The present invention relates to a vent piece used for performing air vent of a raw cover (an unvulcanized tire) in vulcanization molding of a pneumatic tire; and a manufacturing method for pneumatic tire in which vulcanization molding of a pneumatic tire is performed by embedding the vent piece in a vulcanization mold.
Vulcanization molding of a pneumatic tire is performed such that: a raw cover is set in a vulcanization mold; then, a bladder arranged on the inner side of the raw cover is expanded so that the outer surface of the raw cover is pressed against the inner face of the vulcanization mold; followed by heating and pressurizing the raw cover at predetermined temperature and pressure for a predetermined time.
In this vulcanization molding, when air remains in the inner face or the surface of the raw cover, this causes degradation in the external appearance quality serving as a product and in the durability of the pneumatic tire. Thus, for example, a method that a vent hole is provided in the vulcanization mold and then air vent is performed (e.g., Patent Document 1) and a method that a vent piece is embedded in a prepared hole formed in the mold and then air vent is performed have widely been employed.
Nevertheless, in these methods, occurrence of spew caused by rubber extruded into the vent hole or the hole of the vent piece cannot be avoided. Among these, the spew caused by the vent hole need be removed in the manufacturing process. Further, as for the spew caused by the vent piece, when the number of occurrences increases, unpreferable external appearance is caused.
As methods for suppressing such occurrence of spew, the method of dividing the mold into a plurality (e.g., Patent Document 2) and the method of employing a spring-shaped vent piece (a spring vent) have been proposed.
Patent Document 1: JP2873363B
Patent Document 2: JP2003-311742A
Nevertheless, these methods have the following problems.
That is, in the case of the method of dividing the mold into a plurality, air vent can be performed by releasing air through a gap formed between the mating surfaces of the divided molds. Nevertheless, the portion of air vent is determined in the initial design of the mold and hence cannot be added later. Further, in a case that the mold is divided into an excessively large number, a possibility arises that the mold cannot tolerate the pressurization and hence distortion is caused.
In the case of the method of employing a spring vent, as shown in
Thus, an object of the present invention is to provide: a vent piece which can easily be added later in vulcanization molding of a pneumatic tire and is free from restriction in the location for orderly arrangement and in which occurrence of spew can satisfactorily be suppressed; and
The invention described in claim 1 is
The invention described in claim 2 is
The invention described in claim 3 is
The invention described in claim 4 is
The invention described in claim 5 is
According to the present invention, provided are: a vent piece which can easily be added later in vulcanization molding of a pneumatic tire and is free from restriction in the location for orderly arrangement and in which occurrence of spew can satisfactorily be suppressed; and a manufacturing method for pneumatic tire in which vulcanization molding of a raw cover is performed by using a vulcanization mold for pneumatic tire in which the vent piece has been embedded.
The present invention is described below in accordance with an embodiment with reference to the drawings.
As shown in
As a result, when vulcanization molding of a raw cover is performed by using the vulcanization mold in which the vent piece 1 has been embedded, air is released through the gap for air vent formed between the side face part of the vent piece 1 and the side face part of the prepared hole for air vent. Thus, a pneumatic tire can be obtained in which occurrence of spew is suppressed.
The vent piece 1 according to the present embodiment is constructed from a pillar shaped member having a simple structure. Thus, structural restriction like in the spring vent of the conventional art is not caused and a smaller size can be achieved. Accordingly, in whatever locations, orderly embedment and arrangement can be performed without particular restriction.
As the construction material for the vent piece 1, stainless steel, iron, aluminum, or the like is preferable. Among these, stainless steel is particularly preferable.
As the shape of the vent piece 1, from the perspective of easiness in machining at the time of forming the prepared hole in the vulcanization mold and the like, a cylindrical shape is preferable. Specifically, the vent piece 1 having a cylindrical shape in which the diameter D1 of the head part 11 and the diameter D2 of the trunk part 12 are 1.4 to 2.6 mm and the overall length L1 is 6 to 14 mm is preferable.
Here, as for the gap for air vent formed between the side face part of the vent piece 1 and the side face part of the prepared hole for air vent, it is sufficient that a gap capable of satisfactorily releasing air so as to suppress the occurrence of spew is formed. Thus, with taking this point into consideration, the diameter D1 of the head part 11 and the diameter D2 of the trunk part 12 described above are set up suitably within the range given above.
The shape of the vent piece 1 is not limited to the above-mentioned cylindrical shape and may be a prism shape or another pillar shape.
It is preferable that the saw-cut 13 extending in the axial direction is formed in the side face part of the vent piece 1. When the saw-cut 13 like this is provided, even in the vent piece 1 of the same size, a passage of air is more satisfactorily ensured and hence the air vent function is improved further.
