1. Field of the Invention
The present invention relates to a nonvolatile semiconductor memory device and a method of manufacturing the same, particularly, to a gate structure of a semiconductor device having a nonvolatile memory transistor including a floating gate and a control gage, a selective transistor arranged close to said memory transistor, and a peripheral circuit mounted on the same chip.
2. Description of the Related Art
Known is a flash memory having a memory transistor including a floating gate and a control gate, a selective transistor arranged close to the memory transistor, and a peripheral circuit for driving the memory transistor and the selective transistor mounted to the same chip. A typical flash memory is called a NAND type flash memory. The NAND type flash memory includes a plurality of memory transistors connected in series, a selective transistor arranged close to the both edge portions of the memory transistor, and a peripheral circuit transistor for driving the memory transistor and the selective transistor. The region in which are arranged the memory transistors is called a memory cell array region, the region in which is arranged the selective transistor is called a selective gate region, and the region in which is arranged the peripheral circuit transistor is called a peripheral circuit region.
The method of preparing the flash memory of this type includes, for example, the steps of forming a gate insulating film on a semiconductor layer, depositing a polycrystalline silicon (polysilicon) film providing the floating gate of the memory transistor on the gate insulating film, and forming an element isolating region. In this case, a gate electrode of a two layer structure consisting of a floating gate and a control gate is present in at least a portion of the selective gate region and the peripheral circuit region as in the memory cell array region. It should be noted that it is necessary for the transistor in the selective gate region and the peripheral circuit region to be electrically connected to an upper wiring by withdrawing the floating gate. A conventional semiconductor device of this type will now be described.
As shown in
The semiconductor device according to the first prior art described above comprises a floating gate of the double layer structure consisting of the first and second floating gate electrode layers 13a and 13b. In the floating gate of the particular construction, the first floating gate electrode layer 13a is self-aligned with the element isolating region 15, and the second floating gate electrode layer 13b is pulled up onto the element isolating region 15. However, the first prior art described above gives rise to problems.
First of all, in the memory cell array region, it was necessary to set the width P of the open portion 50 such that the open portion 50 is not buried with the second insulating film 16. It was also necessary to ensure an aligning allowance Q between the open portion 50 and the element region 10 in the lithography. However, it was difficult to finely adjust the open portion 50 because of the limit in the resolution of the photoresist in patterning the open portion 50. As a result, it was difficult to achieve the fineness beyond a certain level, with the result that it was difficult to make the memory cell finer.
On the other hand, in the peripheral circuit region, the contact hole 20 is formed on the element isolating region 15, making it possible to avoid the damage done to the element region. However, the element region is formed a long distance away from the connecting portion 25 between the second floating gate electrode layer 13b and the contact hole 20. Therefore, since the second floating gate electrode layer 13b is formed of in general an electrode material having a high resistivity such as polysilicon, the delay caused by the resistance is increased so as to lower the performance of the element. It should also be noted that, if the second floating gate electrode layer 13b is allowed to extend over the element isolating region 15, a capacitance coupling is formed between the semiconductor layer 11 and the floating gate with the insulating film of the element isolating region 15 interposed therebetween, leading to an increased RC delay.
Particularly, when it comes to the selective transistor of the NAND type flash memory, the increase in the RC delay described above is a serious problem to be solved. The contact to the second floating gate electrode layer 13b is formed as required for several cells within the memory cell array. The contact portion requires an area so as to increase the area of the memory cell array. Also, since the contact hole 20 can be formed in only a part of the memory cell array, the contact hole 20 is connected to the transistor via the second floating gate electrode layer 13b formed of polysilicon having a high resistivity. It follows that the problem of the RC delay time to the transistor positioned remote from the contact hole 20 is rendered serious. It should be noted that the increase in the delay time of the selective transistor adversely affects the reading speed of the memory cell.
