Method of forming polycrystalline silicon layer and atomic layer deposition apparatus used for the same

Information

  • Patent Grant
  • 8048783
  • Patent Number
    8,048,783
  • Date Filed
    Friday, February 26, 2010
    15 years ago
  • Date Issued
    Tuesday, November 1, 2011
    13 years ago
Abstract
A method of forming a polycrystalline silicon layer and an atomic layer deposition apparatus used for the same. The method includes forming an amorphous silicon layer on a substrate, exposing the substrate having the amorphous silicon layer to a hydrophilic or hydrophobic gas atmosphere, placing a mask having at least one open and at least one closed portion over the amorphous silicon layer, irradiating UV light toward the amorphous silicon layer and the mask using a UV lamp, depositing a crystallization-inducing metal on the amorphous silicon layer, and annealing the substrate to crystallize the amorphous silicon layer into a polycrystalline silicon layer. This method and apparatus provide for controlling the seed position and grain size in the formation of a polycrystalline silicon layer.
Description
CROSS-REFERENCE TO RELATED APPLICATION

This application claims the benefit of Korean Patent Application No. 10-2009-0018927, filed Mar. 5, 2009 in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference.


BACKGROUND OF THE INVENTION

1. Field of the Invention


Aspects of the present invention relate to a method of forming a polycrystalline silicon layer and an atomic layer deposition apparatus used for the same, and more particularly, to a method of forming a polycrystalline silicon layer and an atomic layer deposition apparatus in which a crystallization-inducing metal may be deposited on an amorphous silicon layer at a predetermined position and a uniform concentration by modifying a predetermined region of a surface of the amorphous silicon layer into a hydrophilic surface or a hydrophobic surface. Thus, seed position and grain size may be controlled.


2. Description of the Related Art


Generally, polycrystalline silicon layers are widely used as semiconductor layers for thin film transistors since the polycrystalline silicon layers have high field effect mobility, and enable application to high-speed operating circuits and formation of CMOS circuits. Thin film transistors using the polycrystalline silicon layers are mainly used for active devices of active-matrix liquid crystal display (AMLCD) devices, and switching and driving devices of organic light emitting diode (OLED) display devices.


Examples of methods of crystallizing amorphous silicon into polycrystalline silicon include solid phase crystallization (SPC), excimer laser crystallization (ELC), metal-induced crystallization (MIC) and metal-induced lateral crystallization (MILC) methods. In the SPC method, an amorphous silicon layer is annealed for several to several tens of hours at a temperature of about 700° C. or less, which is the thermal deformation temperature of glass forming a substrate of a display device using a thin film transistor. In the ELC method, an excimer laser is applied to an amorphous silicon layer to locally heat the amorphous silicon layer for a very short period of time at high temperature. In the MIC method, a crystallization-inducing metal such as nickel, palladium, gold or aluminum is in contact with or injected into an amorphous silicon layer to induce a phase change into a polycrystalline silicon layer, and in the MILC method, a silicide produced by reacting a crystallization-inducing metal with silicon then laterally propagates, sequentially inducing crystallization of the amorphous silicon layer. However, the SPC method requires a long processing time, and easily causes deformation of a substrate due to long annealing at high temperature, and the ELC method requires high-priced laser equipment and has poor interface characteristics between the polycrystallized silicon semiconductor layer and a gate insulating layer due to protrusions occurring on the polycrystallized surface.


Today, research into methods of crystallizing an amorphous silicon layer using a crystallization-inducing metal has been widely conducted because of faster crystallization at a lower temperature than the SPC method. Examples of these crystallization methods using a crystallization-inducing metal include MIC, MILC, and super grain silicon (SGS) crystallization methods.


In the crystallization methods using a crystallization-inducing metal, the crystallization-inducing metal is deposited on an amorphous silicon layer by sputtering, ion implantation or thermal evaporation. However, in these methods, metal particles to be deposited randomly propagate from a metal target, and thus there is a limit in being able to uniformly deposit a metal catalyst to have a concentration as high as 1011 to 1016 atoms/cm2. Recently, while a technique of uniformly depositing crystallization-inducing metals on an amorphous silicon layer using micro-electro-mechanical systems (MEMS) technology has been disclosed, this has disadvantages of length of preparation time in mass-production, which may not be suitable for commercialization.