Further, in the vent piece 1, it is more preferable that the vent line 14 extending in the circumferential direction is formed between the head part 11 and trunk parts 12. When the vent line 14 like this is provided, the air having passed through the gap around the head part 11 is led through the vent line 14 to the saw-cut 13. Thus, the passage for air is more satisfactorily ensured and hence the air vent function is improved further.
As the specific shapes of the saw-cut 13 and the vent line 14, grooves of R0.1 mm to R0.4 mm or, alternatively, of similar shapes are preferable.
The formation of the saw-cut or the vent line is not limited to one location and may be performed at a plurality of, that is, two or more, locations. Further, in a case that passage for air is satisfactorily ensured even without the saw-cut or the vent line, the formation is not necessary.
Further, it is preferable that the twill knurl 15 is formed at least in a part of the surface of the side face part of the trunk part 12. The twill knurl 15 is formed in a diameter D3 that is similar to the prepared hole of the vulcanization mold in which the vent piece 1 is embedded and that is larger than the trunk part 12. Then, the twill knurl 15 prevents the vent piece 1 embedded in the vulcanization mold from falling off from the prepared hole. Further, air is satisfactorily released along a gap for air vent formed between the depressions and protrusions of the twill knurl 15 and the side face part of the prepared hole. Thus, the air vent function is improved further.
Here, the length L3 over which the twill knurl 15 is formed and the pitch of the twill are suitably determined with taking into consideration the embedment workability into the prepared hole of the vent piece 1, the property of preventing fall-off from the prepared hole, and the like. Specifically, a pitch of 0.3 to 0.7 mm is preferable.
Next, vulcanization of a pneumatic tire employing the above-mentioned vent piece is described below. Specifically, the above-mentioned vent piece 1 is embedded into the prepared hole for air vent provided in the inner face of a vulcanization mold 2 for pneumatic tire such that the head part is located on the vulcanization mold surface (
By virtue of this, at the time of vulcanization molding, air can satisfactorily be released through a gap for air vent formed between the side face part of the vent piece and the side face part of the prepared hole for air vent. Thus, a pneumatic tire can be obtained in which air remaining (bear) does not occur and occurrence of spew is also suppressed.
As described above, the size of the vent piece can be reduced in the present embodiment. Thus, at that time, the vent pieces can orderly be arranged and embedded even on a narrow line 21, as shown in
Here, in the vent piece, air is released through a slight gap formed between itself and the prepared hole. Thus, there is a possibility that the vent piece cannot release a large amount of air per piece in comparison with the spring vent. However, as described above, the vent piece can easily and orderly be arranged at a location at which the spring vent cannot orderly be arranged. Thus, the number of arrangements can easily be increased so that a satisfactory amount of air can be released in the entirety.
Further, arrangement of the vent piece can be achieved by providing a prepared hole for air vent in the inner face of the vulcanization mold. Thus, when necessary, additional arrangement can be performed later.
As shown in
The present invention is described below in further detail with reference to an implementation example.
The vent piece shown in
Here, the specification of the vent piece shown in
Embedment of the vent piece was performed at 24 locations on the circumference of the Maximum Flange Shield (MFS) top and at four locations on the circumference of the side part. Here, the reason why a large number of vent pieces were arranged on the circumference of the MFS top was that in the MFS top, when air vent fails, air remaining (bear) definitely occurs.
The external appearance was evaluated by visual observation of the fabricated tire for evaluation.
As a result, vent piece marks were hardly noticeable and hence it has been concluded that a pneumatic tire having a remarkably orderly external appearance was obtained. Further, also in the R40 curved surface in the side face, no abnormality has been found that could cause a particular problem.
Although embodiments of the present invention have been explained above, the present invention is not limited to the above-mentioned embodiments. Various changes can be added to the above-mentioned embodiments within the scope of the same as and equivalent to that of the present invention.
1, 31 vent piece
2 vulcanization mold
3 spring vent
11 head part
12 trunk part
13 saw-cut
14 vent line
15 twill knurl
21 narrow line
32 valve element
33 spring
D1 diameter of the head part
D2 diameter of the trunk part
D3 diameter of the twill knurl
L1 overall length
L2 thickness of the head part
L3 length over which the twill knurl is formed
P1, P2 vent mark
T tire
Number | Date | Country | Kind |
---|---|---|---|
2013-207863 | Oct 2013 | JP | national |
Filing Document | Filing Date | Country | Kind |
---|---|---|---|
PCT/JP2014/074345 | 9/16/2014 | WO | 00 |