The present application claims priority from Korean Patent Application Number 10-2012-0136263 filed on Nov. 28, 2012, the entire contents of which are incorporated herein for all purposes by this reference.
1. Field of the Invention
The present invention relates to a method of fabricating a zinc oxide (ZnO) thin film, and more particularly, to a method of fabricating a ZnO thin film in which the surface shape of the ZnO thin film can be controlled during deposition of the ZnO thin film.
2. Description of Related Art
Transparent conductive oxides such as indium tin oxide (ITO), zinc oxide (ZnO) and tin oxide (SnO2) are widely used as a key material in a variety of products, such as flat panel displays, organic light-emitting displays and CIGS photovoltaic cells which are currently regarded as a big issue. Common properties that these products require for transparent conductive oxides include high transmittance, high electric conductivity and a flat surface shape. In particular, the flat surface shape prevents problems when a semiconductor device is formed on a transparent conductive oxide. In this way, the flat surface shape acts as an important element that is directly related to the yield of display panels.
In contrast, unlike the above-stated products, tandem-type photovoltaic cells, organic light-emitting diodes (OLEDs) for illumination and the like can have a higher efficiency when the surface of a transparent conductive oxide has a patterned textured structure or a random textured structure. This is because the textured surface structure increases the path of light so that the opportunity to absorb light is increased in photovoltaic cells and reduces total internal reflection of light so that more light is extracted to the outside in OLEDs for illumination.
At present, ITO is widely used in products which require a smooth surface shape, whereas ZnO or SnO2 are widely used in products which require a textured surface shape. Among these materials, due to high price of ITO, many attempts have been made to find a substitute for ITO. Accordingly, ZnO having the advantages of high electrical conductivity and high transmittance is being developed for both the smooth surface and the textured surface.
Although the technique for manufacturing ZnO is being continuously developed, the surface shape is dependent on the deposition processing. In general, ZnO has a very smooth surface shape due to sputtering deposition, and a texture is formed on the surface of ZnO due to chemical vapor deposition (CVD). In some cases, etching is required in order to form a texture on the surface of ZnO by sputtering depending on characteristics required for a product. This, however, has the problem of increased cost. In addition, process optimization is required in order to form a ZnO thin film having a smooth surface shape by CVD.
The information disclosed in the Background of the Invention section is provided only for better understanding of the background of the invention, and should not be taken as an acknowledgment or any form of suggestion that this information forms a prior art that would already be known to a person skilled in the art.
Various aspects of the present invention provide a method of fabricating a zinc oxide (ZnO) thin film in which the surface shape of the ZnO thin film can be controlled during deposition of the ZnO thin film.
In an aspect of the present invention, provided is a method of fabricating a ZnO thin film that includes depositing the ZnO thin film on a substrate by chemical vapor deposition (CVD). The CVD feeds an etching gas that etches the ZnO thin film concurrently with a source gas and an oxidizer gas, thereby controlling the surface shape of the ZnO thin film that is being deposited.
According to an exemplary embodiment of the invention, the source gas may be composed of a mixture of diethylzinc and a hydrocarbon-based solvent, and the oxidizer gas may be composed of H2O.
Here, the CVD may include feeding the source gas at 1.0 to 9.0 g/min and the oxidizer gas at 0.5 to 5.0 g/min.
The flow rate of the etching gas may be controlled in the range from 1 to 50 sccm.
The etching gas may be implemented as one selected from the group of fluorine-containing gases consisting of CF4, C2F6, C3F6, C3F8 and NF3.
The method may further include preheating the source gas and the oxidizer gas before feeding the source gas and the oxidizer gas into the process chamber where the CVD is carried out.
The CVD may include feeding the source gas and the oxidizer gas into the process chamber along different paths.
Each of the source gas and the oxidizer gas may be carried into the process chamber on a carrier gas that is composed of an inert gas.
In addition, the CVD may include controlling the substrate to pass through a zone where the etching gas is blown, at a velocity of 2 inch/min.
According to embodiments of the invention, it is possible to planarize the surface shape of the ZnO thin film or convert the surface shape of the ZnO thin film into a concave-convex structure through selective etching by concurrently feeding a source gas and an etching gas that are to form a zinc oxide thin film during a CVD process for deposition of a ZnO thin film and controlling the flow rate of the etching gas.
The methods and apparatuses of the present invention have other features and advantages which will be apparent from, or are set forth in greater detail in the accompanying drawings, which are incorporated herein, and in the following Detailed Description of the Invention, which together serve to explain certain principles of the present invention.
Reference will now be made in detail to a method of fabricating a zinc oxide (ZnO) thin film according to the present invention, embodiments of which are illustrated in the accompanying drawings and described below, so that a person having ordinary skill in the art to which the present invention relates can easily put the present invention into practice.
Throughout this document, reference should be made to the drawings, in which the same reference numerals and signs are used throughout the different drawings to designate the same or similar components. In the following description of the present invention, detailed descriptions of known functions and components incorporated herein will be omitted when they may make the subject matter of the present invention unclear.
The method of fabricating a zinc oxide (ZnO) thin film according to the present invention deposits a ZnO thin film on a substrate by a chemical vapor deposition (CVD) process. Here, the CVD process uses a source gas in order to deposit the ZnO thin film. That is, the CVD process is adapted such that a metal source and an oxidizer in a gaseous state undergo a chemical reaction at a certain temperature and are attached to and deposited on a substrate.
Specifically, the CVD process according to an embodiment of the invention includes, first, loading a substrate into a process chamber and then heating the substrate to a certain temperature, for example, approximately 450° C. Here, the substrate can be implemented as a transparent glass substrate.
