIGS. 1 and 5

, the mold is then opened by separating cavities


10


and


20


and snowboard


60


is removed from cavity


10


of the mold. As the mold opens and snowboard


60


is removed, locator clips


33


and


43


break off, leaving small nipples (not shown) that are later grinded off for aesthetic purposes. Graphics, top sheet designs or drawings may be painted or affixed onto the top surface of the snowboard during the molding process, using in-mold applications, or applied post-process to the completed snowboard.




One presently preferred snowboard produced according to the methods of the present invention has the dimensions shown in Table 1 below. However, it is to be understood that the methods of the present invention are capable of producing a plurality of snowboards and other articles differing substantially in shape and dimension.












TABLE 1











Snowboard Dimensions












ITEM




DIMENSIONS









Overall length, end to end, side view




43.791 inches (111.23 cm)






Thickness, side view






End portions “tip and tail”




0.203 inches (0.52 cm)






Center portion




0.500 inches (1.27 cm)






Camber radius of center portion, side view






Bottom surface




250 inches (635 cm)






Top surface




250.450 inches (636.14 cm)






End portions, tip and tail, side view






Radii




6 inches (15.24 cm)






Height, bottom to top of end portions




2.25 inches (5.72 cm)






Side edge curvature radii, top surface view




300 inches (762 cm)






End portion widths, tip and tail, top surface




9 inches (22.86 cm)






view






Binding mounts/screw threads location, top






surface view






From center of board, length wise




5 inches (12.70 cm)






From center of board, width wise




1.5 inches (3.81 cm)






Apart from each other, center to center




1 inch (2.54 cm)














Other shapes and sizes contemplated by the present invention include, but are not limited to, sizes of snowboards that are commercially available, including snowboards that have a length of anywhere from 90 centimeters to 170 or 180 centimeters. Such snowboards may be found at TransWorld Snowboarding on-line at http://www.twsnow.com. A sampling of sizes of commercially available snowboards, located on the “Board Genie 99” of the above web site is shown in Table 2.












TABLE 2











Commercially Available Snowboard Dimensions




















Eff.




S/C










Manufacturer/Model




Length




Edge




Radius




Nose




Waist




Tail




Stance





















Burton:













Fluid59




159




124




901




29.6




25.6




29.6




18-24






Charger61




161




125




833




29.6




25.2




29.6




18-24






Motion62




161.5




126




810




29.5




24.9




29.5




18-24






FL Project 62




162




126




847




29.3




24.9




29.3




18-24






Johan 63




163




126




793




29.6




24.9




29.6




18-24






Fluid64




164




129




931




30.2




26




30.2




18-24






Joyride:






Factory Series




158




122




807




29.3




24.9




29.3




18.12-24.5 






Factory Series




159




123




875




29.7




25.3




29.7




18.12-24.5 






Premium Series 161 Dir.




161




128




875




29.7




25




29.7




18.12-24.5 






Premium Series 166 Dir.




166




130




899




30.1




25.3




30.1




18.12-24.5 






K2:






Eldorado 158




158.2




123.8




820




29.9




25.6




29.9




18.5-26.5






Fatbob 161




159.7




125.7




864




31.5




27.1




31.4




18.5-26.5






Electra 162




161.4




126.5




815




30




25.4




29.9




18.5-26.5






Brian Savard 161




162.1




127.3




869




29.4




25.1




29.4




18.5-26.5






Eldorado 163




163




126.6




836




30.2




25.7




30.1




18.5-26.5






Dart 165




164




126.4




843




29.5




25




29.5




18.5-26.5






Morrow:






Escape 59




159




127.1




883




29.8




25.1




29.8




20  






Escape Plus 60




160




127.7




883




31.5




26.9




31.5




20.5






Dimension 62




161




130




863




29.7




24.8




29.5




20.6






Rail 65




162




128.8




890




30.1




25.5




30.1




20.5






Master 63




163




131




875




30.1




25.3




30.1




21.5






Escape 64




164




131.6




890




30.2




25.5




30.2




20.5






Ride:






Timeless




161




125




850




29.8




25.5




29.8




17-25






Control




163




127




850




30




25.5




30




17-25






Rossignol:






Butane/Stokes




158




123




950




30




25.5




30




N/A






Strato Wide




159




121




950




30.5




26




29.9




18-24






Nomad




160




121




950




28.7




24.8




28.7




N/A






Levitation Dualtec




161




121




950




29.3




24.8




28.7




18-24






Strato




166




127




*****




29.8




25.1




29.1




18-24






Strato Wide




166




127




*****




31.2




26.5




30.5




18-24






Salomon:






400 LT FR 159 WB




159




125




960




29.7




25.7




29.1




16.92-23.2 






500 pro FR 164




164




127




990




29.4




24.8




29.4




17.32-22  






500 pro FR Adv. 165




165




129.5




996




29.6




25.2




29.1




 18.5-22.44











All sizes are in centimeters.










S/C Radius refers to the side cut radius.










The Nose/Waist/Tail dimensions refer to the width of such sections.










The Stance refers to the range of distances between the bindings for a rider's feet.













Although one embodiment of the present invention is to construct a snowboard as described above, it is to be understood that alternative methods for securing metal rails may be employed to eliminate the need for locator clips. Eliminating locator clips will reduce mold preparation time, material costs and post-mold processing time. Metal rails must be securely fastened to the outer edges of the B side mold cavity to ensure that they are placed along the bottom edges of the completed snowboard article. Injection or co-injection involves a high degree of pressure such that any space between the metal rails and the mold cavity will result in polymer material flowing around the metal rails and covering them. One such method is to utilize a rail shape that works in conjunction with the pressure of the injected polymer material so that the flow of the polymer material forces the metal rails further into the edges of the molded cavity. Such a design may work in conjunction with side magnets utilized to initially place and secure the metal rails in place. The metal rails should also contain an irregular shape within the portion that is embedded within the polymer material so as to ensure mechanical interlocking of the metal rail and the polymer material. The mechanical interlocking will secure the metal rail in the molded article and prevent separation upon use of the snowboard.




Another method is to utilize a rail shape that extends into the polymer material of the snowboard and extends out of the snowboard, to eliminate the need for locator clips. The portion that extends out of the snowboard is used to secure the metal rail to the edge and is milled or ground off following the molding operation.

FIG. 6

shows a metal rail


100


made of a hardened metal such as steel. Metal rail


100


has an irregular or scalloped side


110


for embedding into the molding material, an extended portion


120


for securing metal rail


100


along the side edges of a mold and a cut out notch


125


for easy grinding off of the extended portion


120


after the molding operation. Once the extended portion


120


is ground off, edge


130


becomes the outer edge of the bottom surface of a molded snowboard made in accordance with the present invention.





FIG. 7

illustrates a snowboard


60


made in accordance with the teachings of the present invention. Snowboard


60


contains metal rail edges


35


(one side shown) and binding nuts


55


(two sets of six shown). A cut out portion shows the embedded metal rail


45


within the top portion of snowboard


60


, just below or sometimes flush with the snowboard surface.




Although a preferred embodiment of the present invention is to construct a snowboard via a co-injection molding operation, it is to be understood that other operations may be utilized either alone, sequentially or in conjunction with one another, including, but not limited to, injection molding, compression molding, extrusion molding, structural foam molding, rotational molding, thermoforming, blow molding, reaction injection molding (RIM), gas assisted molding, composites processing, hand lay-up, spray-up, centrifugal casting, matched die molding, resin transfer molding and other operations of similar import.




TWO-STEP MOLDING




An example of another molding operation to construct a snowboard is a two-step molding process, whereby the first step is to mold a snowboard core that partially extends to the surface of the snowboard product and that embeds the non-molded components such as the metal rails and the binding nuts, according to the teachings of the present invention. Thereafter, a second over-molding operation is conducted to create the outer surface of the part and yield a smooth, continuous surface. The advantages of this two-step process are the ability to combine dissimilar core and skin materials and the resulting ability to maximize the characteristics of the core/skin polymer materials. A variation is to design cavities into the first molding operation to secure the non-molded components into, for the second over-molding operation. Care must be taken in the design to allow the second molding operation to mechanically interlock at least some portions of the non-molded components so that de-lamination of the part does not result.




Polymer materials that may be employed in the practice of the present invention include, without limitation, high density polyethylene (HDPE), polypropylene (PP), polyurethane (PU), acetal, surlyn, nylon and acrylonitrile-butadiene-styrene (ABS), among other materials with the proper and necessary characteristics for the particular application. Other suitable polymer materials and processes are contained in the Handbook of Plastic Materials and Technology, John Wiley & Sons, Inc. (New York 1990), incorporated herein by reference. Moreover, any polymer material capable of being incorporated into an injection molding or co-injection molding, or other molding operation may be utilized in the practice of the present invention.




It should be understood, of course, that the foregoing relates only to preferred embodiments of the present invention and that numerous modifications or alterations may be made therein without departing from the spirit and the scope of the invention as set forth in the appended claims.



