The present invention relates to compositions for imparting wear resistance to superalloy articles and, in particular, to compositions for metallurgically bonding alloy wear plates or pads to superalloy articles, such as Z-notch contact surfaces of turbine blades.
Turbine blades used in gas turbine engines for various industrial, power generation, marine, and transportation applications have a shroud with so-called Z-notches which are configurations in the turbine blade shroud having a “Z” shape. Adjacent blades interlock at the Z-notches. Because these Z-notches are points of contact between adjacent turbine blades, the contact faces of Z-notches experience wear and erosion.
Turbine blades are generally cast from superalloys having high levels of nickel and/or cobalt. Surfacing, resurfacing and repairing components made from nickel-based superalloy and other superalloys by welding techniques present serious technical challenges. For example, high heat input weld overlay processes can disadvantageously impart a heat-affected zone to the substrate and alter material characteristics near the heat-affected zone, often causing the blade to become embrittled in that region. Thermal spray processes require substantial clean-up which is inefficient and can risk substrate damage, and the resulting bond is primarily mechanical and not as good as a true metallurgical bond.
In some applications, contact faces of Z-notches are resurfaced with wear pads or plates. Presently available pads exhibit acceptable wear properties at elevated temperatures. However, these wear pads can slump and/or fall off the bucket if the turbine blades experience temperatures above 1200° C. for time periods exceeding 2 hours during blade manufacture or repair. This problem is acute for buckets requiring repair via hot isostatic pressing and rejuvenation steps at temperatures well above 1200° C. In such cases, the wear pads are removed every time the bucket is repaired leading to increases in cost and turbine downtime.
In view of these disadvantages, alloy compositions are provided for imparting wear resistance to superalloy articles, including Z-notches of turbine blades. In some embodiments, the alloy compositions exhibit high temperature stability resistant to deformation during superalloy repair and/or rejuvenation processes. In one aspect, composite preforms are provided for imparting wear resistance to superalloy articles. The composite preforms, in some embodiments, can be employed for metallurgically bonding alloy wear plates or pads to superalloy articles, such as Z-notch contact surfaces of turbine blades. A composite preform, in some embodiments, comprises a powder alloy composition comprising 1-30 wt. % nickel, 0.05-2 wt. % iron, 15-25 wt. % chromium, 10-30 wt. % molybdenum, 0-1 wt. % carbon, 1-5 wt. % silicon, 0.05-2 wt. % boron, 0-5 wt. % tungsten, 0-3 wt. % tantalum, 0-0.1 wt. % manganese, 0-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance cobalt. The powder alloy compositions described herein can be associated with an organic carrier in some embodiments for application to one or more surfaces of a superalloy article.
In some embodiments, a composite preform comprises a powder alloy composition comprising 25-35 wt. % cobalt, 0.1-1 wt. % iron, 12-20 wt. % chromium, 10-20 wt. % molybdenum, 0-0.1 wt. % carbon, 0.5-3 wt. % silicon, 0.5-3 wt. % boron, 0-0.1 wt. % manganese, 0-0.1 wt. % tungsten, 0-2 wt. % tantalum, 0.5-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance nickel.
In another aspect, methods of imparting wear resistance to nickel-based superalloy articles are provided. In some embodiments, a method comprises providing a composite preform comprising a powder alloy composition of 1-30 wt. % nickel, 0.05-2 wt. % iron, 15-25 wt. % chromium, 10-30 wt. % molybdenum, 0-1 wt. % carbon, 1-5 wt. % silicon, 0.05-2 wt. % boron, 0-5 wt. % tungsten, 0-3 wt. % tantalum, 0-0.1 wt. % manganese, 0-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance cobalt and providing a wear plate or pad of cobalt-based alloy. The composite preform is positioned between the wear plate and surface of the nickel-based superalloy article to form an assembly. The assembly is heated to metallurgically bond the wear plate to the surface of the nickel-based superalloy article via a bonding alloy formed by the powder alloy composition. In some embodiments, the composite preform for bonding the wear plate comprises 25-35 wt. % cobalt, 0.1-1 wt. % iron, 12-20 wt. % chromium, 10-20 wt. % molybdenum, 0-0.1 wt. % carbon, 0.5-3 wt. % silicon, 0.5-3 wt. % boron, 0-0.1 wt. % manganese, 0-0.1 wt. % tungsten, 0-2 wt. % tantalum, 0.5-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance nickel.
