The present disclosure generally relates to processes for manufacturing electronic devices. More particularly, the disclosure relates to selectively forming films through cyclic processes such as ALD or sequential/cyclic CVD. Specifically, the disclosure discloses methods to selectively form ALD or sequential/cyclic CVD films with organic reactants.
Water (H2O) has been often used for forming oxides in atomic layer deposition (ALD) processes. Water is a polar molecule due to its lone electron pair. Water is also reactive with many metal halides, which makes it a candidate for some ALD oxide processes. When used as a reactant at low temperatures, however, water has displayed some undesirable behavior.
Most notably, the presence of water as a reactant increases the time to sufficiently purge the tool during an ALD deposition cycle. Specifically, at low temperatures, water tends to stick to various surfaces, including substrates and tools with hydrophilic materials. The sticking of water may make it difficult to purge water from the system and it may cause loss of selectivity if water-based processes are applied on selective deposition schemes. In addition, the nature of water may oxidize some of the surfaces present on the substrate, which in some instances is not desirable.
Prior approaches have described using carboxylic acids for ALD of some metal oxides. However, these have not enabled selective deposition.
As a result, a method for ALD formation of a film that displays efficient purging and effective modification of the surface is desired.
In accordance with at least one embodiment of the invention, a method of selectively forming a metal oxide is disclosed. The method comprises: providing a substrate comprising a dielectric layer and a layer comprising metal for processing in a reaction chamber; exposing the substrate to a metal or semi-metal precursor; exposing the substrate to a purging gas and/or a vacuum; exposing the substrate to an organic reactant; and exposing the substrate to a purging gas and/or the vacuum; wherein a reaction between the metal or semi-metal precursor and the organic reactant selectively forms a metal oxide layer on either the dielectric layer or layer comprising metal. In some embodiments the method of selectively forming a metal oxide comprises a cyclic process using a metal or semi-metal precursor and an organic reactant. In some embodiments the method of selectively forming a metal oxide using a metal or semi-metal precursor and an organic reactant comprises an ALD process. In some embodiments the method of selectively forming a metal oxide process using a metal or semi-metal precursor and an organic reactant comprises a cyclic or sequential CVD process using a metal or semi-metal precursor and an organic reactant. In some embodiments utilizing the cyclic or sequential CVD process, the metal or semi-metal precursor is partly decomposing on the surface. In some embodiments utilizing the cyclic or sequential CVD process, gas-phase reactions of the metal or semi-metal precursor and the organic reactant are substantially avoided. In accordance with exemplary aspects of these embodiments, the selective formation of the metal oxide layer occurs with use of an etchant before and/or after the formation of the metal oxide layer.
For purposes of summarizing the invention and the advantages achieved over the prior art, certain objects and advantages of the invention have been described herein above. Of course, it is to be understood that not necessarily all such objects or advantages may be achieved in accordance with any particular embodiment of the invention. Thus, for example, those skilled in the art will recognize that the invention may be embodied or carried out in a manner that achieves or optimizes one advantage or group of advantages as taught or suggested herein without necessarily achieving other objects or advantages as may be taught or suggested herein.
All of these embodiments are intended to be within the scope of the invention herein disclosed. These and other embodiments will become readily apparent to those skilled in the art from the following detailed description of certain embodiments having reference to the attached figures, the invention not being limited to any particular embodiment(s) disclosed.
These and other features, aspects, and advantages of the invention disclosed herein are described below with reference to the drawings of certain embodiments, which are intended to illustrate and not to limit the invention.
It will be appreciated that elements in the figures are illustrated for simplicity and clarity and have not necessarily been drawn to scale. For example, the dimensions of some of the elements in the figures may be exaggerated relative to other elements to help improve understanding of illustrated embodiments of the present disclosure.
Although certain embodiments and examples are disclosed below, it will be understood by those in the art that the invention extends beyond the specifically disclosed embodiments and/or uses of the invention and obvious modifications and equivalents thereof. Thus, it is intended that the scope of the invention disclosed should not be limited by the particular disclosed embodiments described below.
For selective deposition processes, efficient purging is desirable. Efficient purging may allow for selectivity to take place, as the chemical vapor deposition (CVD) type of gas phase reactions are significantly reduced or absent. Additionally, it is generally desirable for selectivity to have surfaces present with only desired reactivity towards the deposition chemistry. For example, for some surfaces no reaction with the precursors (or reactants) is desired, and for other surfaces quick and complete reactions with the precursors (or reactants) are desired. If not present naturally, surfaces may be modified to exhibit the desired reactivity. For example, some surfaces can be treated to slow down the rate or completely inhibit a certain type of reaction. Surface modifications may be employed when using precursors (or reactants) with undesired reactivity towards a surface present in the system.
