The present invention relates to a Ni-based single crystal superalloy and a turbine blade.
Turbine blades (stator blades and rotor blades) used in aircraft engines, industrial gas turbines and other systems are often operated in high-temperature environments for a prolonged time and thus are made of a Ni-based single crystal superalloy that has an excellent heat resistance. The Ni-based single crystal superalloy is produced in the following manner. Al is first added to base Ni to cause Ni3Al to precipitate for precipitation strengthening. High melting point metals, such as Cr, W and Ta, are then added to form an alloy which is formed as a single crystal.
There is known, as such a Ni-based single crystal superalloy, for example, a second generation alloy or the like (for example, CMSX-4 manufactured by Cannon-Muskegon Corporation, PWA1484 manufactured by United Technologies Corporation) in which high-temperature strength, mainly creep strength (also including high-temperature fatigue strength) is enhanced by inclusion of a first generation alloy containing no Re (for example, CMSX-2 manufactured by Cannon-Muskegon Corporation, PWA1480 manufactured by United Technologies Corporation) and 3 wt % of Re. CMSX and PWA are trademarks of alloys.
[Patent Document 1]
U.S. Pat. No. 4,582,548
[Patent Document 2]
U.S. Pat. No. 4,643,782
[Patent Document 3]
Japanese Unexamined Patent Application, First Publication No. Sho 53-146223
The second generation Ni-based single crystal superalloy is a Ni-based single crystal superalloy in which high-temperature strength, mainly creep strength is enhanced, as compared to the first generation Ni-based single crystal superalloy, by inclusion of Re. Namely, it is known that high-temperature strength, mainly creep strength of the Ni-based single crystal superalloy can be enhanced by inclusion of Re.
However, since Re is rare metal, it is difficult to stably ensure supply of a large amount of Re. The price of Re has recently risen and use of a large amount of Re causes a rise in prices of products.
Therefore, it is desired to develop a Ni-based single crystal superalloy having high-temperature strength, mainly creep strength, which is at least higher than that of the first generation Ni-based single crystal superalloy, and desirably high-temperature strength, mainly creep strength, which is equal to or higher than that of the second generation Ni-based single crystal superalloy, while decreasing the amount of Re as compared to the second generation Ni-based single crystal superalloy.
In light of the problems described above, the present invention has been made and an object thereof is to provide a Ni-based single crystal superalloy which has a low amount of Re and is also excellent in high-temperature strength, mainly creep strength.
The present invention employs, as means for solving the problems described above, the following constitutions.
A first invention is a Ni-based single crystal superalloy which has the following composition by weight: 0.1 wt % or more and 9.9 wt % or less of Co, 5.1 wt % or more and 10.0 wt % or less of Cr, 1.0 wt % or more and 4.0 wt % or less of Mo, 8.1 wt % or more and 11.0 wt % or less of W, 4.0 wt % or more and 9.0 wt % or less of Ta, 5.2 wt % or more and 7.0 wt % or less of Al, 0.1 wt % or more and 2.0 wt % or less of Ti, 0.05 wt % or more and 0.3 wt % or less of Hf, 1.0 wt % or less of Nb and less than 3.0 wt % of Re with the remainder including Ni and unavoidable impurities.
A second invention is a Ni-based single crystal superalloy according to the above first invention, wherein the amount of Re is 2.0 wt % or less by weight.
A third invention is a Ni-based single crystal superalloy according to the above first invention, wherein the amount of Re is 1.4 wt % or less by weight.
A fourth invention is a Ni-based single crystal superalloy according to the above first invention, wherein the amount of Re is 0.8 wt % or less by weight.
A fifth invention is a Ni-based single crystal superalloy according to the any one of the above first to fourth inventions, which contains6.0 wt % of Co, 7.0 wt % of Cr, 1.5 wt % of Mo, 10.0 wt % of W, 5.5 wt % of Ta, 6.0 wt % of Al, 0.1 wt % of Ti and 0.10 wt % of Hf by weight, and contains neither Nb nor Re or contains them as unavoidable impurities.
