The present disclosure relates generally to integrated circuit devices, and in a particular embodiment, the present disclosure relates to methods of forming nanocrystal structures using atomic layer deposition and apparatus making use of such nanocrystal structures.
Integrated circuits are interconnected networks of electrical components fabricated on a common foundation called a substrate. The electrical components are typically fabricated on a wafer of semiconductor material that serves as a substrate. Various fabrication techniques, such as layering, doping, masking, and etching, are used to build millions of resistors, transistors, and other electrical components on the wafer. The components are then wired together, or interconnected, to define a specific electrical circuit, such as a processor or a memory device.
There is a general desire to reduce the sizes of the various components in integrated circuit fabrication. Reducing size is generally accompanied by a reduction in cost, as more and more devices can be fabricated on a single substrate, and a reduction in power requirements, as less power is needed to switch smaller components. However, this size reduction does not come without a cost. As integrated circuit devices become smaller and smaller, current or charge leakage and parasitic capacitance between components become increasingly problematic. An example of the detrimental impact of leakage and parasitic capacitance can be seen in flash memory devices.
Flash memory devices are one particular class of memory devices that have developed into a popular source of non-volatile memory for a wide range of electronic applications. Non-volatile memory is memory that can retain its data values for some extended period without the application of power. Flash memory devices typically use a one-transistor memory cell that allows for high memory densities, high reliability, and low power consumption. Changes in threshold voltage of the cells, through programming of a charge storage node, such as a floating gate, or trapping layers or other physical phenomena, determine the data value of each cell. By defining two or more ranges of threshold voltages to correspond to individual data values, one or more bits of information may be stored on each cell. Common uses for flash memory and other non-volatile memory include personal computers, personal digital assistants (PDAs), digital cameras, digital media players, digital recorders, games, appliances, vehicles, wireless devices, mobile telephones and removable memory modules, and the uses for non-volatile memory continue to expand.
For a flash memory device utilizing floating-gate memory cells, where a level of charge stored on the floating-gate affects its threshold voltage, a reduction in size means less volume for charge storage. If the same material were used for the floating gates of two differently sized memory cells, the smaller memory cell would be capable of a smaller difference in its possible threshold voltages than the larger memory cell. And any charge leakage, such as stress-induced gate leakage, would have a larger impact on the threshold voltage of the smaller memory cell. In addition, due to parasitic capacitive coupling to floating gates of adjacent memory cells, more margin is required to avoid a false reading of the data value of the memory cell. Compensating for leakage and parasitic capacitance concerns with a smaller range of threshold voltages makes it increasingly difficult to distinguish between differing data values of smaller memory cells.
For the reasons stated above, and for other reasons that will become apparent to those skilled in the art upon reading and understanding the present specification, there is a need in the art for alternative structures and their processes in the formation of integrated circuit devices.
In the following detailed description of the present embodiments, reference is made to the accompanying drawings that form a part hereof, and in which is shown by way of illustration specific embodiments in which the disclosure may be practiced. These embodiments are described in sufficient detail to enable those skilled in the art to practice the invention, and it is to be understood that other embodiments may be utilized and that process, chemical, electrical or mechanical changes may be made without departing from the scope of the present disclosure. The terms wafer and substrate used previously and in the following description include any base semiconductor structure. Both are to be understood as including silicon-on-sapphire (SOS) technology, silicon-on-insulator (SOI) technology, thin film transistor (TFT) technology, doped and undoped semiconductors, epitaxial layers of silicon supported by a base semiconductor, as well as other semiconductor structures well known to one skilled in the art. Furthermore, when reference is made to a wafer or substrate in the following description, previous process steps may have been utilized to form regions/junctions in the base semiconductor structure. In addition, directional references, e.g., upper, lower, top, bottom and sides, are relative to one another and need not refer to an absolute direction. The following detailed description is, therefore, not to be taken in a limiting sense.
One or more embodiments include nanocrystal structures, methods of forming such nanocrystal structures and apparatus making use of such nanocrystal structures. Formation and use of these nanocrystal structures will be described in the context of their use within a memory device as one example of an integrated circuit device. However, use of these nanocrystal structures is not limited to their use as described with reference to memory devices.
The nanocrystal structures are formed through the use of atomic layer deposition (ALD). ALD, also known as atomic layer epitaxy (ALE) is a form of chemical vapor deposition (CVD) widely used in semiconductor fabrication to form layers of material of very thin dimensions, typically on the atomic scale. The ALD process consists of an alternating series of self-limiting chemical reactions, called half-reactions, between gas-phase precursors and a substrate. The precursors are pulsed into the reactor in a sequential fashion, with purging of precursors in between. A series of these pulse/purge/pulse/purge cycles are used to form a continuous layer of material.