SUMMARY OF THE INVENTION

Aspects of the present invention provide a method of forming a polycrystalline silicon layer and an atomic layer deposition apparatus used for the same, in which a crystallization-inducing metal is deposited on an amorphous silicon layer at a predetermined position and a uniform concentration, and thus the seed position and the grain size may be controlled.


According to an embodiment of the present invention, a method of forming a polycrystalline silicon layer includes: forming an amorphous silicon layer on a substrate; exposing the substrate having the amorphous silicon layer to a hydrophilic or hydrophobic gas atmosphere; placing a mask having an open and a closed portion on the amorphous silicon layer; irradiating UV light through the mask to the amorphous silicon layer using a UV lamp; depositing a crystallization-inducing metal on the amorphous silicon layer; and annealing the substrate to crystallize the amorphous silicon layer into a polycrystalline silicon layer. Hereafter, an open portion can be at least one open portion and a closed portion can be at least one closed portion.


According to another embodiment of the present invention, an atomic layer deposition apparatus includes: a chamber; a chuck disposed in the chamber; a mask disposed over the chuck and having an open and a closed portion; a UV lamp disposed on the mask; and a gas inlet disposed at a side of the chamber. Hereafter, a gas inlet can be at least one gas inlet and a side of the chamber can be at least one side of the chamber. Moreover, when a first element is said to be “disposed” on a second element, the first element can directly contact the second element, or can be separated from the second element by one or more other elements that can be located therebetween.


Additional aspects and/or advantages of the invention will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the invention.





BRIEF DESCRIPTION OF THE DRAWINGS

These and/or other aspects and advantages of the invention will become apparent and more readily appreciated from the following description of the embodiments, taken in conjunction with the accompanying drawings of which:



FIGS. 1A to 1D are cross-sectional views illustrating a method of forming a polycrystalline silicon layer according to an exemplary embodiment of the present invention;



FIG. 2 is a cross-sectional view of an atomic layer deposition apparatus for the method of forming a polycrystalline silicon layer according to another exemplary embodiment of the present invention; and



FIG. 3 is a cross-sectional view illustrating a method of forming a polycrystalline silicon layer using the atomic layer deposition apparatus of FIG. 2.





DETAILED DESCRIPTION OF THE EMBODIMENTS

Reference will now be made in detail to the present embodiments of the present invention, examples of which are illustrated in the accompanying drawings, wherein like reference numerals refer to the like elements throughout. The embodiments are described below in order to explain the present invention by referring to the figures.



FIGS. 1A to 1D are cross-sectional views illustrating a method of forming a polycrystalline silicon layer according to an exemplary embodiment of the present invention. Referring to FIG. 1A, a substrate 100 formed of glass or plastic is prepared. A buffer layer 110 may be formed on the substrate 100. The buffer layer 110 is formed of a single insulating layer including silicon dioxide or silicon nitride, or a multilayer thereof, by chemical vapor deposition (CVD) or physical vapor deposition (PVD). Here, the buffer layer 110 may prevent diffusion of moisture or impurities generated from the substrate 100, or control the heat transfer rate during crystallization to facilitate the crystallization of an amorphous silicon layer.


Subsequently, an amorphous silicon layer 120 is formed on the buffer layer 110. The amorphous silicon layer 120 is formed by CVD or PVD. During or after the formation of the amorphous silicon layer 120, a process for reducing the hydrogen concentration by dehydrogenation may be performed.