A sixth invention is a Ni-based single crystal superalloy according to the any one of the above first to fourth inventions, which contains 8.0 wt % of Co, 7.0 wt % of Cr, 1.8 wt % of Mo, 8.2 wt % of W, 6.0 wt % of Ta, 5.2 wt % of Al, 1.6 wt % of Ti, 0.10 wt % of Hf and 0.8 wt % of Re by weight, and contains no Nb or contains it as an unavoidable impurity.
A seventh invention is a Ni-based single crystal superalloy according to the any one of the above first to third inventions, which contains 8.0 wt % of Co, 6.5 wt % of Cr, 1.4 wt % of Mo, 8.1 wt % of W, 6.0 wt % of Ta, 5.8 wt % of Al, 1.0 wt % of Ti, 0.10 wt % of Hf and 1.4 wt % of Re, and contains no Nb or contains it as an unavoidable impurity.
An eighth invention is a turbine blade which incorporates the Ni-based single crystal superalloy according to any one of the above first to seventh inventions.
According to the present invention, the amount of Re contained in the Ni-based single crystal superalloy is less than 3.0 wt %. Therefore, the Ni-based single crystal superalloy of the present invention has a smaller amount of Re as compared to the second generation Ni-based single crystal superalloy.
Describing in more detail hereinafter, the Ni-based single crystal superalloy of the present invention has high-temperature strength, mainly creep strength which is higher than that of the first generation Ni-based single crystal superalloy.
Therefore, the Ni-based single crystal superalloy of the present invention has a smaller amount of Re as compared to the second generation Ni-based single crystal superalloy, and is also excellent in high-temperature strength, mainly creep strength as compared to the first generation Ni-based single crystal superalloy.
One embodiment of a Ni-based single crystal superalloy and a turbine blade according to the present invention will be described with reference to the accompanying drawings shown below. In the drawings shown below, the scale of each member has been appropriately altered in order to make each member a recognizable size.
The Ni-based single crystal superalloy of the present embodiment has the following composition by weight: 0.1 wt % or more and 9.9 wt % or less of Co, 5.1 wt % or more and 10.0 wt % or less of Cr, 1.0 wt % or more and 4.0 wt % or less of Mo, 8.1 wt % or more and 11.0 wt % or less of W, 4.0 wt % or more and 9.0 wt % or less of Ta, 5.2 wt % or more and 7.0 wt % or less of Al, 0.1 wt % or more and 2.0 wt % or less of Ti, 0.05 wt % or more and 0.3 wt % or less of Hf, 1.0 wt % or less of Nb and less than 3.0 wt % of Re with the remainder including Ni and unavoidable impurities.
Also, the amount of Re in the Ni-based single crystal superalloy of the present embodiment is more preferably 2.0 wt % or less, 1.4 wt % or less, or 0.8 wt % or less by weight.
“Unavoidable impurities” are impurities which are included without being intentionally introduced in the production process until a Ni-based single crystal superalloy of the present embodiment is obtained and are present in trace amounts (for example, 0.1 wt % or less), and also which do not necessarily exert an influence on characteristics of the Ni-based single crystal superalloy.
Examples of the unavoidable impurities include B, C, Si, Y, La, Ce, V, Zr, Nb, Ru, Re and the like.
The composition ranges of the components of the Ni-based single crystal superalloy are controlled based on their characteristics described below.
Co is an element that increases the solid solubility limit to the matrix containing Al, Ta and other elements in high-temperature environments and causes the fine γ′ phase to disperse and precipitate in heat treatment so as to enhance the high-temperature strength. If more than 9.9 wt % of Co exists, the composition ratio with other elements, including Al, Ta, Mo, W, Hf and Cr, becomes unbalanced. As a result, a harmful phase precipitates to decrease the high-temperature strength. Due to the necessity of enhancing the high-temperature strength, 0.1 wt % or more of Co preferably exists. The amount of Co is therefore preferably 0.1 wt % or more and 9.9 wt % or less.