These and other non-limiting embodiments are further described in the following detailed description.
Embodiments described herein can be understood more readily by reference to the following detailed description and examples and their previous and following descriptions. Elements, apparatus and methods described herein, however, are not limited to the specific embodiments presented in the detailed description and examples. It should be recognized that these embodiments are merely illustrative of the principles of the present invention. Numerous modifications and adaptations will be readily apparent to those of skill in the art without departing from the spirit and scope of the invention.
In one aspect, composite preforms are provided for imparting wear resistance to superalloy articles. The composite preforms can be employed for metallurgically bonding alloy wear plates or pads to superalloy articles. A composite preform can comprise a powder alloy composition comprising 1-30 wt. % nickel, 0.05-2 wt. % iron, 15-25 wt. % chromium, 10-30 wt. % molybdenum, 0-1 wt. % carbon, 1-5 wt. % silicon, 0.05-2 wt. % boron, 0-5 wt. % tungsten, 0-3 wt. % tantalum, 0-0.1 wt. % manganese, 0-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance cobalt. In some embodiments, cobalt-based powder alloy of a composite preform has composition selected from Table I.
In some embodiments, powder alloy of a composite preform has a composition selected from Table II.
Alternatively, a composite preform can comprise a powder alloy composition comprising 25-35 wt. % cobalt, 0.1-1 wt. % iron, 12-20 wt. % chromium, 10-20 wt. % molybdenum, 0-0.1 wt. % carbon, 0.5-3 wt. % silicon, 0.5-3 wt. % boron, 0-0.1 wt. % manganese, 0-0.1 wt. % tungsten, 0-2 wt. % tantalum, 0.5-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance nickel. In some embodiments, powder alloy of a composite preform has a composition selected from Table III.
Powder alloy compositions of composite preforms described herein, in some embodiment, are provided as a single, pre-alloyed powder. In other embodiments, powder alloy compositions can be formed of a mixture of two or more powder components. Two or more powder components can be combined or blended to form a powder alloy composition having any of the parameters described herein. For example, two or more powder components can be mixed to provide a powder alloy composition having parameters selected from Tables I-III herein. In some embodiments, a cobalt powder alloy component and a cobalt braze powder alloy component are combined or mixed in various proportions to provide a powder alloy composition of a composite preform. In some embodiments, the cobalt powder alloy component is a CoCrMoSi alloy or CoCrMoSiB alloy. In particular, the cobalt powder alloy component can have a composition selected from Table IV in some embodiments.
Moreover, the cobalt braze powder alloy component, in some embodiments, has a composition provided in Table V.
Cobalt powder alloy of Table IV and cobalt braze alloy of Table V can be mixed in various proportions to provide powder alloy compositions of composite preforms having parameters selected from Tables I and II herein. In some embodiments, for example, cobalt powder alloy component selected from Table IV is present in an amount of 10-90 weight percent of the powder alloy composition. Additionally, cobalt braze alloy component of Table V can be present in an amount of 30-70 weight percent of the powder alloy composition. In some embodiments, the ratio of cobalt alloy to cobalt braze alloy in a powder alloy composition ranges from 9:1 to 1:3 or from 9:1 to 1:1.
In some embodiments, the cobalt braze alloy component can be replaced by a nickel braze alloy component in preparation of a powder alloy composition of a composite preform. For example, a nickel braze powder alloy can be combined with cobalt powder alloy to provide a powder alloy composition of a composite preform having a composition selected from Table III herein. In some embodiments, a nickel braze alloy for combination with cobalt powder alloy has a composition provided in Table VI.
In some embodiments, nickel braze alloy is present in an amount of 30-70 weight percent of the powder alloy composition. The ratio of cobalt alloy to nickel braze alloy in a powder alloy composition can range from 9:1 to 1:3 or from 9:1 to 1:1.