The substrate 100 having the amorphous silicon layer 120 is exposed to a hydrophilic or hydrophobic gas atmosphere. Referring to FIG. 1B, a mask 130 having an open portion 130a and a closed portion 130b is disposed on the amorphous silicon layer 120, and a UV lamp 140 is disposed above the mask 130. UV light is irradiated onto the amorphous silicon layer 120 through the open portion 130a of the mask 130 using the UV lamp. When UV light is irradiated from the UV lamp, a corresponding predetermined region 150 on the surface of the amorphous silicon layer 120, upon which UV light is irradiated from the UV lamp, is modified into a hydrophilic or hydrophobic surface. Hereafter, an open portion can be at least one open portion and a closed portion can be at least one closed portion. Moreover, when a first element is said to be “disposed” on a second element, the first element can directly contact the second element, or can be separated from the second element by one or more other elements that can be located therebetween.


When the substrate 100 is exposed to a hydrophilic gas atmosphere, an open portion 130a of the mask corresponds to a region that the crystallization-inducing metal will be deposited on the amorphous silicon layer 120. When the substrate 100 is exposed to a hydrophobic gas atmosphere, a closed portion 130b of the mask corresponds to a region that the crystallization-inducing metal will be deposited on the amorphous silicon layer 120. The distance between the mask 130 and the UV lamp 120 may be within the range of distances over which the wavelength of the UV lamp can maintain linearity such that regions irradiated by UV light correspond to an open portion 130a of the mask. The distance may be changed according to the processing pressure, the wavelength of the UV lamp and the kind of the gas.


The hydrophilic gas may include O2, N2O or H2O, and the hydrophobic gas may include one or more of the series of gases CxFy (where x and y are natural numbers). The wavelength of the UV lamp 120 may be a short wavelength (that is, Ultraviolet C or UVC). For efficiency, a vacuum UV lamp (VUV lamp) and an extreme UV lamp (EUV lamp) may be used. The VUV lamp is preferable.


Then, a crystallization-inducing metal 160 is deposited on the amorphous silicon layer 120. Referring to FIG. 1C, the crystallization-inducing metal 160 is preferentially deposited on a predetermined region 150a of the amorphous silicon layer 120 modified into a hydrophilic surface. The crystallization-inducing metal 160 is not deposited on a predetermined region 150b of the surface of the amorphous silicon layer that is not modified into a hydrophilic surface. Conversely, referring to FIG. 1D, the crystallization-inducing metal 160 is not deposited on a predetermined region 150c of the surface of the amorphous silicon layer 120 that is modified into a hydrophobic surface, and preferentially deposited on a predetermined region 150d of the surface of the amorphous silicon layer that is not modified into a hydrophobic surface. Thus, the crystallization-inducing metal 160 may be disposed only on predetermined regions of the amorphous silicon layer 120, so that regions in which a crystallization seed will be formed may be controlled, and thereby the grain size may also be controlled.


The crystallization-inducing metal 160 may be one selected from the group consisting of nickel (Ni), palladium (Pd), titanium (Ti), silver (Ag), gold (Au), aluminum (Al), tin (Sn), antimony (Sb), copper (Cu), cobalt (Co), molybdenum (Mo), terbium (Tb), rubidium (Ru), rhodium (Rh), cadmium (Cd) and platinum (Pt), and preferably Ni. The crystallization-inducing metal may be deposited to have an areal density of 1011 to 1015 atoms/cm2. When the crystallization-inducing metal is deposited to have a density in the predetermined regions of less than 1011 atoms/cm2, the amount of seeds, which are crystallization nuclei, may be too small so that it is difficult to crystallize the amorphous silicon layer into a polycrystalline silicon layer. When the crystallization-inducing metal is deposited to have a density in the predetermined regions of more than 1015 atoms/cm2, the amount of the crystallization-inducing metals diffused to the amorphous silicon layer is large, so that leakage current characteristics of the semiconductor layer formed by patterning the polycrystalline silicon layer may be poor. The crystallization-inducing metal layer 160 may be deposited by CVD such as atomic layer deposition to ensure a uniform thickness and a low concentration.


Subsequently, the substrate 100 having the amorphous silicon layer 120 on which the crystallization-inducing metal 160 is deposited is annealed, thereby crystallizing the amorphous silicon layer 120 into a polycrystalline silicon layer. During annealing, the surface of the amorphous silicon layer 120 is modified into a hydrophilic surface or not modified into a hydrophobic surface, and thereby seeds are formed from the regions 150a and 150c on which the crystallization-inducing metals 160 are deposited, and grains are laterally grown about the regions. Thus, the position of an open portion 130a of the mask 130 controls the a region in which the seeds are formed, and thereby the size of the crystal grains may be controlled.