Cr is an element that has excellent oxidation resistance and improves, altogether with Hf and Al, high-temperature corrosion resistance of the Ni-based single crystal superalloy. If the amount of Cr is less than 5.1 wt %, it is difficult to provide a desired high-temperature corrosion resistance. If the amount of Cr exceeds 10.0 wt %, precipitation of the γ′ phase is inhibited and harmful phases, such as σ phase and μ phase, may precipitate to decrease the high-temperature strength. The amount of Cr is therefore preferably 5.1 wt % or more and 10.0 wt % or less.
Mo is an element that enhances the high-temperature strength by solid-dissolving in the γphase which becomes the matrix, in the copresence of W or Ta, and also improves high-temperature strength due to precipitation hardening. If the amount of Mo is less than 1.0 wt %, it is difficult to provide desired high-temperature strength. If the amount of Mo exceeds 4.0 wt %, the high-temperature strength decreases and the high-temperature corrosion resistance deteriorates. The amount of Mo is therefore preferably 1.0 wt % or more and 4.0 wt % or less.
W is an element that enhances the high-temperature strength due to the actions of solution hardening and precipitation hardening in the copresence of Mo or Ta. In order to enhance the high-temperature strength, 8.1 wt % or more of W preferably exists. If the amount of W exceeds 11.0 wt %, the high-temperature corrosion resistance deteriorates. The amount of W is therefore preferably 8.1 wt % or more and 11.0 wt % or less.
Ta is an element that enhances the high-temperature strength due to the actions of solution hardening and precipitation hardening in the copresence of Mo or W. Ta also enhances the high-temperature strength by the precipitation hardening relative to the γ′ phase. If the amount of Ta is less than 4.0 wt %, it is difficult to provide desired high-temperature strength. If the amount of Ta exceeds 9.0 wt %, a harmful phase, such as a phase and μ phase, may precipitate to decrease the high-temperature strength. The amount of Ta is therefore preferably 4.0 wt % or more and 9.0 wt % or less.
Al combines with Ni to form a 60 to 70% (volume percentage) of an intermetallic compound represented by Ni3Al, which is the fine γ′ phase to be uniformly dispersed and precipitated into the matrix. That is, Al is an element that enhances the high-temperature strength altogether with Ni. Furthermore, Al is excellent in oxidation resistance, and improves, altogether with Cr and Hf, the high-temperature corrosion resistance of the Ni-based single crystal superalloy. If the amount of Al is less than 5.2 wt %, the precipitation amount of the γ′ phase is insufficient and it is thus difficult to provide desired high-temperature strength and high-temperature corrosion resistance. If the amount of Al exceeds 7.0 wt %, a large amount of a coarse eutectic γ phase called a eutectic γ′ phase is formed, which makes it impossible to carry out a solution heat treatment and thus it becomes difficult to provide desired high-temperature strength. The amount of Al is therefore preferably 5.2 wt % or more and 7.0 wt % or less.
Ti is an element that enhances the high-temperature strength due to the actions of solution hardening and precipitation hardening in the copresence of Mo or W. Ti also enhances the high-temperature strength by the precipitation hardening with relative to the γ′-phase. If the amount of Ti exceeds 2.0 wt %, a harmful phase may precipitate to decrease the high-temperature strength. In order to enhance the high-temperature strength, 0.1 wt % or more of Ti preferably exists. The amount of Ti is therefore preferably 0.1 wt % or more and 2.0 wt % or less.
Hf is an element that segregates at the grain boundary and distributed unevenly in grain boundary to strengthen the same so as to enhance the high-temperature strength. Furthermore, Hf is excellent in oxidation resistance, and improves, altogether with Cr and Al, high-temperature corrosion resistance of the Ni-based single crystal superalloy. In order to enhance the high-temperature strength, 0.05 wt % or more of Hf preferably exists. If the amount of Hf exceeds 0.3 wt %, local melting occurs to decrease the high-temperature strength. The amount of Hf is therefore preferably 0.05 wt % or more and 0.3 wt % or less.
Nb is an element that enhances the high-temperature strength. However, if the amount of Nb exceeds 1.0 wt %, a harmful phase precipitates to decrease the high-temperature strength. The amount of Nb is therefore preferably 1.0 wt % or less.