Cobalt powder alloy, cobalt braze alloy and/or nickel braze alloy of the composite preform can have any desired particle size. Particle size can be selected according to various criteria including dispersability in an organic carrier and packing characteristics to provide composite preforms of desired density. In some embodiments, average particle size of one or more components of a powder alloy composition can range from 10 μm to 150 μm or from 40 μm to 125 μm.
The powder alloy composition can be associated with an organic carrier in some embodiments for application to one or more surfaces of a superalloy article. Any organic carrier not inconsistent with the objectives of the present invention can be employed. In some embodiment suitable organic carrier for the powder alloy composition comprises a fibrous polymeric matrix. As detailed further in the examples below, the fibrous polymeric matrix can form a flexible cloth in which the powder alloy composition is dispersed. The flexible polymeric cloth can have any thickness not inconsistent with the objectives of the present invention. For example, the flexible polymeric cloth can generally have a thickness of 0.2-4 mm or 1-2 mm. Any polymeric species operable to adopt a fiber or filament morphology can be used in matrix construction. Suitable polymeric species can include fluoropoymers, polyamides, polyesters, polyolefins or mixtures thereof. In some embodiments, for example, the fibrous polymeric matrix is formed of fibrillated polytetrafluoroethylene (PTFE). In such embodiments, the PTFE fibers or fibrils can provide an interconnecting network matrix in which the powder alloy composition is dispersed and trapped. Moreover, fibrillated PTFE can be combined with other polymeric fibers, such as polyamides and polyesters to modify or tailor properties of the fibrous matrix. The fibrous polymeric matrix generally accounts for less than 1.5 weight percent of the composite preform. In some embodiments, for example, the fibrous polymeric matrix accounts for 1.0-1.5 weight percent or 0.5-1.0 weight percent of the composite preform.
The composite preform can be fabricated by various techniques to disperse the powder alloy composition in the fibrous polymeric matrix. In some embodiments, the composite preform is fabricated by combining polymeric powder, cobalt alloy powder, cobalt braze alloy powder and/or nickel braze alloy powder and mechanically working the mixture to fibrillate the polymeric powder and trap the alloy powders in the resulting fibrous polymeric matrix. In a specific embodiment, for example, components of the powder alloy composition are mixed with 3-15 vol. % of PTFE powder and mechanically worked to fibrillate the PTFE and trap the powder alloy composition in a fibrous PTFE matrix. As described herein, components of the powder alloy composition can be selected from Tables IV-VI above. Mechanical working of the powder mixture can include ball milling, rolling, stretching, elongating, extruding, spreading or combinations thereof. In some embodiments, the resulting PTFE-flexible composite preform cloth is subjected to cold isostatic pressing. A composite preform described herein can be produced in accordance with the disclosure of one or more of U.S. Pat. Nos. 3,743,556, 3,864,124, 3,916,506, 4,194,040 and 5,352,526, each of which is incorporated herein by reference in its entirety.
As detailed in the examples below, a composite preform formed by a polymeric carrier having the powder alloy composition positioned therein, in some embodiments, can exhibit green density of at least 50 percent the density of a wear pad bonded to the superalloy article. In some embodiments, green density of a composite preform can be at least 60 percent or at least 65 percent the density of the wear pad. Green density of the composite preform can also be 50-75 percent or 60-70 percent of wear pad density. High green density of the composite preform can assist in forming a strong metallurgical bond between the wear pad and superalloy article. High green density can also assist in reducing or eliminating porosity in the bonding alloy formed by heating the composite preform according to methods described herein.
Alternatively, the powder alloy composition can be associated with a liquid carrier for application to one or more surfaces of a superalloy article. Aqueous and/or organic liquid carriers may be employed depending on specific powder alloy composition and properties.