The annealing process may be one of a furnace process, a rapid thermal annealing (RTA) process, a UV process and a laser process, and may be performed in the range from 200 to 900° C. for several seconds to hours. Over those temperatures and times, deformation of the substrate due to excessive annealing may be prevented, improved yield may be obtained, and production costs may be reduced.


In another embodiment of the present invention, the crystallization-inducing metal 160 may be deposited by atomic layer deposition. An atomic layer deposition apparatus used herein and a method of depositing a crystallization-inducing metal on an amorphous silicon layer using the same will be described. Except for additional descriptions below, these will be explained with reference to the descriptions of the previous exemplary embodiment.



FIG. 2 is a cross-sectional view of an atomic layer deposition apparatus to be used for the method of forming a polycrystalline silicon layer according to an exemplary embodiment of the present invention. FIG. 3 is a cross-sectional view illustrating a method of forming a polycrystalline silicon layer using the atomic layer deposition apparatus of FIG. 2.


Referring to FIG. 2, the atomic layer deposition apparatus according to the exemplary embodiment of the present invention includes a chamber 200 having an internal space in which a deposition process is performed. A chuck 210 is disposed to load a substrate in the chamber 200. A UV lamp 220 is disposed on the chuck 210. A mask 230 having an open portion 230a and a closed portion 230b is disposed between the UV lamp 220 and the chuck 210. The wavelength of the UV lamp 220 may be a short wavelength (that is, Ultraviolet C or UVC). For efficiency, a VUV lamp or a EUV lamp may be used, and a VUV lamp is preferable.


At one side of the chamber 200, a gas inlet 240 is disposed to supply a gas to be used in the process. A plurality of gas inlets 240 may be disposed in the chamber 200 and may be disposed on one or more sides of the chamber 200. In addition, an exhaustion hole 250 for exhausting the used gases or residual products may be disposed under the chuck 210. A plurality of exhaustion holes 250 may also be disposed in the chamber 200.


Referring to FIG. 3, as shown in FIG. 1A, the substrate 100 having the amorphous silicon layer 120 is loaded on the chuck 210 in the chamber 200. Subsequently, UV light is irradiated from the UV lamp 220, and a hydrophilic or hydrophobic gas is provided from a gas inlet 240.


When a hydrophilic gas is provided, an open portion 230a of the mask 230 corresponds to a region where the crystallization-inducing metal will be deposited on the amorphous silicon layer 120. When a hydrophobic gas is provided, a closed portion 230b of the mask 230 corresponds to a region that the crystallization-inducing metal will be deposited on the amorphous silicon layer 120. The distance between the mask 230 and the UV lamp 220 may be within the range of distances over which the wavelength of the UV lamp may maintain linearity such that a region on which UV light is irradiated from the UV lamp corresponds to an open portion 230a of the mask 230. The distance may be changed depending on the processing pressure, the wavelength of the UV lamp and the kind of the gas. The hydrophilic gas may include O2, N2O or H2O, and the hydrophobic gas may include one or more of the series of gases, CxFy (where x and y are natural numbers).


As shown in FIG. 1C, a crystallization-inducing metal 160 is deposited on the amorphous silicon layer 120 by supplying a crystallization-inducing metal precursor through a gas inlet 240. During supply of the crystallization-inducing metal precursor, the crystallization-inducing metal 160 is preferentially deposited on a predetermined region 150a of the amorphous silicon layer 120 that is modified into a hydrophilic surface. The crystallization-inducing metal 160 is not deposited on a predetermined region 150b of the surface of the amorphous silicon layer 120 that is not modified into a hydrophilic surface. Conversely, referring to FIG. 1D, the crystallization-inducing metal 160 is not deposited on a predetermined region 150c of the surface of the amorphous silicon layer 120 that is modified into a hydrophobic surface, and preferentially deposited on a predetermined region 150d of the surface of the amorphous silicon layer 120 that is not modified into a hydrophobic surface. Thus, the crystallization-inducing metal 160 may be disposed only on predetermined regions 150a and 150d of the amorphous silicon layer 120, so that regions in which crystallization seeds will be formed may be controlled, and thereby the grain size may also be controlled.