Re is an element that enhances the high-temperature strength due to solid-solution strengthening by solid-dissolving in the γ phase which is the matrix. Re also enhances the corrosion resistance. However, if the amount of Re is 3.0 wt % or more, it becomes necessary to use Re in the same amount as that of a conventional second generation Ni-based single crystal superalloy. However, since it may be difficult to stably ensure supply of Re and also Re is expensive, the price of a Ni-based single crystal superalloy drastically rises when the amount of Re is large. In the present embodiment, even if the amount of Re is inhibited or Re is not included, it is possible to maintain enhanced high-temperature strength, mainly high creep strength in high-temperature environments by setting a composition ratio of other elements at an optimum range.
In the Ni-based single crystal superalloy of the present embodiment, the amount of Re is less than 3 wt %. Furthermore, in the Ni-based single crystal superalloy of the present embodiment, the amount of Re is preferably 2.0 wt % or less, more preferably 1.4 wt % or less, and still more preferably 0.8 wt % or less.
Subsequently, the results of tests carried out so as to make a comparison in a creep life between a Ni-based single crystal superalloy of the present embodiment and the first and second generation Ni-based single crystal superalloys with reference to
Black dots A to C shown in
The method of producing a Ni-based single crystal superalloy of the present embodiment is as follows.
First, a molten Ni-based single crystal superalloy is prepared using a vacuum melting furnace and an alloy ingot is casted using this molten alloy.
Furthermore, the alloy ingot is subjected to a solution heat treatment and an aging treatment to obtain a Ni-based single crystal superalloy. The solution heat treatment is carried out by raising the ingot from a temperature within a range of 1,503 to 1,563 K (1,230 to 1,290° C.) to a temperature within a range of 1,573 to 1,613 K (1,300 to 1340° C.) by a multi-stage step, followed by maintaining of such a temperature for 1 to 10 hours or more. The aging treatment is carried out by a primary aging treatment of maintaining the ingot at a temperature within a range of 1,273 to 1,423 K (1,000° C. to 1,150° C.) for 3 to 5 hours. Then, a secondary aging treatment of maintaining the ingot at a temperature within a range of 1,073 to 1,223 K (800° C. to 950° C.) for 15 to 25 hours is carried out.
CMSX-2, CMSX-4, ReneN4, ReneN5, PWA1480 and PWA1484 shown by white dots in
As is apparent from
As used herein, “do not contain Re as a useful component” includes, in addition to the case where no Re is included at all, the case where Re is included as an unavoidable impurity.
From the creep life of CMSX-2, PWA1480, ReneN4, ReneN5, CMSX-4 and PWA1484, it is assumes that, when the amount of Re in these conventional Ni-based single crystal superalloys varies within a range of 3.0 wt % or less, the life of the Ni-based single crystal superalloy is included in the region R1 shown in
It is possible to confirm that the Ni-based single crystal superalloy C of the present embodiment clearly has longer creep life as compared to the creep life to be assumed in the case where a conventional Ni-based single crystal superalloy contains 1.4 wt % of Re, and also has higher creep strength.
As is apparent from
As is apparent from
As is apparent from
As is apparent from
Regarding an actual value of the creep life in the present test, the actual values of the creep life of the Ni-based single crystal superalloys A of the present embodiment (which do not contain Re as a useful component) are 72 hours and 87 hours, the actual value of the creep life of the Ni-based single crystal superalloy B of the present embodiment (Re: 0.8 wt %) is 149 hours, the actual value of the creep life of the Ni-based single crystal superalloy B2 of the present embodiment (Re: 0.8 wt %) is 101 hours, the actual value of the creep life of the Ni-based single crystal superalloy C of the present embodiment (Re: 1.4 wt %) is 170 hours, the actual value of the creep life of PWA 1480 is 18 hours, the actual value of the creep life of ReneN4 is 31 hours, the actual value of the creep life of CMSX-2 is 45 hours, the actual value of the creep life of PWA1484 is 141 hours, the actual value of the creep life of ReneN5 is 89 hours, and the actual value of the creep life of CMSX-4 is 74 hours, respectively.