In another aspect, methods of imparting wear resistance to a nickel-based superalloy article are provided. In some embodiments, a method comprises providing a composite preform comprising a powder alloy composition 1-30 wt. % nickel, 0.05-2 wt. % iron, 15-25 wt. % chromium, 10-30 wt. % molybdenum, 0-1 wt. % carbon, 1-5 wt. % silicon, 0.05-2 wt. % boron, 0-5 wt. % tungsten, 0-3 wt. % tantalum, 0-0.1 wt % manganese, 0-3 wt. % aluminum, 0-0.1 wt % yttrium and the balance cobalt and providing a wear plate or pad of cobalt-based alloy. The composite preform is positioned between the wear plate and surface of the nickel-based alloy article to form an assembly. The assembly is heated to metallurgically bond the wear plate to the surface of the nickel-based superalloy article via a bonding alloy formed by the powder alloy composition. In some embodiments, the powder alloy composition of the composite preform has parameters selected from Tables I and II herein. Alternatively, the powder alloy composition of the composite preform can comprise 25-35 wt. % cobalt, 0.1-1 wt. % iron, 12-20 wt. % chromium, 10-20 wt. % molybdenum, 0-0.1 wt. % carbon, 0.5-3 wt. % silicon, 0.5-3 wt. % boron, 0-0.1 wt % manganese, 0-0.1 wt. % tungsten, 0-2 wt. % tantalum, 0.5-3 wt. % aluminum, 0-0.1 wt. % yttrium and the balance nickel. For example, the powder alloy composition can have parameters selected from Table III herein.
Composite preforms can have any properties and construction described in Section I above. In some embodiments, the composite preform comprises a polymeric carrier for the powder alloy composition. The flexible, cloth like nature of the polymeric matrix can facilitate application of the composite preform to surfaces of varying geometry and/or curvature of the nickel-based superalloy article. Moreover, the composite preforms can exhibit high green densities described above. Composite preforms can be used to bond one or more wear pads to any contact or wear surface of the nickel-based superalloy article. Wear surface design and geometry can be derived by the function of the nickel-based superalloy article. In some embodiments, the nickel-based superalloy article can comprise turbine blades wherein wear pads are bonded to contact surfaces of the Z-notches. In some embodiments, a single composite preform is applied between the wear plate and surface of the nickel-based superalloy article. Alternatively, multiple composite preforms can be applied between the wear pad and surface of the nickel-based superalloy part. For example, composite preforms can be applied in a layered format between the wear pad and superalloy surface. Layering the composite preforms can enable production of bonding alloy of any desired thickness. The surface of the nickel-based superalloy article may be cleaned by chemical and/or mechanical means prior to composite preform application, such as by fluoride ion cleaning.
An assembly is formed by application of one or more composite preforms between the wear pad and surface of the nickel-based superalloy article. The assembly is heated to metallurgically bond the wear plate to the surface of the nickel-based superalloy article via a bonding alloy formed by the powder alloy composition. Heating the assembly decomposes the polymeric fibrous matrix, and the bonding alloy is formed from the powder alloy composition of the composite preform. As described herein, the powder alloy composition can be formed of multiple powder components including cobalt powder alloy in combination with cobalt braze alloy or nickel braze alloy. The assembly is generally heated to a temperature in excess of the melting point of the cobalt braze powder alloy component or nickel braze powder alloy component and below the melting point of the cobalt powder alloy component. Molten flow characteristics of the cobalt braze alloy or nickel braze alloy can permit formation of a void-free or substantially void-free interface between the wear plate and the nickel-based superalloy article. Heating temperature and heating time period are dependent on the specific compositional parameters of the nickel-based superalloy part and composite preform. In some embodiments, for example, the assembly is heated under vacuum to a temperature of 1200-1230° C. for a time period of 5-30 minutes. In some embodiments, heating is continued at 1100-1150° C. for 1 to 4 hours.
Cobalt-based alloy of the wear plate can have any composition not inconsistent with the objectives of the present invention. In some embodiments, the cobalt-based alloy forming the wear plate is a CoCrMoSi alloy. Cobalt-based alloy of the wear pad, for example, can have composition selected from Table VII.
In some embodiments, cobalt-based alloy of the wear pad has a composition selected from Table VIII.
In some embodiments, the wear pad is formed of cobalt-based alloy operable to withstand deformation at temperatures in excess of 1200° C. or 1220° C. The cobalt-based alloy wear pad, for example, can withstand deformation or softening at temperatures in excess of 1200° C. or 1220° C. for time periods exceeding 2 hours or more. High temperature stability of the wear pad can enable the wear pad to avoid degradation during turbine blade repair processes including hot isostatic pressing and rejuvenation steps at temperatures in excess of 1200° C. while maintaining strong metallurgical bonding with the nickel-based superalloy article.