The crystallization-inducing metal 160 may be one selected from the group consisting of Ni, Pd, Ti, Ag, Au, Al, Sn, Sb, Cu, Co, Mo, Tb, Ru, Rh, Cd and Pt, and preferably Ni. The crystallization-inducing metal layer may be deposited to have an areal density of 1011 to 1015 atoms/cm2. When the crystallization-inducing metal is deposited to have an areal density less than 1011 atoms/cm2, an amount of seeds, which are crystallization nuclei, may be too small so that it is difficult to crystallize the amorphous silicon layer 120 into a polycrystalline silicon layer, and when the crystallization-inducing metal 160 is deposited to have an areal density more than 1015 atoms/cm2, an amount of the crystallization-inducing metals diffused to the amorphous silicon layer 120 is large so that leakage current characteristics of the semiconductor layer formed by patterning the polycrystalline silicon layer may be poor.


The substrate 100 is unloaded from the atomic layer deposition apparatus, and the substrate 100 having the amorphous silicon layer 120 on which crystallization-inducing metals are deposited is annealed, and thereby the amorphous silicon layer 120 is crystallized into a polycrystalline silicon layer.


Thus, a crystallization-inducing metal can be deposited at predetermined positions on an amorphous silicon layer by modifying predetermined regions of a surface of the amorphous silicon layer into a hydrophilic or hydrophobic surface, and the crystallization-inducing metal can be deposited using an atomic layer deposition apparatus to have a uniform concentration, thereby controlling the seed position and the grain size to form a polycrystalline silicon layer. In addition, a thin film transistor can be formed using the polycrystalline silicon layer, so that the characteristic distribution of the thin film transistor, which occurs due to the non-uniform size of the grain, can be minimized.


Although a few embodiments of the present invention have been shown and described, it would be appreciated by those skilled in the art that changes may be made in this embodiment without departing from the principles and spirit of the invention, the scope of which is defined in the claims and their equivalents.