Subsequently, the results of a simulation carried out so as to make a comparison in a creep life between a Ni-based single crystal superalloy of the present embodiment and the first and second generation Ni-based single crystal superalloys with reference to
The present simulation was carried out using “JMatPro V.5.0” developed by Sente Software Co. of Great Britain. The present software enables calculation of values of physical, thermodynamic and mechanical properties of a metal alloy by a chemical component thereof and it has already been proved that the creep life of the Ni-based single crystal superalloy corresponding to the technical field of the present invention can also be predicted with satisfactory accuracy as shown in FIG. 16 of the following literature (Literature: N. Saunders, Z. Guo, X. Li, A. P. Miodownik and J-Ph. Schille: MODELLING THE MATERIAL PROPERTIES AND BEHAVIOUR OF Ni-BASED SUPERALLOYS, Superalloys 2004, (TMS, 2004), pp.849-858.)
The inventors of the present invention produced some single crystal superalloys and carried out a creep rupture test under the conditions at 1,100° C. under 137 MPa in the same manner as in the above test, and then made a comparison with the calculated value of the rupture life using “JMatPro V.5.0”.
As shown in
Herein, black dots shown in
CMSX-2, CMSX-4, ReneN4, ReneN5, PWA1480 and PWA1484 4 shown by white dots in
As is apparent from
From the creep life of CMSX-2, PWA1480, ReneN4, ReneN5, CMSX-4 and PWA1484, it is assumes that, when the amount of Re in these conventional Ni-based single crystal superalloys varies within a range of 3.0 wt % or less, the life of the Ni-based single crystal superalloy is included in the region R2 shown in
It is possible to confirm that the Ni-based single crystal superalloy “c and p” of the present embodiment clearly has longer creep life as compared to the creep life (region R2) to be assumed in the case where a conventional Ni-based single crystal superalloy contains 1.4 wt % of Re, and also has higher creep strength. As is apparent from
Furthermore, the Ni-based single crystal superalloy “r” of the present embodiments is that for comparison and contains 3.0 wt % of Re, which is equal to that in the conventional second generation Ni-based single crystal superalloy, and it is possible to confirm that the creep strength becomes higher as compared to the conventional Ni-based single crystal superalloy.
As is apparent from
Specifically, it is possible to confirm that the Ni-based single crystal superalloy of the present embodiment has characteristics improved by 30% or more as compared to the conventional Ni-based single crystal superalloy having the same content of Re.
The amount of Re in the above-described Ni-based single crystal superalloy of the present embodiment (excluding comparative Ni-based single crystal superalloy “r” used in the simulation) is less than 3.0 wt %. Therefore, the Ni-based single crystal superalloy of the present embodiment has smaller amount of Re as compared to the second generation Ni-based single crystal superalloy.
The Ni-based single crystal superalloy of the present embodiment has higher creep strength as compared to the first generation Ni-based single crystal superalloy.
Therefore, the Ni-based single crystal superalloy of the present embodiment has smaller amount of Re as compared to the second generation Ni-based single crystal superalloy, and is also excellent in creep strength as compared to the first generation Ni-based single crystal superalloy.
In the conventional Ni-based single crystal superalloy, it is necessary to add Ru, as rare metal, so as to inhibit the generation of a deteriorated layer due to the addition of Re. However, in the Ni-based single crystal superalloy of the present embodiment, it is not necessary to contain Ru and thus it becomes possible to perform cost reduction.
Subsequently, the results of a test carried out so as to make a comparison in a fatigue strength and a creep life between Ni-based single crystal superalloys of the present embodiment (Ni-based single crystal superalloys A and B2 (described above)) and the first and second generation Ni-based single crystal superalloys with reference to
As is apparent from
As is apparent from
The Ni-based single crystal superalloy of the present embodiment can be used as the material that forms a turbine blade 1 shown in
The turbine blade 1 which incorporates the Ni-based single crystal superalloy of the present embodiment has small amount of Re and is also excellent in high-temperature strength, mainly creep strength. Therefore, a turbine blade 1, which is inexpensive and has high strength, can be obtained.