As shown in the drawing, a first insulating film 12 is formed on a semiconductor layer 11, and a floating gate electrode layer 13 is formed on the first insulating film 12. Then, an element isolating groove is formed, followed by filling the element isolating groove with an insulating film. An element isolating region 15 is formed by planarizing the insulating film until the surface of the floating gate electrode layer 13 is exposed to the outside. Then, an upper portion of the element isolating region 15 in the memory cell array region and the selective gate region is removed so as to allow the upper surface of the element isolating region 15 in the memory cell array region and the selective gate region to be positioned lower than the upper surface of the floating gate electrode 13. Further, a second insulating film 16 is formed on the floating gate electrode layer 13 and the element isolating region 15, followed by removing the second insulating film 16 in the peripheral circuit region and the selective gate region. In the nest step, a control gate electrode layer 18 is formed on the second insulating film 16, the floating gate electrode layer 13 and the element isolating region 15, followed by patterning the control gate electrode layer 18, the second insulating film 16 and the floating gate electrode layer 13. After the patterning step, a third insulating film 19 is formed on the entire surface of the semiconductor layer 11, followed by forming a contact hold 20 in the third insulating film 19. In the nest step, a wiring 21 connected to the contact hole 20 is formed.
In the semiconductor device according to the second prior art described above, it is unnecessary to ensure an aligning allowance Q in the lithography, which is required in the first prior art, so as to make it possible to miniaturize the memory cell. Also, since the control gate electrode layer 18 is deposited after removal of the selective gate region and the second insulating film 16 of the peripheral circuit region, the limitation in the position of the contact hole 20 can be eliminated even if the circuit is separated such that the floating gate is left unremoved in only the element region 10. However, the second prior art gives rise to the problem as described below.
First, the second insulating film 16 is interposed between the floating gate electrode 13 and the control gate electrode layer 18 in the gate in the memory cell array region. However, the second insulating film 16 is not interposed between the floating gate electrode 13 and the control gate electrode layer 18 in the gate in the peripheral circuit region and the selective gate region. In other words, the memory cell array region, the peripheral circuit region and the selective gate region differ from each other in the laminate structure of the gate. As a result, in forming the gate, it is necessary for the memory cell array region, the peripheral circuit region and the selective gate region to be different from each other in the etching conditions, giving rise to the problem that it is impossible to form simultaneously the gates in the memory cell array region, peripheral circuit region and the selective gate region.
It should also be noted that, if it is impossible to form simultaneously the gates in the memory cell array region, the peripheral circuit region and the selective gate region, the electrode layer is left unremoved in the boundary portion between the memory cell array region, the peripheral circuit region and the selective gate region. Also, it is necessary to ensure a sufficient allowance region in order to prevent the semiconductor layer from being dug by the etching treatment performed twice. In order to process accurately both the memory cell array region, the peripheral circuit region and the selective gate region differing from each other in the laminate structure, it is necessary to ensure various allowances in the boundary portion, leading to an increase in the chip area. Particularly, in the construction of the NAND type flash memory, it is necessary to diminish the distance D between the memory cell and the selective transistor as much as possible in order to increase the degree of integration of the memory cell array, as shown in
As described above it was very difficult to avoid the resistance delay in the peripheral circuit region and the selective gate region while miniaturizing the memory cell array region and to form simultaneously the gates in the memory cell array region, the peripheral circuit region and the selective gate region in the semiconductor device according to each of the first and second prior arts.
According to a first aspect of the present invention, there is provided a semiconductor device, comprising a semiconductor layer; a first insulating film formed on the semiconductor layer; a first electrode layer formed on the first insulating layer; an element isolating region comprising an element isolating insulating film formed to extend through the first electrode layer and the first insulating film to reach an inner region of the semiconductor layer, the element isolating region isolating an element region and being self-aligned with the first electrode layer; a second insulating film formed on the first electrode layer and the element isolating region, an open portion exposing a surface of the first electrode layer being formed in the second insulating film; and a second electrode layer formed on the second insulating film and the exposed surface of the first electrode layer, the second electrode layer being electrically connected to the first electrode layer via the open portion.