Claims
  • 1. A method of forming a polycrystalline silicon layer, comprising: forming an amorphous silicon layer on a substrate;exposing the substrate having the amorphous silicon layer to a hydrophilic gas atmosphere;placing a mask having an open and a closed portion over the amorphous silicon layer;irradiating UV light at the amorphous silicon layer through the open portion of the mask using a UV lamp;depositing a crystallization-inducing metal on the amorphous silicon layer; andannealing the substrate to crystallize the amorphous silicon layer into a polycrystalline silicon layer.
  • 2. The method according to claim 1, wherein the open portion of the mask corresponds to a region in which the crystallization-inducing metal will be deposited on the amorphous silicon layer.
  • 3. The method according to claim 1, wherein the crystallization-inducing metal is deposited only on a region of the amorphous silicon layer at which UV light is irradiated from the UV lamp through an open portion of the mask.
  • 4. The method according to claim 1, wherein the hydrophilic gas is O2, N2O or H2O.
  • 5. The method according to claim 1, wherein the crystallization-inducing metal is deposited by atomic layer deposition.
  • 6. The method according to claim 1, wherein the distance between the mask and the UV lamp is within the range of distances over which the wavelength of the UV lamp maintains linearity.
  • 7. The method of claim 1, wherein a buffer layer is disposed between the substrate and the amorphous silicon layer.
  • 8. The method of claim 7, wherein the buffer layer is silicon dioxide or a multilayer thereof.
  • 9. The method of claim 7, wherein the buffer layer is formed by chemical vapor deposition (CVD) or physical vapor deposition (PVD).
  • 10. The method of claim 1, wherein an open portion is at least one open portion and a closed portion is at least one closed portion.
  • 11. The method of claim 1, wherein the UV lamp is a short wave lamp (Ultraviolet C or UVC).
  • 12. The method of claim 11, wherein the UV lamp is a vacuum UV lamp (VUV) or an extreme UV lamp (EUV).
  • 13. The method of claim 12, wherein the UV lamp is a vacuum UV lamp (VUV).
  • 14. The method of claim 1, wherein the crystallization-inducing metal is one selected from the group consisting of nickel (Ni), palladium (Pd), titanium (Ti), silver (Ag), gold (Au), aluminum (Al), tin (Sn), antimony (Sb), copper (Cu), cobalt (Co), molybdenum (Mo), terbium (Tb), rubidium (Ru), rhodium (Rh), cadmium (Cd) and platinum (Pt).
  • 15. The method of claim 14, wherein the crystallization-inducing metal is nickel (Ni).
  • 16. The method of claim 1, wherein the crystallization-inducing metal is deposited at an areal density of 1011 through 1015 atoms/cm2.
  • 17. The method of claim 1, wherein the annealing process is performed by a furnace process, rapid thermal annealing (RTA), UV, or a laser.
  • 18. The method of claim 1, wherein the annealing is performed in the range from 200 to 900° C.
  • 19. A method of making a thin film transistor comprising a polycrystalline silicon layer, the method comprising: forming an amorphous silicon layer on a substrate;exposing the substrate having the amorphous silicon layer to a hydrophilic gas atmosphere;placing a mask having an open and a closed portion over the amorphous silicon layer;irradiating UV light at the amorphous silicon layer through an open portion of the mask using a UV lamp;depositing a crystallization-inducing metal on the amorphous silicon layer; andannealing the substrate to crystallize the amorphous silicon layer into a polycrystalline silicon layer.
Priority Claims (1)
Number Date Country Kind
10-2009-0018927 Mar 2009 KR national
US Referenced Citations (16)
Number Name Date Kind
5814540 Takemura et al. Sep 1998 A
6294815 Yamazaki et al. Sep 2001 B1
6806099 Takeda et al. Oct 2004 B2
7341907 Li et al. Mar 2008 B2
7615421 Lee et al. Nov 2009 B2
7618852 Jang et al. Nov 2009 B2
20020063261 Zhang May 2002 A1
20040173796 Miyasaka Sep 2004 A1
20050023531 Shoji et al. Feb 2005 A1
20050161742 Isobe et al. Jul 2005 A1
20050184290 Ohnuma Aug 2005 A1
20050275019 Seo et al. Dec 2005 A1
20060121651 Park et al. Jun 2006 A1
20060130939 Jang et al. Jun 2006 A1
20080157083 Park et al. Jul 2008 A1
20090239352 Kitagawa et al. Sep 2009 A1
Foreign Referenced Citations (31)
Number Date Country
1779985 May 2006 CN
1903604 Mar 2008 EP
2226833 Sep 2010 EP
05-173177 Jul 1993 JP
06-067203 Mar 1994 JP
07-013196 Jan 1995 JP
08-045850 Feb 1996 JP
2001-189275 Jul 2001 JP
2001-337348 Dec 2001 JP
2003-100629 Apr 2003 JP
10-1992-0006076 Jul 1992 KR
10-1997-0072491 Jul 1997 KR
10-2000-0055877 Sep 2000 KR
10-0285865 Mar 2001 KR
10-0317638 Dec 2001 KR
10-2002-0021546 Mar 2002 KR
10-2003-0028696 Apr 2003 KR
10-2004-0036761 May 2004 KR
10-2004-0040762 May 2004 KR
10-2004-0098958 Nov 2004 KR
10-0470274 Feb 2005 KR
10-2006-0018533 Mar 2006 KR
1020060058934 Jun 2006 KR
10-0623228 Sep 2006 KR
10-0628989 Sep 2006 KR
10-0772347 Oct 2007 KR
10-2007-0107142 Nov 2007 KR
10-2007-0107168 Nov 2007 KR
10-0778781 Nov 2007 KR
10-0839735 Jun 2008 KR
10-2008-0086967 Sep 2008 KR
Related Publications (1)
Number Date Country
20100227458 A1 Sep 2010 US