Claims
  • 1. A method of molding a snowboard in a single step operation comprising:preparing a mold cavity configured to a desired shape, having an upper half and a lower half with each half having two sides, a front end and a rear end such that the upper half, lower half, front end, rear end and sides of the mold correspond to the top, bottom, front, rear and sides of the snowboard being produced; securing a plurality of binding mounts or screw threads to the upper half mold cavity; securing metal rails flush against the bottom sides of the lower half mold cavity; and molding the snowboard in a single step molding operation.
  • 2. The method of claim 1 wherein securing a plurality of binding mounts comprises:preparing the upper half mold cavity with a plurality of pocket cavities, each configured to accommodate a binding mount insert; preparing binding mount inserts comprising a top side, a bottom side and a plurality of screws that are threaded through the binding mount insert with nuts attached to said screws along the bottom side of the binding mount insert so that the nuts extend out of the bottom side of the binding mount insert and are touching the bottom side of the binding mount insert; and inserting the binding mount insert into each pocket cavity so that the top side of the binding mount insert presses against the pocket cavity wall and the bottom side of the binding mount insert is flush with the upper half mold cavity wall, thereby extending the nuts outward into the mold.
  • 3. The method of claim 1 wherein securing metal rails comprises:preparing a metal rail with a solid three dimensional rectangular portion perpendicular to a grooved or scalloped shape portion; preparing the lower half mold cavity with a pocket cavity on each side of the lower half mold cavity, each configured to accommodate less than the entire solid portion of the metal rail; and inserting the solid portion of the metal rail into the pocket cavity so that part of the solid portion extends into the mold and the grooved or scalloped shape portion extends into the mold.
  • 4. The method of claim 1 further comprising:securing at least one metal rail along the bottom of the upper half mold cavity, corresponding to the top of the snowboard, prior to molding.
  • 5. The method of claim 4 further comprising:inserting in-mold graphics along the bottom of the upper half mold cavity, corresponding to the top of the snowboard, prior to molding.
  • 6. The method of claim 1 further comprising:inserting in-mold graphics along the bottom of the upper half mold cavity, corresponding to the top of the snowboard, prior to molding.
  • 7. The method of claim 1 wherein the single molding step operation is selected from the group consisting of injection molding, co-injection molding, compression molding, reaction injection molding (RIM), and gas assisted molding.
  • 8. A method of molding a snowboard in a single step operation comprising:(I) preparing a mold cavity configured to a desired shape, having an upper half and a lower half with each half having two sides, a front end and a rear end such that the upper half, lower half, front end, rear end and sides of the mold correspond to the top, bottom, front, rear and sides of the snowboard being produced; (II) securing a plurality of binding mounts or screw threads to the upper half mold cavity; (III) securing metal rails flush against the bottom sides of the lower half mold cavity, comprising (a) preparing the lower half mold cavity with a pocket cavity on each side of the lower half mold cavity, each configured to accommodate a rail insert; (b) preparing rail inserts comprising (i) locating a plurality of clips along metal rails having grooves; and (ii) inserting said clips into cavities prepared in the rail inserts to accommodate said clips; and (c) inserting the rail inserts into each pocket cavity so that the rails are flush with the bottom sides of the lower half mold cavity; and (IV) molding the snowboard in a single step molding operation.
  • 9. A method of molding a snowboard in a single step operation comprising;(I) preparing a mold cavity configured to a desired shape, having an upper half and a lower half with each half having two sides, a front end and a rear end such that the upper half, lower half, front end, rear end and sides of the mold correspond to the top, bottom, front, rear and sides of the snowboard being produced; (II) securing a plurality of binding mounts or screw threads to the upper half mold cavity; (III) securing metal rails flush against the bottom sides of the lower half mold cavity; (IV) securing at least one metal rail along the bottom of the upper half mold cavity coresponding to the top of the snowboard, comprising (a) preparing the upper half mold cavity with at least one pocket cavity in the upper half mold cavity, each configured to accommodate a rail insert; (b) preparing rail inserts comprising (i) locating a plurality of clips along metal rails having grooves; and (ii) inserting said clips into cavities prepared in the rail insert(s) to accommodate said clips; and (c) inserting the rail insert(s) into each pocket cavity so that the rails are along the bottom of the upper half mold cavity; and (V) molding the snowboard in a single step molding operation.
US Referenced Citations (21)
Number Name Date Kind
3958810 Bohm May 1976
4026575 Hartwig May 1977
4337963 Stevenson Jul 1982
4725070 Maruyama Feb 1988
4731038 Hancock et al. Mar 1988
4897063 Scheurer et al. Jan 1990
5173226 Cazaillon et al. Dec 1992
5338051 Szafranski et al. Aug 1994
5445403 Cazaillon et al. Aug 1995
5449425 Renard et al. Sep 1995
5544908 Fezio Aug 1996
5687983 Feketa et al. Nov 1997
5695209 Deborde et al. Dec 1997
5716562 Peart et al. Feb 1998
5769445 Morrow Jun 1998
5782482 Andrus et al. Jul 1998
5823562 Stubblefield Oct 1998
5851331 Grenetier et al. Dec 1998
5855389 Andrus et al. Jan 1999
5871224 Vance Feb 1999
6042126 Muller et al. Mar 2000
Non-Patent Literature Citations (5)
Entry
Thomas W. Betts, Co-Injection Molding '95: Market Outlook, Battenfeld of America (1995).
Thomas W. Nash and Ralph J. McDonald, Molded-In Shielding Using the Coinjection Process, IBM Application Business Systems, Rochester, MN 55901 (Undated).
Bruce R. Denison, Coinjection Molding with Automotive Polyolefins, D & S Plastics International (Undated).
Joseph McRoskey and Thomas W. Nash, Recycling—Why Not Use Co-Injection Molding? (Undated).
Joseph McRoskey, Co-Injection Molding: Current Applications, Co-Mack Technology, Inc., May 31-Jun. 2, 1998 Plastics Product Design & Development Forum.