According to a second aspect of the present invention, there is provided a semiconductor device, comprising a semiconductor layer; a first insulating film formed on the semiconductor layer; a first electrode layer firmed on the first insulating layer; an element isolating region comprising an element isolating insulating film formed to extend through the first electrode layer and the first insulating film to reach an inner region of the semiconductor layer, the element isolating region isolating an element region and being self-aligned with the first electrode layer; a second insulating film formed on the first electrode layer and the element isolating region, an open portion exposing a surface of the first electrode layer being formed in the second insulating film; a second electrode layer formed an the second insulating film; and a third electrode layer formed on the second electrode layer and the exposed surface of the first electrode layer, the third electrode layer being electrically connected to the first electrode layer via the open portion.
According to a third aspect of the present invention, there is provided a method of manufacturing a semiconductor device in a selective gate region provided a selective gate transistor formed adjacent to a memory cell array region, comprising: forming a first insulating film on a semiconductor layer; forming a first electrode layer on the first insulating film; forming an element isolating region comprising an element isolating insulating film extending through the first electrode layer and the first insulating film to reach an inner region of the semiconductor layer, the element isolating region isolating an element region; forming a second insulating film on the element isolating region and the first electrode layer; forming an open portion within the second insulating film to expose a surface of the first electrode layer; forming a second electrode layer on the second insulating film and the exposed surface of the first electrode layer; and selectively removing the first electrode layer, the second insulating film and the second electrode layer to form a gate electrode.
According to a fourth aspect of the present invention, there is provided a method of manufacturing a semiconductor device in a selective gate region provided a selective gate transistor formed adjacent to a memory cell array region, comprising: forming a first insulating film on a semiconductor layer; forming a first electrode layer on the first insulating film; forming an element isolating region comprising an element isolating insulating film extending through the first electrode layer and the first insulating film to reach an inner region of the semiconductor layer, the element isolating region isolating an element region; forming a second insulating film on the element isolating region and the first electrode layer; forming a second electrode layer on the second insulating film; forming an open portion within the second insulating film to expose a surface of the first electrode layer; forming a third electrode layer on the second electrode layer and the exposed surface of the first electrode layer; and selectively removing the first electrode layer, the second insulating film, the second electrode layer and the third electrode layer to form a gate electrode.
According to a fifth aspect of the present invention, there is provided a method of manufacturing a semiconductor device in a selective gate region provided a selective gate transistor formed adjacent to a memory cell array region, comprising: forming a first insulating film on a semiconductor layer; forming a first electrode layer on the first insulating film; forming an element isolating region comprising an element isolating insulating film extending through the first electrode layer and the first insulating film to reach an inner region of the semiconductor layer, the element isolating region isolating an element region; forming a second insulating film on the element isolating region and the first electrode layer; forming a second electrode layer on the second insulating film; forming a first mask layer on the second electrode layer; forming a groove comprising a pair of mutually facing side surfaces in the first mask layer, the groove being formed to expose partly a surface of the second electrode layer; forming a side wall comprising a second mask layer on the exposed side surface of the groove; selectively removing the second electrode layer and the second insulating film by using the first and second mask layers to form an open portion exposing a surface of the first electrode layer; removing the first and second mask layers; forming a third electrode layer on the second electrode layer and the exposed surface of the first electrode layer; and selectively removing the first electrode layer, the second insulating film, the second electrode layer and the third electrode layer to form a gate electrode.
The present invention is directed to the gate structure of a semiconductor device having a nonvolatile memory transistor including a floating gate, a selective transistor arranged close to the memory cell, and a transistor of a peripheral circuit for driving the memory cell array mounted to the same chip. The present invention is applied to, for example, a NAND type flash memory.
Some embodiments of the present invention will now be described with reference to the accompanying drawings. In the following description, the common portions of the semiconductor device are denoted by the common reference numerals. Incidentally, in the drawings, the memory cell array region denotes the region in which a memory transistor is arranged, the selective gate region denotes the region in which the selective transistor is arranged, and the peripheral circuit region denotes the region in which the peripheral circuit transistor is arranged.
A first embodiment is directed to the constructions of the memory transistor and the selective transistor. In this case, an open portion is formed in a part of the insulating film between the first and second electrodes constituting a selective transistor.
As shown in
As shown in
It should be noted that the surface of the element isolating region 15 is positioned lower than the surface of the first electrode layer 13. In the memory cell array region, the first electrode 13 performs the function of a floating gate, and the second electrode layer 18 performs the function of a control gate.