In one or more of the disclosed embodiments, however, instead of completing the ALD process, the process is halted prematurely to leave a discontinuous formation of nanocrystals which are then capped by a different material. For example, an ALD process can be used to form a metal nitride material on a substrate and halted before the metal nitride material forms a continuous layer, followed by the formation of a polysilicon material over the discontinuous metal nitride as a bulk portion to encase the discontinuous metal nitride. The two materials may be of the same type, e.g., both conductors, or may be of differing types, e.g., one insulator and one semiconductor.
Memory device 100 includes an array of memory cells 104 arranged in rows and columns. The memory device 100 and/or processor 130 include nanocrystal structures formed in accordance with an embodiment of this disclosure. For a further embodiment, the array of memory cells 104 include memory cells having a charge storage node or floating gate in accordance with an embodiment of this disclosure. Although various embodiments will be described primarily with reference to NAND memory arrays, the various embodiments are not limited to a specific architecture of the memory array 104. Some examples of other array architectures suitable for the present embodiments include NOR arrays, AND arrays, and virtual ground arrays.
A row decode circuitry 108 and a column decode circuitry 110 are provided to decode address signals. Address signals are received and decoded to access memory array 104. Memory device 100 also includes input/output (I/O) control circuitry 112 to manage input of commands, addresses and data to the memory device 100 as well as output of data and status information from the memory device 100. An address register 114 is coupled between I/O control circuitry 112 and row decode circuitry 108 and column decode circuitry 110 to latch the address signals prior to decoding. A command register 124 is coupled between I/O control circuitry 112 and control logic 116 to latch incoming commands. Control logic 116 controls access to the memory array 104 in response to the commands and generates status information for the external processor 130. The control logic 116 is coupled to row decode circuitry 108 and column decode circuitry 110 to control the row decode circuitry 108 and column decode circuitry 110 in response to the addresses.
Control logic 116 is also coupled to a cache register 118. Cache register 118 latches data, either incoming or outgoing, as directed by control logic 116 to temporarily store data while the memory array 104 is busy writing or reading, respectively, other data. During a write operation, data is passed from the cache register 118 to data register 120 for transfer to the memory array 104; then new data is latched in the cache register 118 from the I/O control circuitry 112. During a read operation, data is passed from the cache register 118 to the I/O control circuitry 112 for output to the external processor 130; then new data is passed from the data register 120 to the cache register 118. A status register 122 is coupled between I/O control circuitry 112 and control logic 116 to latch the status information for output to the processor 130.
Memory device 100 receives control signals at control logic 116 from processor 130 over a control link 132. The control signals may include a chip enable CE#, a command latch enable CLE, an address latch enable ALE, and a write enable WE#. Memory device 100 receives commands (in the form of command signals), addresses (in the form of address signals), and data (in the form of data signals) from processor 130 over a multiplexed input/output (I/O) bus 134 and outputs data to processor 130 over I/O bus 134.
Specifically, the commands are received over input/output (I/O) pins [7:0] of I/O bus 134 at I/O control circuitry 112 and are written into command register 124. The addresses are received over input/output (I/O) pins [7:0] of bus 134 at I/O control circuitry 112 and are written into address register 114. The data are received over input/output (I/O) pins [7:0] for an 8-bit device or input/output (I/O) pins [15:0] for a 16-bit device at I/O control circuitry 112 and are written into cache register 118. The data are subsequently written into data register 120 for programming memory array 104. For another embodiment, cache register 118 may be omitted, and the data are written directly into data register 120. Data are also output over input/output (I/O) pins [7:0] for an 8-bit device or input/output (I/O) pins [15:0] for a 16-bit device. It will be appreciated by those skilled in the art that additional circuitry and signals can be provided, and that the memory device of
Memory array 200 includes NAND strings 2061 to 206M. Each NAND string includes floating-gate transistors 2081 to 208N, each located at an intersection of a word line 202 and a bit line 204. The floating-gate transistors 208 represent non-volatile memory cells for storage of data. The floating-gate transistors 208 of each NAND string 206 are connected in series source to drain between a source select gate 210, e.g., a field-effect transistor (FET), and a drain select gate 212, e.g., an FET. Each source select gate 210 is located at an intersection of a bit line 204 and a source select line 214, while each drain select gate 212 is located at an intersection of a bit line 204 and a drain select line 215.
A source of each source select gate 210 is connected to a common source line 216. The drain of each source select gate 210 is connected to the source of the first floating-gate transistor 208 of the corresponding NAND string 206. For example, the drain of source select gate 2101 is connected to the source of floating-gate transistor 2081 of the corresponding NAND string 2061. A control gate 220 of each source select gate 210 is connected to source select line 214. If multiple source select gates 210 are utilized for a given NAND string 206, they would be coupled in series between the common source line 216 and the first floating-gate transistor 208 of that NAND string 206.
The drain of each drain select gate 212 is connected to a bit line 204 for the corresponding NAND string at a drain contact 228. For example, the drain of drain select gate 2121 is connected to the bit line 2041 for the corresponding NAND string 2061 at drain contact 2281. The source of each drain select gate 212 is connected to the drain of the last floating-gate transistor 208 of the corresponding NAND string 206. For example, the source of drain select gate 2121 is connected to the drain of floating-gate transistor 208N of the corresponding NAND string 2061. If multiple drain select gates 212 are utilized for a given NAND string 206, they would be coupled in series between the corresponding bit line 204 and the last floating-gate transistor 208N of that NAND string 206.
Typical construction of floating-gate transistors 208 includes a source 230 and a drain 232, a floating gate 234, and a control gate 236, as shown in
Floating-gate transistors 308 are located at each intersection of a word line 302 and a local bit line 304. The floating-gate transistors 308 represent non-volatile memory cells for storage of data. Construction of floating-gate transistors 308 includes a source 310 and a drain 312, a floating gate 314, and a control gate 316, as shown in
Floating-gate transistors 308 having their control gates 316 coupled to a word line 302 typically share a common source depicted as array source 318. As shown in
To reduce problems associated with high resistance levels in the array source 318, for example, the array source 318 may be regularly coupled to a metal or other highly conductive line to provide a low-resistance path to ground. The array ground 320 serves as this low-resistance path.
The gate dielectric 410 is formed over an active region of the substrate 405, over which memory cells will be formed. The gate dielectric 410 might be formed by thermal oxidation of the silicon substrate 405. Alternatively, the gate dielectric 410 could be formed by a blanket deposition of a dielectric material, such as by chemical vapor deposition (CVD) or physical vapor deposition (PVD). For one embodiment, gate dielectric 410 contains silicon oxide (SiO2), but may alternatively or additionally include high-K dielectrics such as HfO2, ZnO2, Al2O3, etc.
Source/drain regions 415 are formed in the substrate 405 generally adjacent the gate dielectric 410. A channel region of the memory cell 400 is defined by the area of the substrate 405 between the source/drain regions 415. Source/drain regions 415 will generally have a conductivity type opposite the conductivity type of the substrate 405. For example, for a p-type substrate 405, the source/drain regions 415 might have an n+-type conductivity.
A charge storage node 420 is formed over the gate dielectric 410. The charge storage node 420 is one or more layers capable of storing a charge indicative of a programmed state of the memory cell 400 and containing nanocrystal structures in accordance with embodiments of the disclosure. In general, the nanocrystal structures are formed of conductive materials which are then encapsulated or isolated by a dielectric material. These isolated nanocrystals serve to store charge and can thus collectively be thought of as a floating gate in a floating-gate memory cell. For some embodiments, the nanocrystals contain a metal component. For example, the nanocrystals may be formed of conductive metal nitrides or metal oxides, such as conductive refractory metal nitrides or conductive refractory metal oxides. In one embodiment, the nanocrystals are titanium nitride. As other examples, nanocrystals can be doped semiconductors (doped Ge or Si), pure metals (example Ru, Re, Pt), metal nitrides (TiN, TaN), metal oxides (RuOx), metal alloys (RuAl, RuTi), or metal-alloy-nitrides (ternary nitrides like RuAlN, TaAlN). These could be formed by using specific precursors to control the nanocrystal density during ALD. For example TiN when deposited using a TiCl4 precursor forms a continuous film easily, while when deposited by a metal organic precursor like Ti precursor [Ti(OCH2CH2NMe2)4, Ti(dmae)4] (dmae=dimethylaminoethoxide) forms nanocrystals in the initial stages of growth. However, other molecular structures could be used in the floating gate 420 provided the resulting nanocrystals serve as charge-storage sites within the bulk material. Formation of the charge storage node 420 will be described in more detail with reference to subsequent
The intergate dielectric 425 may be formed over the charge storage node 420. The intergate dielectric 425 contains a dielectric material. For one embodiment, intergate dielectric 425 contains silicon oxide (SiO2), but may alternatively or additionally include high-K dielectrics such as hafnium oxide (HfO2), zirconium oxide (ZrO2), zinc oxide (ZnO2), aluminum oxide (Al2O3), aluminum hafnium oxide (AlHfOx), etc. However, the intergate dielectric 425 may be omitted if the nanocrystals of the charge storage node 420 are sufficiently isolated by dielectric material, such as of the type described for intergate dielectric 425.
A control gate 430 is formed over the intergate dielectric 425, or a dielectric portion of charge storage node 420 if the intergate dielectric 425 is omitted. The control gate 430 is generally one or more layers of conductive material. For one embodiment, the control gate 430 contains a conductively-doped polysilicon. For a further embodiment, the control gate 430 includes a metal-containing layer over a polysilicon layer, e.g., a refractory metal silicide layer formed on a conductively-doped polysilicon layer. The metals of chromium (Cr), cobalt (Co), hafnium (Hf), molybdenum (Mo), niobium (Nb), tantalum (Ta), titanium (Ti), tungsten (W), vanadium (V) and zirconium (Zr) are generally recognized as refractory metals. For another embodiment, the control gate 430 contains multiple metal-containing layers, e.g., a titanium nitride (TiN) barrier layer over the intergate dielectric 425, a titanium (Ti) adhesion layer over the barrier layer and a tungsten (W) layer over the adhesion layer.
A cap 435 is generally formed over the control gate 430 to act as an insulator and barrier layer to protect the control gate 430 during subsequent processing. The cap 435 contains a dielectric material and may include such dielectrics as silicon oxides (SiOx), silicon nitride (SiNx), and silicon oxynitrides (SiOxNy). For one embodiment, the cap 435 is a silicon nitride, formed by such methods as CVD.
The gate stack, i.e., gate dielectric 410, charge storage node 420, intergate dielectric 425 (if used) and control gate 430, along with cap 435, may be patterned to define access lines, i.e., word lines, of a memory device. It is noted that additional layers may form the gate stack, such as barrier layers to inhibit diffusion between opposing layers or adhesion layers to promote adhesion between opposing layers. Sidewall spacers 440 may be formed on the sidewalls of the gate stacks to protect and insulate the sidewalls. Sidewall spacers 440 are typically the same dielectric material as used for the cap 435, but may include other dielectric materials. Formation may include a blanket deposit of a layer of dielectric material on the patterned gate stacks followed by an anisotropic etch to preferentially remove horizontal portions of the layer of dielectric material, leaving vertical portions adjacent the sidewalls of the gate stacks.
The discontinuous portions 5221 and 5222 are each composed of a conductive material. However, the discontinuous portions 5221 may be composed of the same or a different conductive material than the discontinuous portions 5222, and the continuous portion 5241 may be composed of the same or a different dielectric material than the continuous portion 5242. Thus, for each layer of the charge storage node 520B, the material for the discontinuous portions may be chosen independently of the materials of the discontinuous portions of other layers, and the material for the continuous portion may be chosen independently of the materials of the continuous portions of other layers. However, consideration should be given to compatibility of materials that will be in contact with each other, e.g., compatibility between discontinuous portions 5222 and both the continuous portion 5241 and the continuous portion 5242. It is noted that the continuous portion of the uppermost layer, e.g., continuous portion 5242 of layer 5322 in this example, could serve the function of the intergate dielectric 425 of
Note that
In ALD, gaseous precursors are introduced one at a time to the substrate surface mounted within a reactor (e.g., a reaction chamber). This introduction of the gaseous precursors takes the form of sequential pulses of each gaseous precursor. In a pulse of a precursor gas, the precursor gas is made to flow into a specific area or region for a short period of time. Between the pulses, the reaction chamber is purged with a gas, which in many cases is an inert gas, and/or evacuated. The first precursor material be introduced may be called the precursor, and the next material introduced may be called the reactant, but both materials are precursors to the eventual material formed by the ALD reaction, and thus both will be referred to herein as precursors.
In
In
In
For one embodiment, different precursors could be used during different cycles of an ALD process. For example, TiN could be deposited during one or more initial ALD cycles using a large titanium precursor for the first pulsing phase, such as [Ti(OCH2CH2NMe2)4, Ti(dmae)4], to define the nucleation density for TiN islands. Subsequent ALD cycles could then use a smaller titanium precursor for their first pulsing phase, such as TiCl4, to preferentially grow TiN only on the nucleated islands having a pre-defined density. In this example, the nitrogen precursor for the second pulsing phase, such as ammonia, could be the same for both titanium precursors, although different precursors could also be used for different second pulsing phases. Alternatively, smaller precursors could be used during initial ALD cycles to define a higher nucleation density, and subsequent ALD cycles could use a larger precursor to limit further increases in density of the resulting islands.
Using the techniques described herein, the density of nanocrystals formed can reach approximately 1E13/cm2. Such densities are significantly higher than known techniques involving ion implantation or thin-layer deposition, followed by annealing to cause recrystallization. In addition, thermal damage is reduced and/or thermal budget is improved by not requiring an annealing process in the formation of the nanocrystals.
Although specific embodiments have been illustrated and described herein, it will be appreciated by those of ordinary skill in the art that any arrangement that is calculated to achieve the same purpose may be substituted for the specific embodiments shown. Many adaptations of the disclosure will be apparent to those of ordinary skill in the art. Accordingly, this application is intended to cover any adaptations or variations of the disclosure.