In a further aspect, composite preforms of Section I herein can be applied to surfaces of the wear pad after the wear pad has been metallurgically bonded to the nickel-based superalloy article. The composite preform is subsequently heated to form an alloy wear layer on the wear pad. In this way, the wear properties of the wear pad can be enhanced and/or restored. For example, the wear pad may become worn after use of the nickel-based superalloy article in its operating environment. The wear pad may be restored by application of one or more composite preforms herein followed by heating to form an alloy wear layer. The alloy wear layer may replace material of the wear pad that was lost or degraded during use of the nickel-based superalloy article. Composite preforms of any composition and/or properties can be applied to surfaces of cobalt-based alloy wear pads for restoration and/or enhancement of wear properties.
As described herein, the powder alloy composition can be formed of separate powder components including a combination or mixture of cobalt powder alloy with cobalt braze alloy or nickel braze alloy. In some embodiments, individual components of the powder alloy composition can be associated with separate carriers. For example, cobalt powder alloy can be positioned in a first organic carrier, and the cobalt braze powder alloy or nickel braze powder alloy can be positioned in a second organic carrier. In some embodiments, the first organic carrier is a first polymeric sheet, and the second organic carrier is a second polymeric sheet. The first and second sheets are layered to provide the composite preform. The layered composite preform is positioned between the wear pad and surface of the nickel-based superalloy part to form the assembly. The assembly is heated to metallurgically bond the wear plate to the surface of the nickel-based superalloy article via a bonding alloy formed by the powder alloy composition.
In further aspects, the powder alloy composition can be provided in a liquid carrier for application to one or more surfaces of the nickel-based superalloy. In some embodiments, all components of the powder alloy composition are in a single liquid carrier. For example, the cobalt alloy powder component can be added to a liquid carrier with the cobalt braze powder component or nickel braze powder component. In other embodiments, individual powder components of the powder alloy composition can be added to separate liquid carriers and applied to one or more surfaces of the nickel-based superalloy.
These and other embodiments are further illustrated in the following non-limiting examples.
Cobalt-based alloy wear pads were provided and metallurgically bonded to contact surfaces of Z-notches of turbine blades as follows. The Z-notch contact surfaces and associated turbine blades were formed of nickel-based superalloy of composition substantially similar to Rene 80. Composite preforms were formed by providing a powder alloy of Composition 2 selected from Table I above. The powder alloy composition was a mixture of 65 weight percent cobalt powder alloy and 35 weight percent cobalt braze powder alloy. The cobalt powder alloy was a CoCrMoSi alloy having nominal composition of 0.5-2 wt. % iron, 16-19 wt. % chromium, 28-30 wt % molybdenum, 0.01-0.1 wt % carbon, 3-4 wt. % silicon, 0-0.2 wt. % boron, 0-0.1 wt % manganese and the balance Co. The cobalt braze powder alloy had nominal composition of 9-11 wt. % nickel, 24-26 wt. % chromium, 0.5-1 wt % carbon, 2-3 wt. % boron, 6-8 wt. % tungsten, 3-4 wt % tantalum and the balance cobalt. The powder alloy composition was mixed with 5-15 vol. % of powder PTFE. The mixture was mechanically worked to fibrillate the PTFE and trap powder alloy composition and then rolled, thus forming the composite preform as a cloth-like flexible sheet of thickness 1-2 mm.
A composite preform 11 was positioned between each Z-notch contact surface 10 and the wear pad 12 as illustrated in
The assemblies were heated under vacuum at 1200-1220° C. for 5-20 minutes followed by a hold at 1100-1150° C. for 1-3 hours. The heat treatment metallurgically bonded the cobalt alloy wear pads to the Z-notch contact surfaces via bonding alloy formed by the powder alloy composition.
The wear pads and associated Z-notch contact surfaces were subjected to superalloy ageing and rejuvenation at 1200-1210° C. for a time period of 4 hours.
Various embodiments of the invention have been described in fulfillment of the various objects of the invention. It should be recognized that these embodiments are merely illustrative of the principles of the present invention. Numerous modifications and adaptations thereof will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention.