The invention relates to charge coupled devices in general and particularly to a charge coupled device that includes an antireflection coating.
Scientific grade silicon CCD detectors offer substantial improvements in performance for detection of photons in the ultraviolet (100-300 nm) range of the electromagnetic spectrum. In particular, back-illuminated CCDs constructed using delta-doping technology and that have been passivated exhibit at least 30% quantum efficiency (QE) over that entire range, compared to the ˜5-10% achieved by microchannel plates that have been previously flown in space missions such as Galex. However, the performance of these delta-doped CCDs is limited due to the inherent reflectivity of the silicon itself. Anti-reflection coatings can, in principle, be applied to the silicon detector to improve the performance up to quantum efficiencies as high as 70%. However, the interface and film quality is critical for this theoretical performance to be achieved. Conventional sputtering and thermal evaporation techniques can be used to deposit films such as HfO2, MgF2, and MgO that should behave as anti-reflection coatings. However, recent experiments with these processes show that the film and interface quality achieved by these techniques are insufficient to achieve the desired quantum efficiency.
High carrier concentrations, for example carrier concentrations that can be induced by intense illumination such as a laser pulse, can lead to many body effects, band flattening, and reduction in minority carrier lifetime near the surface. Despite the exceptionally high charge density in the delta-doped layer, these effects may lead to nonlinearities in the detector response. In general, the quantum efficiency observed at high illumination levels may be lower than the quantum efficiency observed at significantly lower illumination intensities. However, hot carriers produced at such high illumination levels should not induce permanent changes to the detector.
At relatively low intensities, UV radiation can damage the Si—SiO2 interface by hot carrier degradation of the oxide and consequent formation of interface traps, as described by U. Arp et al., “Damage to solid-state photodiodes by vacuum ultraviolet radiation,” Journal of Electron Spectroscopy and Related Phenomena, 144-147: 1039-1042 (2005) and by P-S. Shaw et al., “Stability of photodiodes under irradiation with a 157-nm pulsed excimer laser,” Applied Optics, 44(2): 197-207 (2005). Trap formation is cumulative, and potentially irreversible, which is one reason why surface and interface passivation technologies that rely on initially low defect densities, such as thermally grown oxides and hydrogen passivation, may not remain stable under UV illumination.
At higher intensities, such as those achievable with pulsed laser sources, a single laser pulse may carry enough energy to cause extremely rapid melting and recrystallization of the surface under nonequilibrium conditions, as described by I. Luk{hacek over (e)} et al., “Study of Excimer Laser Induced Melting and Solidification of Si by Time-Resolved Reflectivity Measurements,” Applied Physics A, 54: 327-333 (1992), by R. {hacek over (C)}erný et al., “Nonequilibrium Solidification of Monocrystalline Si Induced by ArF-Excimer-Laser Irradiation,” Thermochimica Acta, 218: 173-182 (1993) and by T. Scheidt et al., “Ultraviolet pulse laser induced modifications of native silicon/silica interfaces analyzed by optical second harmonic generation,” Journal of Applied Physics, 100, 023118 (2006).
Nonequilibrium melting/recrystallization of the silicon surface can occur upon exposure to excimer laser pulses above an energy threshold of ˜0.4 J/cm2. Scheidt et al. measured a damage threshold using a nonlinear optical technique that is sensitive to interface trap density. According to Scheidt et al., the damage threshold is based on peak intensity, so even if the average intensity over the beam is lower than the threshold, they still observe damage at the center of the beam. The damage threshold corresponds to melting and recrystallization induced by single-pulse exposures. However, multiple subthreshold pulses are observed to create interfacial traps, with a cumulative effect on the Si—SiO2 interface. Assuming that the local temperature required to melt the surface is the same as the bulk silicon melting temperature (approximately 1410 C), then subthreshold exposures may cause high enough local temperatures to break bonds in the oxide. Silicon-hydrogen bonds can be broken at temperatures in the vicinity of 400-450 C, and SiO2 decomposition at the silicon surface occurs at temperatures above 800 C. Because the decomposition of SiO2 at the interface involves a chemical reaction with silicon at the interface, the chemical stability of the interface is also a potential concern under conditions of intense illumination.
At still higher intensities, laser ablation occurs, and the surface literally boils and explodes, leaving behind a crater, as described by Q. Lu et al., “Theory analysis of wavelength dependence of laser-induced phase explosion of silicon,” Journal of Applied Physics, 104, 083301 (2008).
With respect to devices having a delta-doped layer, there are at least three potential damage mechanisms relating to high UV illumination fluxes that one should consider. These include UV illumination-induced modifications of the Si—SiO2 interface (Scheidt et al.), UV illumination-induced oxidation of the interface as described by T. E. Orlowski, D. A. Manteli, “Ultraviolet laser-induced oxidation of silicon: The effect of oxygen photodissociation upon oxide growth kinetics,” Journal of Applied Physics, 64(9): 4410-4414 (1988), and UV illumination-induced surface melting and recrystallization as described by Luk{hacek over (e)} et al. and {hacek over (C)}erný et al.
Unlike other surface passivation technologies, delta-doped CCDs exhibit excellent stability when only a native oxide is present on the surface. Moreover, the sharply-peaked electronic potential at the delta-doped layer serves as a tunnel barrier to suppress the injection of surface-generated dark current into the bulk silicon comprising the minority carrier collection volume of the detector. Consequently, for low illumination intensities, UV-induced trap formation is not expected to be a significant threat to the stability of the delta-doped surface. This is in sharp contrast with chemisorption charging, which is vulnerable to permanent band-flattening due to accumulation of interface and oxide trapped charge, enhanced surface-generated dark current due to trap formation at the Si—SiO2 interface, and hot-carrier induced degradation of chemisorbed charge.
Under high photon fluxes, dynamic charging of the oxide may take place, as the surface is flooded with hot electrons and hot holes. In particular, different lifetimes of electron and hole traps in the oxide contribute to dynamic charging effects. These dynamic effects depend on materials and coating methods, including possible enhancement in thicker coatings due to the larger volumes involved. High quality, low defect oxides do not ensure long-term stability, as UV-induced damage is known to cause the formation of traps. Because of the high, localized charge in the delta-doped layer, the delta-doped surface is buffered against dynamic charging.
In delta-doped, n-channel CCDs and CMOS imaging arrays, the delta-doped surface comprises a sheet of dopant atoms typically located only 1-2 nm below the Si—SiO2 interface. At these length scales and for high-intensity illumination, UV-induced chemical reactions are a potential concern, depending on the illumination intensity and the ambient environment. UV laser irradiation is known to cause oxidation of the silicon surface, especially at photon energies sufficient to cause photodissociation of oxygen, as described by Orlowski et al. Orlowski et al. compared irradiation at 193 nm and 248 nm, and showed that photodissociation of oxygen at the shorter wavelengths dramatically increases the oxidation rate. The highest laser intensities in the Orlowski study reached the melting/recrystallization threshold.
According to Luk{hacek over (e)} et al., the depth to which melting occurs is sufficient to engulf the delta-doped layer. In some instances, an excimer laser can be powerful enough to induce melting/recrystallization of the surface when focused to subpixel spot sizes.
The ultraviolet represents an extremely important region of the electromagnetic spectrum as it has a critical role in a wide variety of scientific, commercial, and government applications. For example, ultraviolet spectroscopy can be utilized to study planetary atmospheres to determine whether basic elements for life such as oxygen, nitrogen, and hydrogen are present. A UV spectrometer can also detect evidence small quantities of complex organic molecules, (e.g., tholins), from the UV reflectivity of the surface of an icy moon providing information on how prebiotic chemistry takes place on extraterrestrial bodies. High sensitivity astronomical observations in the UV regime could enable the observation of faint emission from the baryons that form the intergalactic medium, which likely represent 50% of the detectable baryonic mass in the universe. Recent measurements enabled by the first all sky UV survey mission, GALEX, have uncovered a startling comet-like tail behind a red giant star that is streaking through space at nearly 300,000 miles per hour. This phenomenon is unique and can only be observed in the UV, and has now provided a means to characterize how stars can die and ultimately seed new solar systems through the shedding of carbon, oxygen, and other elements. Extreme UV lithography is utilized to pattern the finest features of the latest generation of semiconductor devices. UV laser inspection and imaging is therefore critical to identify defects in the fabrication process to maximize yield and reduce cost in this highly competitive industry. UV imaging has also recently been used in medical imaging to study how caffeine affects calcium ionic pathways in the brain. Rockets produce significant UV emission due to the production of excited nitrogen oxide species in their plumes. While infrared imaging is clearly an important anti-missile defense technology, UV can offer significant advantages in this application due to the ability to observe even in direct sunlight using “solar-blind” imaging. Bite marks can be readily observed and identified in forensic investigations since human saliva (wet or dry) shines brightly under UV illumination. Bruises are also evident for many days in UV after they have disappeared to the naked eye. As this only represents a small fraction of the real world applications of UV detectors, there is clearly strong motivation to have detectors with the highest possible sensitivity.
Unfortunately, despite this wide range of applications, scientific imaging in the ultraviolet is extremely difficult because the technology for sensing UV light is substantially limited by the quantum efficiency of available detectors and the transparency of optical coating materials. Many materials strongly absorb Near and Far UV light such that thicknesses of 20 nanometers or less are completely opaque. Thus, the UV throughput of an instrument is highly sensitive to impurities on, or contained in, any of the optical elements or the detector itself The absorption depth of UV photons is also very short, making collection of photo-induced current difficult with traditional materials. Compounding this problem is that many important sources of UV light are faint, so maximizing detector sensitivity is critical to unlock the true potential of UV imaging for the above applications.
Table 1 outlines two examples of ultraviolet sensitive detectors that are currently in use in space missions along with their typical quantum efficiencies in the near and far UV. Although new classes of III-V Nitride materials based on MBE or MOCVD grown GaN or AlGaN hold significant promise for future generations of UV detectors, they are expensive and extremely difficult to grow at sufficient quality to fabricate into imagers with low dark current and high responsivity. Silicon based charge coupled devices (CCDs), however, are based on the same fabrication technologies utilized in the semiconductor industry and are widely used in commercial imaging applications such as digital cameras. This makes silicon CCDs cheap to manufacture with the added benefit that pixel design and layout are both extremely flexible. CMOS (Complementary Metal Oxide Semiconductor) based imagers are also widespread, and their use in commercial and scientific applications has been accelerating over the last few years due to the rapid progress of the overall CMOS industry. Unfortunately, the native oxide that naturally forms on silicon causes unfavorable distortions in silicon's electronic band structure in the near surface region. This leads to the capture of UV produced photoelectrons in surface traps and thus very poor response below 300 nm for silicon imagers. This can be overcome though a combination of techniques known as back illumination and back surface passivation.
Prior art methods, such as chemisorption and ion implant/laser anneal, do exist to passivate the back surface of silicon CCDs. However, these methods have limitations in that they either do not achieve 100% internal quantum efficiency, have undesirably high dark current, and/or are subject to hysteresis and stability issues due to adsorption of oxygen and other gases in the environment on the surface of the CCD. There are also issues relating to the use of antireflection coatings with such passivation systems.
There is a need for systems and methods that can prevent damage to delta-doped back surface illuminated CCD photodetectors designed to operate in the UV region of the electromagnetic spectrum.
According to one aspect, the invention features a silicon photodetector. The silicon photodetector comprises a silicon die having at least one photodetector element configured to detect electromagnetic radiation in a wavelength of interest, the silicon die having a silicon surface configured to receive the electromagnetic radiation, and having at least one terminal configured to provide an electrical signal representative of a property of the electromagnetic radiation, the silicon die having a doped layer situated within 5 nanometers of the surface, the silicon die having a silicon oxide layer with a first oxide surface adjacent the silicon surface and a second oxide surface on a side opposite the first oxide surface; a buffer layer comprising a chemically-resistant material having a first buffer layer surface adjacent the second surface of the silicon oxide layer, the buffer layer of the chemically-resistant material having a thickness configured to render the buffer layer of chemically-resistant material optically innocuous at the wavelength of interest, and having a second buffer layer surface on a side opposite the first buffer layer surface; and an antireflection layer configured to be transparent to electromagnetic radiation in the wavelength of interest, the antireflection layer having a first antireflection layer surface adjacent the second buffer layer surface. The buffer layer is configured to prevent the electromagnetic radiation in the wavelength of interest from causing a chemical reaction of the silicon oxide layer with the antireflection layer.
In one embodiment, the doped layer situated within 5 nanometers of the surface is a delta-doped layer.
In another embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using MBE technology.
In still another embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using ion implantation.
In a further embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using chemical vapor deposition.
In one embodiment, the buffer layer comprising a chemically-resistant material is Al2O3.
In another embodiment, the Al2O3 buffer layer has a thickness in the range of 1 nm to 23 nm.
In yet another embodiment, the antireflection layer comprises at least one material selected from the group of materials consisting of HfO2, MgF2, Al2O3, SiO2, LiF, Si3N4, and MgO.
In still another embodiment, the electromagnetic radiation in a wavelength of interest is electromagnetic radiation in the wavelength range of 100 nm to 300 nm.
According to another aspect, the invention relates to a method of providing an antireflection layer on a silicon photodetector. The method comprises the steps of providing an silicon photodetector comprising a silicon die having at least one photodetector element configured to detect electromagnetic radiation in a wavelength of interest, and having at least one terminal configured to provide an electrical signal representative of a property of the electromagnetic radiation; producing on the silicon die a doped layer with an overcoat of silicon configured to situate the doped layer within 5 nanometers of a silicon surface; creating a silicon oxide layer with a first oxide surface adjacent the silicon surface and a second oxide surface on a side opposite the first oxide surface; depositing on the second oxide surface of the silicon oxide layer a buffer layer comprising a chemically-resistant material having a first buffer layer surface adjacent the second surface of the silicon oxide layer, the buffer layer of the chemically-resistant material having a thickness configured to render the buffer layer of chemically-resistant material optically innocuous at the wavelength of interest, and having a second buffer layer surface on a side opposite the first buffer layer surface; and depositing on the second buffer layer surface an antireflection layer configured to be transparent to electromagnetic radiation in the wavelength of interest, the antireflection layer having a first antireflection layer surface adjacent the second buffer layer surface. The buffer layer is configured to prevent the electromagnetic radiation in the wavelength of interest from causing a chemical reaction of the silicon oxide layer with the antireflection layer.
In one embodiment, the doped layer situated within 5 nanometers of the surface is a delta-doped layer.
In another embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using MBE technology.
In still another embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using ion implantation.
In a further embodiment, the doped layer situated within 5 nanometers of the surface is a doped layer fabricated using chemical vapor deposition.
In one embodiment, the buffer layer comprising a chemically-resistant material is a buffer layer of Al2O3.
In another embodiment, the buffer layer of Al2O3 has a thickness in the range of 1 nm to 23 nm.
In still another embodiment, the buffer layer of Al2O3 is deposited using atomic layer deposition.
In yet another embodiment, the antireflection layer comprises at least one material selected from the group of materials consisting of HfO2, MgF2, Al2O3, SiO2, LiF, Si3N4, and MgO.
According to yet another aspect, the invention relates to a silicon photodetector. The silicon photodetector comprises a silicon die having at least one photodetector element configured to detect electromagnetic radiation in a wavelength of interest, the silicon die having a silicon surface configured to receive the electromagnetic radiation, and having at least one terminal configured to provide an electrical signal representative of a property of the electromagnetic radiation, the silicon die having a doped layer situated within 5 nanometers of the surface, the silicon die having a silicon oxide layer with a first oxide surface adjacent the silicon surface and a second oxide surface on a side opposite the first oxide surface; and a chemical passivation layer comprising a chemically-resistant material having a first chemical passivation layer surface adjacent the second surface of the silicon oxide layer, and having a second chemical passivation layer surface on a side opposite the first chemical passivation layer surface, the chemical passivation layer configured to be transparent to electromagnetic radiation in the wavelength of interest, the chemical passivation layer configured to prevent the electromagnetic radiation in the wavelength of interest from causing a chemical reaction of the silicon oxide layer.
The foregoing and other objects, aspects, features, and advantages of the invention will become more apparent from the following description and from the claims.
The objects and features of the invention can be better understood with reference to the drawings described below, and the claims. The drawings are not necessarily to scale, emphasis instead generally being placed upon illustrating the principles of the invention. In the drawings, like numerals are used to indicate like parts throughout the various views.
Atomic Layer Deposition (ALD) is a thin film deposition technique similar to chemical vapor deposition (CVD) in which a desired film is grown using sequential surface reactions, one monolayer at a time. The ALD method enables the growth of smooth, dense, pin-hole free films with angstrom level thickness control over arbitrarily large surface areas. In particular, the layer by layer growth allows one to precisely tailor the interface between the imager where the photons are adsorbed and the anti-reflection coating. This is highly advantageous as the MBE grown delta-doped layer is located less than 2 nm from the surface of the imager, and any reaction at the interface with the AR coating, for example, forming HfSiO4 (hafnium silicate), would disrupt the surface and degrade the device performance. Using the atomic scale control of the surface that is achievable with delta-doping and atomic layer deposition, both the stability and the interfacial band offsets are amenable to engineered improvements by the design of the delta-doped layer structure, and by the incorporation of nanometer-scale interlayers that have reduced chemical reactivity at the interface.
One can chemically passivate the silicon surface using ALD growth of stable, nanometer-scale passivation layers. SiO2 is known to be unstable over time, and other surface coatings have been proven to be more stable against UV-induced damage. Chemical passivation of the interface can be done by coating the surface with a thin layer of Al2O3, either on top of the native SiO2 or on a hydrogen-passivated surface. If an antireflection coating is desired, the same process can be used to incorporate a chemically stable interlayer (such as Al2O3) between the silicon surface and the antireflection coating. Such an interlayer is expected to improve the stability of the surface against UV-induced chemical reactions at the interface. A chemical passivation layer can prevent laser-induced chemical reactivity from causing permanent damage to the silicon surface or surface passivation layer.
High performance surface passivation layers, such as delta-doping and multilayer doping layers formed by molecular beam epitaxy, may require protection against UV-induced oxidation or other chemical attack to the silicon surface. A chemical passivation layer, such as a layer of Al2O3 that is between 1 nm and 2 nm in thickness is expected to prevent such chemical attacks from damaging the surface passivation layer. A chemical passivation layer is expected to extend the lifetime of the detector by slowing the rate of chemical attack. A chemical passivation layer is expected to extend the lifetime of detectors exposed to UV laser radiation.
Our work on anti-reflective ALD Al2O3 as a single layer anti-reflective coatings has been demonstrated to have >50% QE at 180 nm. This same approach using different chemical precursors suitable for deposition of MgF2, MgO, HfO2 and other dielectrics is expected to provide antireflection coatings covering the 100-300 spectral range with a promise of reaching 50-70% QE and potentially improving the current UV QE by nearly an order of magnitude, as compared to GALEX detectors having a QE of about 5-10%.
In one embodiment, wafers of Si CCD detectors were diced into “raft” sections with 12 die per raft. These rafts were thinned using standard wet processing techniques to produce frame supported Si membranes for each die. These membranes were cleaned to remove surface contamination and oxides, and were subsequently delta-doped by MBE. The completed raft was then diced into the 12 individual die. The die were individually cleaned. To apply an AR coating, one of these die was loaded into an Atomic Layer Deposition system. A shadow mask was placed on the imaging surface to define a coated and uncoated region. An antireflection coating was applied. The coated region was verified to have the desired QE by testing the device in a vacuum UV test stand.
Prior to this work, we were unaware of any anti-reflection coatings that have been successfully demonstrated for silicon based imagers in the 100 nm-250 nm range of the ultraviolet spectrum. Atomic layer deposition is the first successful approach that can be used over this entire wavelength range due to its ability to produce high quality Al2O3, MgO, MgF2, SiO2, and HfO2 coatings. In the present embodiments, extremely thin ALD Al2O3 layers (˜1 nm thick) are used as buffer layers between the MBE delta-layer and the potentially reactive AR coatings. The 1 nm ALD Al2O3 is sufficiently thin to be optical inactive, but thick enough to be a chemical barrier to preserve separation the silicon and AR coatings. This approach of ultra-thin barrier layers embedded in multilayer AR coatings can only be accomplished with methods such as ALD that allow the deposition of substantially monoatomic layers.
We describe a new technique that combines the atomic precision of molecular beam epitaxy and atomic layer deposition, to fabricate silicon CCD detectors that demonstrate high detector quantum efficiency (>50%) in the near and far ultraviolet (155 nm-300 nm). We describe in detail the unique surface engineering approaches used and demonstrates the robustness of detector performance that is obtained by achieving atomic level precision at all steps in the fabrication process. The characterization, materials, and devices produced are compared to results obtain using other approaches. As ultraviolet imaging systems have the potential to detect life on other planets, explain the origins of the universe, identify defects in the latest generation of semiconductor devices, perform medical imaging and brain mapping, improve missile defense, and even solve crimes, this new approach to UV detector fabrication is expected to have an important impact on a wide range of fields.
Surface passivation by delta-doping using silicon molecular beam epitaxy, enables precise control over the band structure at the CCD surface to get ideal Si reflection-limited response (see
Even with ideal back surface passivation, the inherent reflectivity of silicon significantly limits the absolute detector quantum efficiency of silicon CCDs. This is illustrated by the dip in quantum efficiency to ˜25% near 280 nm in
AR coatings are widely utilized for many detector systems (silicon, III-V, and others) in the visible and infrared to improve absolute quantum efficiency. However, producing UV anti-reflection coatings is extremely challenging as the coatings must be extremely high quality. The AR coatings preferably should exhibit low impurity/defect concentration to avoid UV absorption, and preferably should be pinhole free and dense to prevent humidity interaction with the imager surface. In addition, the index of refraction of silicon varies significantly over the UV, and therefore multiple different materials may be required to cover the Near and Far UV effectively. This is especially important because even ideal materials have absorption cut offs that make them opaque in certain regions of the UV. In addition, a change of 2 nm or less can dramatically shift the peak anti-reflection performance or lead to dramatic changes in absorption cutoffs, especially in the far UV, making controllable and reproducible fabrication of ultrahigh performance AR coated silicon CCDs difficult. Recent modeling results by Hamden et al. (submitted to Applied Optics (2011)) have demonstrated that the target thicknesses for UV anti-reflective coatings range from 10 to 25 nm. When all of these constraints are combined (back-illumination, silicon band structure engineering/surface passivation, and AR coating deposition with sub-nanometer precision and accuracy), a series of sequential robust, nanoscale, surface-engineering processes are required to produce the best possible UV sensitive CCDs.
Wafers containing fully fabricated CCDs of several types were acquired for from multiple commercial sources. These included flight spare CCD wafers, manufactured by Loral for the imagers in the Cassini spacecraft mission that is currently flying in the Saturn system, CCDs imagers obtained from EG&G Reticon, and wafers containing newly designed electron-multiplied CCDs (EM-CCDs) from e2v (of 520 White Plains Road, Suite 450, Tarrytown, N.Y. 10591). These EM-CCDs combine the high ultraviolet quantum efficiency of silicon imagers with a gain register which results in measurements with extremely high signal to noise ratio (as high as 10,000:1), enabling them to be utilized in photon counting applications. These three different types CCDs were utilized to demonstrate the robustness of the techniques in this investigation and show that this is a generally applicable approach to enhance the UV quantum efficiency of any type of silicon imager.
The CCDs were set up for back-illumination to remove the front side circuitry from the photon pathway. The bulk thickness of the CCDs is reduced by polishing and chemical etching to leave a thin membrane. The final thickness of the membrane after this process is thick enough so that it has sufficient mechanical strength to withstand its environment. The membrane is also thin enough so that charge carriers produced at the back surface do not drift too far laterally as they are swept to their destination pixel on the front side. This maps the point of photon impact to a specific front side pixel in the image. CCDs are produced with an epitaxial layer that provides a natural definition for the membrane thickness. It is uniform across the entire CCD and provides a chemical etch-stop for the thinning process. The membrane is created in a way that makes it monolithic with a thick frame of original silicon from the CCD. The front side CCD circuitry resides over regions that are thick frame and thin membrane. The thick frame serves the purpose of mechanically supporting the membrane and it makes it convenient to wire bond the imaging device using its existing bond pads. Residual stresses in the imaging membrane can result in macroscale deformations when the frame thinning approach is used (see
In the frame thinning approach, the backside of the CCD wafer is polished by chemical mechanical polishing (CMP) and the membrane region is defined by a nitride mask on the polished surface. The bulk silicon is aggressively etched by hot 55% KOH except for the frame defined by the nitride mask. We monitor the progress of the etch and terminate when it comes within 20 microns of the known epitaxial layer thickness. The surface texture of the KOH etch is rough by comparison to the CMP surface. This condition is rectified by the next step in which etching is performed using a specific mixture of hydrofluoric, nitric and acetic acids (HNA) in the relative volumes of 1:3:8. This mixture of HNA continues the etch to the epitaxial layer where it self-terminates upon exhaustion of bulk silicon. The well defined etch stop is caused by the higher resistivity of the epitaxial layer. The epitaxial layer has many orders of magnitude fewer charge carriers on hand for participation in the chemical reaction of the etch. The etch reaction stops as it is starved for charge carriers. Additional brief etch exposures are made to mixtures of 1:40:15 HNA and KMnO4/HF. These solutions help to remove certain stains and haze which are left by the previous reactions. The resulting thin membrane has a smooth mirror-like specular finish.
The CCDs are brought into an inert and clean glove box environment to prepare for electrical passivation and band structure engineering. A UV ozone clean is utilized to remove carbon and other organics, and a HF-ethanol spin clean is utilized to remove the native oxide from the imaging membrane. Thes backside surface of the imager is then passivated by delta-doping. Briefly, in delta-doping, an extremely thin silicon layer is grown epitaxially using a low temperature (lower than 450° C.) molecular beam epitaxy process. This silicon epitaxially grown layer is delta-doped during the growth process by incorporating a third of a monolayer of boron atoms, effectively as a single atomically thin sheet that does not interrupt the overall silicon epitaxy, but dramatically affects the electronic band structure of the silicon in the near surface region. This delta-doped layer enables the CCD to operate at 100% internal quantum efficiency (QE), limited only by reflection of light from the silicon surface. In some embodiments, a plurality of delta-doped layers, separated by layers of silicon having no deliberately added dopants, may be provided, as described in more detail in U.S. patent application Ser. No. 13/160,534.
Anti-reflection (AR) coatings were tested to improve the imaging performance of these silicon CCDs. However, the index of refraction of the silicon changes significantly in the ultraviolet region of the spectrum, especially from 100 to 300 nm. Therefore, to obtain optimum quantum efficiency, it was necessary to test multiple different thin film coatings and coating methods. Contact shadow masks such as the one shown in
Once the AR coatings were applied to the CCDs, they were packaged for testing in a custom built UV-Visible CCD characterization system described in Jacquot, B. C. et al., “A system and methodologies for absolute QE measurements from the vacuum ultraviolet through the NIR,” Rev Sci Instrum (2011, in review). Briefly, imaging performance of the CCD was characterized from 121.6 nm to 650 nm starting from the longer wavelength end of the spectrum by taking flat field images over controlled exposure times. Two separate light sources were used for illumination (Deuterium lamp at FUV and Tungsten-Halogen for NUV). Absolute QE measurement was made by comparison to a NIST calibrated photodiode that could be positioned in the same location as the CCD being characterized. Some of the CCD characterization data was obtained at Reticon in a different testing system of similar design.
Thinned, delta-doped Cassini and Reticon CCDs were utilized to evaluate thin film AR coating techniques and materials for their ability to improve absolute detector quantum efficiency. Magnesium oxide and hafnium oxide were deposited by physical sputtering. Hafnium oxide AR coatings were also deposited by electron beam evaporation and thermal evaporation. Hafnium oxide and aluminum oxide were deposited by atomic layer deposition. This combination of materials and deposition methods was chosen to elucidate the efficacy of each deposition technique within the constraints of the limited number of CCDs available for the experiments. Examples of flat field images obtained from some of the partially AR coated CCDs produced in this work are shown in
The design and accurate prediction of the performance of ALD AR coatings was straightforward due to the inherent reproducibility and control of the ALD technique.
As ALD's inherent advantages of control and uniformity make the technique preferable to thermal evaporation, PEALD HfO2 was also pursued. However, since remote plasma ALD of hafnium oxide on hydrogen terminated silicon is known to lead to the formation of a hafnium silicate interfacial layer, transmission electron microscopy was utilized to determine whether a similar silicate would form during HfO2 deposition on a delta doped silicon wafer. An air exposure step occurs between the delta-doping process and the deposition of the ALD AR coating, so a native oxide silicon oxide is present prior to the ALD process. The TEM image in
X-ray photoelectron spectroscopy (XPS) was employed to provide further confirmation of whether the 2 nm aluminum oxide layer was sufficient to prevent the formation an interfacial layer. Samples were prepared where twenty five ALD cycles (˜1.2 nm) of HfO2 were deposited on silicon and 2 nm of Al2O3 were deposited on silicon.
Since the problem that the aluminum oxide solves is degradation of the doping layer near the back surface of the thinned wafer, it is expected that the aluminum oxide layer will control the degradation of the back surface of a silicon photodetector without regard to how the doping layer is fabricated. By way of example, it is expected that application of the Al2O3 technology will be equally effective if the doping near the back surface is provided using MBE, ion implantation, CVD, or any other deposition process.
A back-illuminated photodetector device having at least one delta-doped layer close to the surface that is expected to receive the illumination and having a thin layer of a chemically stable (or chemically-resistant) material such as Al2O3 that is provided as a layer that provides separation between an oxide such as SiO2 present on the device and materials applied to provide an antireflection coating so as to prevent their chemical reaction, but that is thin enough to be optically innocuous, can be fabricated as described hereinabove. The antireflection coating is fabricated from one or more materials which can be selected to provide optical transparency in a desired region of the electromagnetic spectrum. In some embodiments, the antireflection coating can include one material in a single layer. In other embodiments, the antireflection coating can comprise a plural number of layers of different materials.
It is recognized that any material, of any thickness, will in principle modify or change the properties of electromagnetic illumination that interacts with the material. As used herein, the term “optically innocuous” means that the chemically stable or chemically-resistant material is thin enough that it does not interact with incident illumination having a wavelength of interest to an extent that the optical properties of the illumination are changed enough to affect a measurement of such optical properties. The optical properties of the incident illumination that are expected not to be affected can include, but need not be limited to, one or more of such properties as an intensity, a wavelength, and a polarization of the incident illumination.
Although the theoretical description given herein is thought to be correct, the operation of the devices described and claimed herein does not depend upon the accuracy or validity of the theoretical description. That is, later theoretical developments that may explain the observed results on a basis different from the theory presented herein will not detract from the inventions described herein.
Any patent, patent application, or publication identified in the specification is hereby incorporated by reference herein in its entirety. Any material, or portion thereof, that is said to be incorporated by reference herein, but which conflicts with existing definitions, statements, or other disclosure material explicitly set forth herein is only incorporated to the extent that no conflict arises between that incorporated material and the present disclosure material. In the event of a conflict, the conflict is to be resolved in favor of the present disclosure as the preferred disclosure.
While the present invention has been particularly shown and described with reference to the preferred mode as illustrated in the drawing, it will be understood by one skilled in the art that various changes in detail may be affected therein without departing from the spirit and scope of the invention as defined by the claims.
This application claims priority to and the benefit of co-pending U.S. provisional patent application Ser. No. 61/357,922, filed Jun. 23, 2010, which application is incorporated herein by reference in its entirety. This application is also related to U.S. patent application Ser. No. 12/965,790 filed Dec. 12, 2010 (which was published on Jun. 16, 2011 as U.S. patent application Publication No. 2011/0140246 A1), to U.S. patent application Ser. No. 13/160,534 filed Jun. 15, 2011, and to U.S. Pat. Nos. 4,798,598, 4,822,748, 4,882,609, 5,316,586, 5,376,810, 5,701,016, 6,403,963, 7,786,421 and 7,800,040, each of which patents, patent application publications and patent applications is incorporated herein by reference in its entirety, and all of which are commonly assigned to the assignee of the present application.
The invention described herein was made in the performance of work under a NASA contract, and is subject to the provisions of Public Law 96-517 (35 USC 202) in which the Contractor has elected to retain title.
Number | Date | Country | |
---|---|---|---|
61357922 | Jun 2010 | US |