Afterwards, a source gas and an oxidizer gas that are to be deposited to form a ZnO thin film are blown into the process chamber. According to an embodiment of the invention, a mixture of diethylzinc (DEZn) and a hydrocarbon-based solvent is used as the source gas and H2O vapor is used as the oxidizer gas. Here, in order to prevent the source gas and the oxidizer gas from prematurely mixing before entering the process chamber, it is preferable to control the supply of the source gas and the oxidizer gas along different paths. In addition, the source gas and the oxidizer gas can be heated before being supplied in order to activate a chemical reaction between the source gas and the oxidizer gas. The source gas and the oxidizer gas can be carried into the process chamber on carrier gases that are implemented as an inert gas such as nitrogen, helium or argon.
When the ZnO thin film that is fabricated according to an embodiment of the invention is applied, for example, for a transparent electrode of a photovoltaic cell, electrical conductivity must be ensured. For this, according to an embodiment of the invention, a variety of dopants can be injected into the ZnO thin film that is being deposited. Such a dopant substitutes for Zn or O in the internal lattice of ZnO, thereby improving electrical characteristics of ZnO.
According to an embodiment of the invention, as a scheme for controlling the surface shape of the ZnO thin film that is to be deposited, an etching gas that etches the ZnO thin film is concurrently fed with the source gas and the oxidizer gas that are blown into the process chamber in which the substrate is loaded for ZnO deposition. In this case, according to an embodiment of the invention, the substrate is controlled such that it passes, at a velocity of 2 inch/min, through a zone where these gases are blown.
Here, the flow rate of the etching gas is adjusted in the range from 1 to 50 sccm in the etching gas feed process. In addition, the flow rate of the source gas is adjusted in the range from 1.0 to 9.0 g/min, and the flow rate of the oxidizer gas is adjusted in the range from 0.5 to 5.0g/min. The flow rate of the etching gas can be adjusted while the flow rate of the source gas and the flow rate of the oxidizer gas are being fixed. For example, after the flow rate of the source gas is fixed at 5.5 g/min and the flow rate of the oxidizer gas is fixed at 0.8 g/min, the flow rate of the etching gas can be adjusted within the above-stated range.
As described above, the etching gas is fed together with the source gas and the oxidizer gas, and the flow rate of the etching gas is adjusted. This makes it possible to planarize the surface of the ZnO thin film or form the concave-convex structure, or the texture, on the surface of the ZnO thin film. Furthermore, the degree of planarization or texturing on the surface of the ZnO thin film can be controlled.
Here, the etching gas that is used to control the surface shape of the ZnO thin film is required neither to form a film nor to leave a precipitate through a reaction with the source gas, the oxidizer gas or the dopant. Thus, the etching gas must be implemented as a substance that does not react with the source gas, the oxidizer gas, the dopant, or the like. In addition, the etching gas must be made of a substance that can planarize the surface by selectively etching the surface concaves and convexes or convert the flat surface into the concave-convex structure through selective etching without changing the growth axis of ZnO that is being deposited. Therefore, according to an embodiment of the invention, the etching gas is implemented as one selected from among fluorine-containing gases consisting of CF4, C2F6, C3F6, C3F8 and NF3. The fluorine-containing gases are widely used as a dry etching gas for an indium tin oxide (ITO) or indium zinc oxide (IZO) thin film in semiconductor processes. The fluorine-containing gases are decomposed into F− ions by plasma energy generated by a sputter or reactive ion etching (RIE) equipment to chemically react with a material that is to be etched. After this chemical reaction, halogen group compounds tend to easily break away from the etched material due to their high vapor pressure. According to an embodiment of the invention, the surface shape of the ZnO thin film that is being deposited is controlled using this characteristic of the fluorine-containing gases. When the etching gas selected from among the fluorine-containing gases is concurrently fed with the source gas, a reaction between the etching gas and the ZnO thin film that is being deposited can etch the portions of the ZnO thin film that are in the high energy state and unstable, thereby deforming the surface shape of the ZnO thin film.
A glass substrate was loaded into a process chamber, and then was heated to a temperature of 450° C. A mixture of gaseous DEZn and a hydrocarbon-based solvent was fed at a flow rate of 5.5 g/min and H2O vapor was fed at a flow rate of 2.0 g/min so that a ZnO thin film was deposited on the substrate, and C2F6 was concurrently fed at respective flow rates of 0 sccm (
Referring to these figures, it is noticeable that, while the grain size of the surface concave-convex structure of the ZnO thin film varies depending on the flow rate of C2F6, the end portion of the surface has a hexagonal shape and was grown along the c-axis of the (002) face (
A glass substrate was loaded into a process chamber, and then was heated to a temperature of 450° C. A mixture of gaseous DEZn and a hydrocarbon-based solvent was fed at a flow rate of 5.5 g/min, H2O vapor was fed at a flow rate of 2.0 g/min, and a mixture of tetramethylguanidine (TMG) and triethanolamine (TEA) was fed at a flow rate of 0.4 g/min so that a ZnO thin film was deposited on the substrate, and C2F6 was concurrently fed at respective flow rates of 5 sccm (
Referring to
The foregoing descriptions of specific exemplary embodiments of the present invention have been presented with respect to the drawings. They are not intended to be exhaustive or to limit the invention to the precise forms disclosed, and obviously many modifications and variations are possible for a person having ordinary skill in the art in light of the above teachings.
It is intended therefore that the scope of the invention not be limited to the foregoing embodiments, but be defined by the Claims appended hereto and their equivalents.
Number | Date | Country | Kind |
---|---|---|---|