As shown in
Incidentally, the pattern of the open portion 17 extends over the element separating region 15 in the selective gate region as shown in
It should be noted that the second electrode layer 18 has a resistivity lower than that of the first electrode layer 13. Therefore, it is desirable for the second electrode layer 18 to be formed of, for example, a metal layer having a high melting point or a lamination layer film comprising a metal silicide layer having a high melting point and a polysilicon layer. Also, it is desirable for the second insulating film 16 to be formed of a composite insulating film comprising a silicon nitride film such as an ONO (Oxide Nitride Oxide) film. The silicon nitride film effectively prevents the etching damage in the formation of the contact hole 20 and also prevents effectively the layer for the metal wiring formed within the contact hole from adversely affecting the gate insulating film 12.
First of all, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
According to the first embodiment described above, the first electrode layer 13 is self-aligned with formation of the element isolating region 15, with the result that the fine processing of the first electrode layer 13 can be performed easily, compared with the 20 first prior art referred to previously It follows that it is possible to miniaturize the memory cell array region.
Also, in the selective gate region, the electrical connection between the wiring 21 for supplying signals to the first electrode layer 13 and the first electrode layer 13 is achieved via the second electrode layer 18 extended over the element isolating region 15.
In other words, it is unnecessary to draw the first electrode layer 13 having a high resistively onto the element isolating region 15, making it possible to avoid the problem of the delay caused by the resistance of the first electrode layer 13 and to avoid the problem of the RC delay caused by the capacitive coupling between the semiconductor layer 11 and the first electrode layer 13. In addition, since the second electrode layer 18 is formed of a metal layer having a high melting point or a low resistance layer including a metal silicide layer having a high melting point, it is possible to avoid the problem of the resistance delay, making it possible to obtain an operating speed substantially equal to that of the transistor formed of a gate electrode layer of a single layer structure having a low resistivity. It follows that it is possible to avoid the problem that the reading speed of the memory cell is adversely affected by the increase in the delay time.
Concerning the gate of the selective gate region, the open portion 18 is formed in the center of the second electrode layer 18. Therefore, the gate is of a two-layer structure consisting of the first electrode layer 13 and the second electrode layer 18. However, the gate is of a three-layer structure, consisting of the first electrode layer 13, the second electrode layer 18, and the second insulating film 16 interposed between the first electrode layer 13 and the second electrode layer 18 in the edge portion of the second electrode layer 18 in which the gate is formed.
It follows that, concerning the region in which the gate is formed, the memory cell array region and the selective gate region are equal to each other in the laminate structure of the gate. As a result, it is possible to form simultaneously the gates in the memory cell array region and the selective gate region.
In addition, since a special structure is not required between the selective gate region and the memory cell array region, it is possible to set the distance D between the memory cell and the selective transistor at, for example, the minimum processing size.
Also, in the open portion 17 of the insulating film 16, the length of the open portion 17 in a direction perpendicular to the direction of the gate length L is large, though the width of the open portion 17 in the direction of the gate length L is small. As a result, the resolution is facilitated in the lithography process in patterning the open portion 10. It follows that it is possible to form a fine open portion 17 even in the case where the gate length L of the selective transistor is rendered long in accordance with miniaturization of the selective transistor.
As described above, the first embodiment of the present invention makes it possible to decrease the memory cell size and to improve the degree of integration including the selective transistor. Particularly, it is possible to decrease the size of the memory cell array of the NAND type flash memory.
A second embodiment is featured in that the control gate is formed of a plurality of electrode layers in order to prevent the deterioration in the reliability of the second insulating film in the memory cell array region in forming an open portion.
In the first step, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
In the next step, as shown in
The second embodiment, which produces the effect similar to that obtained in the first embodiment, further produces an additional effect as follows.
