The present invention relates to the mechanical cleaning of ferrous and non-ferrous metal wire forming a semi-finished product produced in coils by means of hot rolling, which is usually defined as wire rod, and intended for the production of drawn products.
Drawing is a cold process that consists in passing a wire through a die with a smaller section than the wire, which assumes the same shape as the die because of plastic deformation. Such a process can be repeated in subsequent steps until a wire with a desired diameter or profile is obtained, which can be different from the round shape.
Drawing is a very simple technological process, which has been known since ancient times to draw metals and has never changed conceptually. On the other hand, the boundary conditions have changed, making this process more and more efficient and cost-effective.
During the passage of the hot semi-finished products to the cold working, which is typical of the drawing process, the wire must be adequately prepared by accurately removing an aggregate of oxides and hydroxides that is inevitably formed on the surface of the material at high temperature in a damp, oxidizing environment, such as the natural atmosphere.
In ferrous materials, such an aggregate is composed of chemically and physically diversified layers, ranging from superficial oxidation to the formation of very minute, powdery and extremely adherent scales housed within the typical craterings of a laminated surface, up to millimeter dimensions, which are puff-shaped, crusty and very brittle. In the various chemical and physical forms, these scales are hard and remarkably abrasive.
A removal of these formations is necessary before drawing because, in addition to being an unwanted component for the quality of the product, the presence of these formations determines a rapid wear of the die, a strong limitation of the working speed, a substantial limitation of the efficiency of the systems, and very importantly, a conditioning to any further processing after the drawing process.
According to the prior art, such a preparation is performed with operating methods that are essentially attributable to two conceptual principles, which respectively correspond to methods of chemical or mechanical type.
The chemical methods are implemented by means of processes that basically perform a wet pickling of the wire rod. These techniques offer very high-quality levels of cleaning and preparation, with the application of particular compounds, which are optimal for drawing. However, they entail considerable installation costs, and especially management costs, because a rigorous treatment of the waste water is mandatory to guarantee compliance with the anti-pollution parameters. Nevertheless, in spite of an unquestionable quality of the products, these chemical methods are relentlessly regressing at worldwide level and are exclusively reserved to strategic materials with a high technological profile.
In spite of the lower cleaning quality, the mechanical methods are increasingly acquiring a predominant role in large-scale product consumption because of the simplicity of the devices and of the low operating costs that are especially determined by a limited environmental impact. Furthermore, production users are increasingly demanding and pretending high-performing results that are similar to the yield of the chemical method also at qualitative level. It goes without saying that this only applies to cleaning, since the mechanical method is exclusively a removal method, whereas the preparation for drawing, with the addition of specific products, evidently requires a chemical method, the efficiency of which depends on the accuracy of the surface preparation. At present, a multitude of techniques of different kind are proposed and compared based on cost-effectiveness, in terms of both installation and operation, and effectiveness. However, effectiveness is generally not reconciled with the desirable cost-effectiveness in terms of investment and management.
The most interesting and most popular techniques of the prior art, which will be briefly described below, are characterized by advantages and, inevitably, by disadvantages that must be carefully evaluated when making a choice.
Almost all of these techniques involve a multi-stage treatment. A first preliminary stage that is common to all methods consists in the removal of the outer, coarse and easily removable scale. Such a first stage takes place in a relatively simple way by breaking the scale, alternately bending the wire rod, which is uncoiled and pulled by the drawing machine, with passages on different rollers arranged sequentially and lying in the space on different planes.
Although the calamine is removed almost completely in this stage, the remaining quantity is small, but difficult to remove. This is the aspect in which the various methods differentiate.
A very important and accredited method consists in sanding or shot blasting, wherein abrasive grains are ejected at high speed onto the surface of the wire rod, being conveyed by a flow of air generated by turbines. The quality of such a method is very high, given that the grains are able to penetrate right into the lamination craterisations and expel even the smallest calamine residues, while adapting to any form of material shape. Conversely, costs are high both for the installation, which is structured in a very complex set of components, and for the management because of the low yield, due to the limited surface exposed to the abrasive flow and, above all, due to the considerable energy expenditure.
Other systems provide for using different types of abrasives that are directly applied with rigid or flexible supports. Said systems can be either dynamic, wherein a rotational or sliding motion is combined with the movement of the wire, or static systems, wherein the abrasion action solely occurs because of the forward movement of the wire rod.
The multiplicity of systems is truly varied and each one of them is characterized by its own specificity. Among these, a family of devices is distinguished for its diffusion and application variants, which use rapidly rotating circular steel brushes that act in tangent direction with the tip, with elementary wires, on the external part of the wire rod to be treated. Furthermore, a new family of devices has recently been added, which uses abrasive bands in sliding and in planetary rotation on the axis of the wire rod. It is an effective, yet especially expensive technique.
Another system consists in the use of steel wool as abrasive, in loose form and unconstrained by any reinforcement, as for the aforementioned brushes. The use of such an abrasive has numerous advantages, even considerable ones, compared to the methods described:
In the name of the same applicant, EP0931601 and EP1110638 disclose devices for the cleaning of wire rods that use steel wool manually wrapped around a wire and clamping jaws that apply pressure on the steel wool.
In the name of the same applicant, EP0630697 discloses a device used to apply pressure on the steel wool.
The devices described in EP0931601, EP1110638 and EP0630697 adopt a system of clamping jaws suitable for confining the steel wool in a volume around the profile of the wire rod and for applying such a pressure to induce an abrasion action on the surface of the wire in transit with the lateral cutting edges of the thin strip that forms it into the shape of a blade. The abrasive effect is determined by both the applied pressure and, above all, the relative speed of the cutting edge with respect to the surface of the material. In EP0931601 and EP1110638 the abrasive effect is exclusively given by the speed of the wire rod in transit, wherein in EP0630697 the abrasive effect is combined with a rotational movement that depends on the rotational speed of the rotor, which supports and confines the steel wool, and on the diameter of the wire rod that, in this case, must necessarily have a circular profile.
Evidently, in EP0931601 and EP1110638, the cutting speed is not very high, depending on the specifications of the drawing machine and on the process; also in EP0630697, in spite of having a high rotational component, the cutting speed can never reach very high levels due to the intrinsic smallness of the wire diameter.
In fact, the quality of the treated material depends on many factors, above all its composition, the type of cooling during the rolling stage and the exposure to atmospheric elements during storage. In many cases these real limitations do not prevent a general good result, always relative to the destination of the final product, especially in view of the incomparable simplicity and operating economy.
DE7019427U and DE10224603A1 disclose different devices wherein a glass wool container is rotated around a wire.
The purpose of the present invention is to eliminate the drawbacks of the prior art, by disclosing a device for the mechanical cleaning of wire rods for the production of drawn metallic wire that is efficient, effective and reliable.
Another purpose is to disclose such a device for the mechanical cleaning of wire rods that is versatile and simple to make and use.
These purposes are achieved in accordance to the invention with the characteristics of the independent claim 1.
Advantageous embodiments of the invention appear from the dependent claims.
The device for the mechanical cleaning of wire rods according to the invention is defined by the independent claim 1.
The adoption of steel wool is more attractive than the prior art and a more effective effect is desirable for cases where a better finishing is required.
The present invention provides for applying the steel wool in loose form at high speed.
Due to its loose state, the steel wool must be contained in a defined volume, i.e. a container, which is closed around the wire in the case of the aforementioned applications. However, if a high relative speed is to be achieved, this container must be inevitably freed from the wire and external, similarly to a brush, but without reinforcements or prefabricated structures. Furthermore, in order to exert its action on the wire rod, the abrasive must come into contact with the wire rod through appropriate openings. Consequently, the container cannot be completely closed.
In conditions of rapid rotation within such a volume, for geometrical reasons of annular conformation, centrifugal forces are generated, which increase with the distance from the axis of rotation and with the square of the angular velocity. With the same peripheral speed of a generic portion of abrasive, the higher the size of the radius of curvature of the trajectory, the lower said forces will be. However, since the physical dimensions of the device must be limited, for convenience and practicality of use, the forces acting on the loose mass are of considerable value, and therefore the loose mass must be constrained, necessarily excluding circumferential openings of any type to prevent the loose mass from escaping and being subsequently broken down.
Additional characteristics of the invention will appear manifest from the following description, with reference to the appended drawings, which are a merely illustrative and not limiting embodiment, wherein:
With reference to the figures of the appended drawings, the invention relates to a device (1) for the mechanical cleaning of a wire rod (20) used in particular for the production of metal wires by means of drawing.