While the invention has been described by way of forgoing Examples, but is not limited to the Examples. Also various combinations and selections of various disclosed essential elements are for illustrative purpose only and can be made without departing from the scope of the present invention.
According to the present invention, it is possible to obtain a Ni-based single crystal superalloy which has a smaller amount of Re as compared to a conventional Ni-based single crystal superalloy, and is also excellent in high-temperature strength, mainly creep strength.
1: Turbine blade
A-C, a-r: Ni-based single crystal superalloys
| Number | Date | Country | Kind |
|---|---|---|---|
| 2009-185757 | Aug 2009 | JP | national |
The present patent application is a divisional of prior U.S. patent application Ser. No. 13/375,987, now abandoned, filed Dec. 2, 2011, by Yasuhiro Aoki and Akihiro Sato, entitled “Ni-BASED SINGLE CRYSTAL SUPERALLOY AND TURBINE BLADE,” which is a 35 U.S.C. §§ 371 national phase conversion of International Application No. PCT/JP2010/063486, filed Aug. 9, 2010, which claims priority of Japanese Patent Application No. 2009-185757, filed Aug. 10, 2009. The PCT International Application was published in the Japanese language. The contents of each of the patent applications listed above are incorporated in full herein by reference.
| Number | Name | Date | Kind |
|---|---|---|---|
| 4582548 | Harris et al. | Apr 1986 | A |
| 4643782 | Harris et al. | Feb 1987 | A |
| 4719080 | Duhl et al. | Jan 1988 | A |
| 5100484 | Wukusick et al. | Mar 1992 | A |
| 5154884 | Wukusick et al. | Oct 1992 | A |
| 5489194 | Yoshinari et al. | Feb 1996 | A |
| 6054096 | Duhl et al. | Apr 2000 | A |
| 6159314 | Koizumi | Dec 2000 | A |
| 8771440 | Sato et al. | Jul 2014 | B2 |
| 20030041930 | DeLuca et al. | Mar 2003 | A1 |
| 20040221925 | Tamaki et al. | Nov 2004 | A1 |
| 20080112814 | Nazmy et al. | May 2008 | A1 |
| 20110076180 | Suzuki et al. | Mar 2011 | A1 |
| Number | Date | Country |
|---|---|---|
| 2048756 | Mar 1992 | CA |
| 1 184 473 | Mar 2002 | EP |
| 1431405 | Jun 2004 | EP |
| 1 876 263 | Jan 2008 | EP |
| 1 592 237 | Jul 1981 | GB |
| 2 234 521 | Feb 1991 | GB |
| 53-146223 | Dec 1978 | JP |
| 59-019032 | Jan 1984 | JP |
| 7-070679 | Mar 1995 | JP |
| 11-246924 | Sep 1999 | JP |
| 2026399 | Jan 1995 | RU |
| 2297466 | Apr 2007 | RU |
| WO 2006067189 | Jun 2006 | WO |
| WO 2007037277 | Apr 2007 | WO |
| WO 2007122931 | Nov 2007 | WO |
| Entry |
|---|
| International Search Report and Written Opinion dated Nov. 2, 2010 in corresponding PCT International Application No. PCT/JP2010/063486. |
| N. Saunders et al., “Modelling the Material Properties and Behaviour of Ni—Based Superalloys,” Superalloys 2004 (TMS, 2004), pp. 849-858. |
| Canadian Office Action dated Nov. 22, 2012 issued in corresponding Canadian Patent Application No. 2,764,664. |
| Chinese Office Action and English translation dated Mar. 6, 2013 issued in corresponding Chinese Patent Application No. 201080028753.3. |
| Russian Federation Notice of Allowance, dated Jan. 23, 2014, issued in corresponding Russian Patent Application No. 2011153366/02(080297). English translation. Total 11 pages. |
| Extended European Search Report and European Search Opinion dated Feb. 4, 2015 in corresponding European Patent Application No. 10808201.7 (10 pages). |
| Number | Date | Country | |
|---|---|---|---|
| 20160010183 A1 | Jan 2016 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 13375987 | US | |
| Child | 14858421 | US |