In the first embodiment, a resist forming the mask 22 is formed on the second insulating film 16 in the memory cell array region in the lithography process, i.e., the step shown in
A third embodiment is directed to a method that is effective in the case where it is desired to decrease the width of the open portion referred to previously in conjunction with the first embodiment. For example, the miniaturization has proceeded to the stage that the gate length of the selective transistor has been decreased to about 0.2 μm in the NAND type flash memory. If an open portion is to be formed in only the central portion of the gate, it is necessary to form a pattern having a width of, for example, 0.1 μm. The third embodiment is effective for such a case. Incidentally, the semiconductor device according to the third embodiment of the present invention is substantially equal to the semiconductor device according to the second embodiment and, thus, description of semiconductor device according to the third embodiment is omitted.
In the first step, as shown in
In the next step, as shown in
Then, as shown in
In the next step, the electrode layer 18a and the second insulating film 16 are selectively removed by using the first and second mask layers 22, 23 as a mask so as to form the open portion 17 above the element region 10, as shown in
Further, the third electrode layer 18b is formed on the second electrode layer 18a and the first electrode layer 13, as shown in
The third embodiment permits producing the effects similar to those obtained in the first and second embodiments.
It should also be noted that the second electrode layer 18a constituting a part of the control gate and the second insulating film 16 are self-aligned with the open portion 17. As a result, it is possible to form the open portion 17 with a width smaller than the size that can be achieved by the lithography, making it possible to achieve the connection between the first electrode layer 13 and the third electrode layer 18b with a space smaller than that in the first embodiment. It follows that It is possible to further miniaturize a gate length of the selective transistor, compared with the first embodiment.
As described above, the third embodiment is highly effective in the cases where the gate length of the selective transistor is small so as to make it impossible to form the open portion in the center of the gate with a size.
Incidentally, the method utilizing formation of the side wall described above permits forming the open portion 17 with a width smaller than that in the case of using the lithography. Alternatively, it is also possible to employ the method of, for example, swelling the photoresist by the heat treatment after the lithography process so as to form the open portion of a smaller space. As a result, it is possible to form the open portion having the width smaller than the width of the groove formed by the lithography process.
In each of the first to third embodiments of the present invention, the technical idea of the present invention is applied to the memory cell array region and the selective gate region. On the other hand, a fourth embodiment of the present invention is featured in that the structure similar to that of the selective gate region is also applied to the peripheral circuit region.
As shown in
As shown in
The fourth embodiment, which produces the effect similar to that obtained in the first embodiment, further produces an additional effect as follows.
First of all, in the fourth embodiment of the present invention, the first electrode layer 13 having a low resistivity is connected to the second electrode layer 18 having a low resistivity right above the element region 10. As a result, it is possible to shorten the RC delay time of the peripheral circuit, compared with the prior art, as in the selective transistor.
Also, the open portion 17 is not present in the edge portions of the first electrode layer and the second electrode layer above the element region 10. Therefore, in the process step of the gate, it is possible to process simultaneously the peripheral circuit region in addition to the memory cell array region and the selective gate region. Where the gates of all the elements can be processed simultaneously, the aligning allowance in the lithography process requiring the contact hole and the gate electrode can be decreased in the subsequent step of forming the contact hole.
A fifth embodiment is a modification of the fourth embodiment and is featured in that the second insulating film in the peripheral circuit region is removed completely.
Depending on the performance and the operating voltage required for the peripheral circuit, the gate of the transistor constituting the peripheral circuit must be made very short in some cases. In this case, it is necessary to make small the open portion 17 of the second insulating film 17. However, if the size of the opening is very small, it is very difficult to form the open portion 17 if using the third embodiment.
Such being the situation, the second insulating film 16 is completely removed in the transistor of the peripheral circuit region, as shown in
In other words, the peripheral circuit region of the semiconductor device according to the fifth embodiment of the present invention comprises the semiconductor layer 11, the semiconductor isolating region 15 isolating the element region 10 of the semiconductor layer 11, the first electrode layer 13 formed above the element region 10 with the first insulating film 12 interposed therebetween and self-aligned with the element isolating region 15, and the second electrode layer 18 formed on the first electrode layer 13 and the element isolating region 15.
The fifth embodiment of the present invention produces the effects similar to those produced by the fourth embodiment.
Further, the fifth embodiment is effective in the case where the gate length of the transistor is very short. It should be noted, however, that, since the peripheral circuit transistor differs from the memory transistor and the selective transistor in the gate structure, it is necessary to apply the gate processing separately to the memory cell array region, the selective gate region and the peripheral circuit region, leading to an increase in the number of manufacturing steps. However, since the memory transistor and the selective transistor are equal to each other in the construction of the gate edge portion, the memory cell array region and the selective gate region can be processed simultaneously so as to make it unnecessary to provide processing boundary. It follows that the fifth embodiment produces a prominent effect in decreasing the total area of the memory cell array like the other embodiments described previously.
Incidentally, the selective transistor is generally designed somewhat longer than the minimum possible size of the lithography because the selective transistor is required to withstand a high voltage required for driving the memory cell. It follows that it is sufficiently possible to form the fine open portion 17 by, for example, the method described previously in conjunction with the third embodiment of the present invention.
A sixth embodiment is featured in that a contact hole is formed above the element region in which the second insulating film is present so as to decrease the area of the peripheral transistor.
As shown in
The sixth embodiment produces effects similar to those produced by the fourth embodiment and additional effects as described below.
In general a barrier metal film (Ti/TiN), an Al—Cu film, etc. are formed in the contact hole 20 by a sputtering method for connection of the contact hole 20 to the gate. What should be noted is that Ti in the barrier metal film reacts with polysilicon forming the second electrode layer 18 so as to form a TiSi layer. Therefore, where the second insulating film 16 is not formed, the TiSi layer is formed to extend from the interface between the contact hole 20 and the second electrode layer 18 to reach a region near the first insulating film 12, making it possible to destroy the first insulating film 12. Such being the situation, the contact hole 20 connected to the gate is not formed in general above the element region 10.
In the sixth embodiment, however, the second insulating film 16 is interposed between the first electrode layer 13 and the second electrode layer 18. What should be noted is that the second insulating film 16 thus formed acts as a protective film so as to avoid the problem described above. Particularly, where a composite film including a silicon nitride film is used as the second insulating film 16, the nitride film is highly effective for avoiding the influences given to the metal of the upper layer having a high melting point and to the underlying polysilicon film of the silicide layer.
As described above, according to the sixth embodiment of the present invention, the second insulating film 16 is left unremoved so as to make it possible to form the contact hole 20 above the element region 10. It follows that it is possible to obtain prominent effects similar to those obtained in each of the first to third embodiments described previously, as described below.
First of all, the sixth embodiment of the present invention shown in
What should also be noted is that the sixth embodiment of the present invention makes it possible to increase the inversion voltage of the element separating region 15 without increasing the peripheral circuit region. To be more specific, in a semiconductor device using a high voltage such as a NAND type flash memory, it is necessary to increase the inversion voltage of the element separating region 15 below the gate. In this case, it was necessary to take measures. For example, it was necessary to increase the impurity concentration in the impurity diffusion layer 11′ of the semiconductor layer 11 below the element separating region 15, as shown in
Incidentally, the sixth embodiment of the present invention can also be applied to the case where the control gate of the memory cell is of a two-layer structure consisting of the second electrode layer 18a and the third electrode layer 18b as in the second and third embodiments described previously.
A seventh embodiment of the present invention is featured in that the widths of the open portions of the insulating films are made equal to each other in a plurality of peripheral circuit transistors.
As shown in
The seventh embodiment produces effects similar to those produced by the fourth embodiment and additional effects as described below.
The widths c of the open portions 17 in all the gate electrodes on the chip are made equal to each other. As a result, where the open portions 17 are filled with the third electrode layer 18b, it is possible to suppress to the minimum level the nonuniformity in the stepping of the third electrode layer 18h. It follows that the seventh embodiment is adapted for depositing flat the third electrode layer 18b.
It should also be noted that If the widths c of the open portions 17 are made equal to each other, the patterning by the lithography can be controlled easily in forming the open portions 17.
Further, the seventh embodiment of the present invention makes it possible to suppress the dimensional nonuniformity of the widths c of the open portions 17.
An eighth embodiment is featured in that a plurality of open portions are formed in the same gate electrode and the widths of these open portions are made equal to each other.
As shown in
According to the eighth embodiment of the present invention, since the widths c of the open portions 17 are equal to each other, it is possible to obtain the effects similar to those produced by the seventh embodiment.
Further, a plurality of open portions 17 are formed in the same gate electrode so as to increase the connection area between the first electrode layer 13 and the third electrode layer 18b. As a result, it is possible to decrease the contact resistance between the first electrode layer 13 and the third electrode layer 18b.
Incidentally, in forming a plurality of open portions within the same gate electrode, it is possible to form the open portions 17 in the cross (+) shape as shown in
An ninth embodiment is featured in that, in forming a plurality of open portions in the same gate electrode as in the eighth embodiment distances between the adjacent open portions 17 are made uniform.
As shown in
According to the ninth embodiment of the present invention, since a plurality of open portions 17 are formed and the widths c of these open portions are equal to each other, it is possible to obtain the effects similar to those obtained in the seventh and eighth embodiments described previously.
Further, the distances d between the adjacent open portions 17 formed in the gate electrode are equal to each other. It should be noted that, in order to form the open portions 17 at a uniform interval, it is necessary to form the light exposure portions at the same width in the lithography step for forming the open portions 17, as shown in
It is possible to apply the ninth embodiment of the present invention to a NAND type flash memory.
In the NAND type flash memory, the selective transistor and the peripheral circuit transistor, which differ from each other in the gate length, are formed in same chip, as shown in
In general the size of the selective transistor is smaller than that of the peripheral circuit transistor. Therefore, in order to miniaturize the element, it is advisable to determine the distances e1 and e2 noted above such that the distance e2 between the adjacent open portions in the peripheral circuit transistor is determined in accordance with the distance e1 between the open portions 17 in the selective transistor on the basis of the distance e1 noted above.
A tenth embodiment is featured in that the open portion is allowed to extend from above the element region onto the element isolating region in the direction of the channel width.
In the fourth embodiment, etc. described previously, the open portion 17 is formed within the element region 10 as shown in
According to the ninth embodiment of the present invention, which produces the effect similar to that obtained in the fourth embodiment.
Further, the open portion 17 is allowed to extend from above the element region 10 onto the element isolating region 15 in the direction of the channel width f. As a result, the open portion 17 can be formed without being restricted by the limit of the processing of the lithography even in the case of a transistor having a small channel width f.
An eleventh embodiment is featured in that defined is the relationship between the width of the open portion and the thickness of the electrode layer deposited in a manner to fill the open portion.
As shown In
According to the eleventh embodiment of the present invention, which produces the effect similar to that obtained in the fourth embodiment.
Further, the widths c of the open portions of the transistors are made equal to each other, and the thickness of the third electrode layer 18b when deposited is set at a value not smaller than c/2.
As a result, the open portion 17 is filled completely with the third electrode layer 18b without fail, and the third electrode layer 18c can be deposited in manner to have a smooth upper surface.
It should also be noted that, since the width c of the open portion 17 is made small, it is possible to decrease the thickness of the third electrode layer 18b required for allowing the surface of the third electrode layer 18b to be smooth. It follows that it is possible to decrease the total height of the gate electrode. As a result, the aspect ratio of the space S of the gate electrode of the memory cell array region is diminished so as to make it possible to bury easily a third insulating film 19 for insulating the upper wiring (not shown) and the gate electrode in the space s of the gate electrode, as shown in
Since the eleventh embodiment produces the particular effects described above, it is possible to avoid the problems described below.
The first problem is that, where the width of the open portion 17 is at least twice the deposition thickness a of the third electrode layer 18b, a stepped portion is formed on the surface of the third electrode layer 18b on the open portion 17, if the third electrode layer 18b is deposited within the open portion 17, as shown in
The second problem is that a fourth electrode layer 18c, e.g., a WSi layer, is formed on the third electrode layer 18b, followed by forming a resist 22′ on the fourth electrode layer 18c, as shown in
The third problem is that, where a fourth electrode layer 18c is deposited on the third electrode layer 18b as shown in
The fourth problem is that, in order to deposit the third electrode layer 18b in a manner to have a flat surface in all the transistors differing from each other in the gate length, it is necessary for the deposition thickness of the third electrode layer 18b to be at least half the maximum width of the open portion so as to fill the open portion having the maximum width of the open portion as shown in
The fifth problem is that, if the deposition thickness of the third electrode layer 18b is increased as pointed out in conjunction with the fourth problem, the space s between the adjacent gate electrodes is formed in the memory cell array region in a manner to have a high aspect ratio as shown in
As a result, it is rendered difficult to fill sufficiently the space S with an interlayer insulating film 19 for insulating the upper wiring (not shown) and the element region 10, giving rise to generation of a void 31.
A twelfth embodiment is featured in that the relationship between the width of the open portion and the thickness of the electrode layer filling the open portion is defined and a treatment to planarize the surface of the electrode layer is applied.
As shown in
According to the twelfth embodiment of the present invention, which produces the effect similar to that obtained in the eleventh embodiment.
Further, the thickness of the third electrode layer 18b can be made smaller than the thickness in the step of depositing the third electrode layer by planarizing the surface of the third electrode layer 18b by CDE or CMP. In other words, since the total thickness of the gate electrode can be decreased, the clearance between the adjacent gate electrodes can be filled more easily with the third insulating film 19 than in the eleventh embodiment.
Incidentally, in each of the first to twelfth embodiments of the present invention described above, the first electrode layer 13 is of a single layer structure for the sake of brevity. However, it is possible to modify the first electrode layer 13 in various fashions. For example, it is possible for the first electrode layer to be of a two-layer structure consisting of electrode layers 13a and 13b. It is also possible for the first electrode layer to have a two dimensional convex-concave portion. Also, in each of the first to twelfth embodiments described above, the first electrode layer 13 is self-aligned with the element region 10. However, it is possible for the first electrode layer 13 to protrude in a self-aligned fashion from the element region 10 toward the element separating region 15.
Additional advantages and modifications will readily occur to those skilled in the art. Therefore, the invention in its broader aspects is not limited to the specific details and representative embodiments shown and described herein. Accordingly, various modifications may be made without departing from the spirit or scope of the general inventive concept as defined by the appended claims and their equivalents.
Number | Date | Country | Kind |
---|---|---|---|
2000-291910 | Sep 2000 | JP | national |
2001-272224 | Sep 2001 | JP | national |
This application is a continuation of U.S. application Ser. No. 13/421,248, filed Mar. 15, 2012, which is a continuation of U.S. Ser. No. 13/085,884 filed Apr. 13, 2011, which is a continuation of U.S. Ser. No. 12/435,842 filed May 5, 2009, which is a continuation of U.S. Ser. No. 11/556,299 filed Nov. 3, 2006, which is a division of U.S. Ser. No. 11/399,657 filed Apr. 7, 2006, which is a division of U.S. Ser. No. 11/168,410 filed Jun. 29, 2005, which is a division of U.S. Pat. No. 6,927,449, issued Aug. 9, 2005, which is a division of U.S. Pat. No. 6,835,978, issued Dec. 28, 2004, and is based upon and claims the benefit of priority from the prior Japanese Patent Applications No. 2000-291910, filed Sep. 26, 2000, and No. 2001-272224, filed Sep. 7, 2001, the entire contents of each of which are incorporated herein by reference.
Number | Date | Country | |
---|---|---|---|
Parent | 11399657 | Apr 2006 | US |
Child | 11556299 | US | |
Parent | 11168410 | Jun 2005 | US |
Child | 11399657 | US | |
Parent | 10991521 | Nov 2004 | US |
Child | 11168410 | US | |
Parent | 09956986 | Sep 2001 | US |
Child | 10991521 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 13837552 | Mar 2013 | US |
Child | 14707968 | US | |
Parent | 13421248 | Mar 2012 | US |
Child | 13837552 | US | |
Parent | 13085884 | Apr 2011 | US |
Child | 13421248 | US | |
Parent | 12435842 | May 2009 | US |
Child | 13085884 | US | |
Parent | 11556299 | Nov 2006 | US |
Child | 12435842 | US |