With reference to
A shaft (6) supports the elements (8) in specular position relative to a plane of symmetry (17). The elements (8) can be easily removed from the shaft (6). The elements (8) are mounted in an assembly between an adapter (11) and a spacer (7) and are tightened on the shaft (6) by means of a nut (12) and a stud bolt (13).
The shaft (6) is revolvingly supported by rolling bodies on a suitable structure (7a) (shown with a broken line), in such a way that the shaft (6) can rotate at a high speed, for example in the direction of the arrow (21).
Each element (8) comprises components that define a compartment (40) where an agglomerate abrasive material, such as steel wool (4), is housed. The steel wool (4) is the active abrasive component.
A hub (5) is coupled with the shaft (6).
With reference to
Advantageously, the shaft (6) and the hub (5) are of splined type for a splined coupling.
With reference to
With reference to
A space (19), which is wider than the diameter of the wire rod (20), remains between the flat disks (2) of the two elements (8). In view of this, the wire rod (20) can be inserted in the space (19) without obstacles or interferences. As a matter of fact, the wire rod (20) exclusively interferes with the steel wool (4) that comes out of the openings (18) of the flat disk (2).
The shaft (6) rotates at high speed around its rotation axis (25) along the rotational direction (21) or in opposite direction. The rotation of the shaft (6) drives the two elements (8) into rotation.
During the rotation of the two elements (8), centrifugal forces (9) are exerted on the steel wool (4), expanding the steel wool (4) radially outwards.
Given the tapered conformation of the truncated-conical body (3), the steel wool (4) is wedged radially into an ever-smaller volume of the element, generating an axial component (10) that pushes the steel wool (4) towards the flat disk (2).
Such an axial component (10) forces the steel wool (4) to come out of the holes (18) of the flat disk (2). Due to the particular shape of the openings (18) of the flat disk (2) and to the elastic property of the steel wool, the steel wool (4) is only partially ejected into bulges that escape from the openings (18) of the flat disk (2), partially occupying the space (19) that is transversely crossed by the wire rod (20) in a skewed direction with respect to the axis of rotation (25) of the shaft.
Because of the rotation of the device (1), the steel wool pads that are extroflected from the openings (18) of the flat disk (2) interfere with the rod wire (20) in transit, in a controlled manner, exerting a simultaneous rubbing on the two opposite sides.
The abrasive effect of the steel wool (4) is directly correlated with the contact speed of the cutting edges of the steel wool, and with the surface of the wire rod in contact with the cutting edges of the steel wool. Such a contact speed depends on the rotational speed of the device (1) and on the distance of the wire rod (20) from the axis of rotation (25) of the shaft (6).
The value of the forces applied on the steel wool mass also depends on the angular velocity of said steel wool mass. Such an angular velocity of the steel wool mass cannot be excessively high to avoid instability phenomena due to cohesion failure and consequent uncontrolled expulsion of steel wool parts.
However, it is essential to ensure an axial thrust such as to extroflect the steel wool through the openings (18) of the flat disk (2). The centrifugal forces (9) that are inertially created on the low density mass of the steel wool, at a safety rotational regime, are insufficient to ensure a stable and reliable working equilibrium during operation.
For this reason, it is necessary to create an additional controllable centrifugal thrust. Such an additional centrifugal thrust is given by the construction of the hub (5) that incorporates the oscillating masses (15).
With reference to
With reference to
In view of the above, the efficiency of such a device is manifest, it being able to maintain control of a loose and non-compact mass, such as the steel wool, subject to disintegrating forces, and to exploit the high effectiveness of the high-speed abrasion process of the steel wool.
The wire rod (20) travels in forward direction with a continuous movement along the forward traveling direction indicated by the arrow (27) towards a drawing machine installed downstream the device (1). The wire rod (20) is driven by pulleys (22).
By rotating the mobile support (28) around the axis of rotation (29) in the direction of the arrow (26), the device (1) passes from the non-operating position to an operating position (shown in
With reference to
A system can comprise a plurality of devices (1). Each device (1) is sequentially applied along a forward traveling direction of the wire rod (20) and on different working planes that are parallel to the axis of the wire rod in order to increase the cleaning effect and the uniformity on the entire circumference of the profile of the wire rod.
Number | Date | Country | Kind |
---|---|---|---|
102018000010644 | Dec 2018 | IT | national |
Filing Document | Filing Date | Country | Kind |
---|---|---|---|
PCT/EP2019/082544 | 11/26/2019 | WO | 00 |