When using water as a reactant, the above goal of efficient purging is difficult to achieve. Water molecules are said to be polar because they exhibit an external dipole moment. This causes water to stick easily on surfaces. If water is used in selective deposition schemes, surface modifications may be used to passivate the surfaces against water. One example of such a passivation may include fluorinated or highly methyl covered surfaces, exhibiting high water contact angle. Water contact angle is a measure of the surface energy towards water. Surfaces with high water contact angle are typically passive against water. Additionally, the nature of water makes achieving only the right kind of surface reactivity more difficult, possibly resulting in a desire for surface modifications to protect a formed material, for example. Especially at temperature ranges of 100-150° C., water may prove to be problematic to remove at time scales suitable for production, due to the extended periods of time used to fully purge the water from the system and all the surfaces. Such temperatures may be encountered in many parts of a film deposition tool, outside the film deposition region.
Organic reactants, such as formic acid (HCOOH) or other carboxylic acids, may prove to be a better choice for ALD processes due to their properties. Specifically, organic reactants are not generally polar substances that stick to surfaces. In addition, organic reactants have a different nature when compared to water. Specifically, HCOOH may be able to produce reductive reactions. Additionally, organic reactants such as HCOOH begin decomposing at elevated temperatures and do not liberate H2O at 100-150° C.
In some embodiments, the organic reactant is a vapor phase organic reactant that may demonstrate thermal stability within a range of process temperatures. For example, the vapor phase organic reactant may be thermally stable across a desired range of process temperatures such that growth-disturbing condensable phases do not form on the substrate and/or the vapor phase organic reactant does not generate harmful levels of impurities on the substrate surface through thermal decomposition. In some embodiments, the vapor phase organic reactant may exhibit sufficient vapor pressure such that a desired quantity of chemical molecules is present in the gas phase near the substrate surface to enable the reduction reactions.
In some embodiments, a vapor phase organic reactant may be selected based on its ability to decompose into two or more reactive components, at least one of which can react with the surface.
In some embodiments, the vapor phase organic reactant may comprise formic acid. In some embodiments, the vapor phase organic reactant may comprise acetic acid (CH3COOH) and/or propanoic acid (CH3CH2COOH). In some embodiments, the (e.g., vapor phase) organic reactant may include an alcohol. In some embodiments, the (e.g., vapor phase) organic reactant may include an aldehyde. In some embodiments, the (e.g., vapor phase) organic reactant may have at least one functional group selected from the group consisting of alcohol (—OH), aldehyde (—CHO), and carboxylic acid (—COOH).
Without being limited by any particular theory or mode of operation, the process for depositing metal oxide films selectively using organic reactants may also reduce the metal or metal oxide surfaces present on the substrate. For example, the carboxylic acid may reduce oxidized copper such that the oxidized copper may be restored to its elemental state. In some embodiments, the organic reactant, when used as oxygen source, may keep the metal surface as elemental metal or metallic or conductive state.
Organic reactants containing at least one alcohol group may be preferably selected from the group consisting of primary alcohols, secondary alcohols, tertiary alcohols, polyhydroxy alcohols, cyclic alcohols, aromatic alcohols, and other derivatives of alcohols.
Preferred primary alcohols have an —OH group attached to a carbon atom, which may be bonded to another carbon atom, in particular primary alcohols, according to the general formula (I):
R1—OH (I)
wherein R1 is a linear or branched C1-C20 alkyl or alkenyl groups, preferably methyl, ethyl, propyl, butyl, pentyl or hexyl groups. Examples of preferred primary alcohols include methanol, ethanol, propanol, butanol, 2-methyl propanol and 2-methyl butanol.
Preferred secondary alcohols have an —OH group attached to a carbon atom that is bonded to two other carbon atoms. In particular, preferred secondary alcohols have the general formula (II):
wherein each R1 is selected independently from the group of linear or branched C1-C20 alkyl and alkenyl groups, preferably methyl, ethyl, propyl, butyl, pentyl or hexyl groups. Examples of preferred secondary alcohols include 2-propanol and 2-butanol.
Preferred tertiary alcohols have an —OH group attached to a carbon atom that is bonded to three other carbon atoms. In particular, preferred tertiary alcohols have the general formula (III):
wherein each R1 is selected independently from the group of linear or branched C1-C20 alkyl and alkenyl groups, preferably methyl, ethyl, propyl, butyl, pentyl or hexyl groups. An example of a preferred tertiary alcohol is tert-butanol.
Preferred polyhydroxy alcohols, such as diols and triols, have primary, secondary and/or tertiary alcohol groups as described above. Examples of preferred polyhydroxy alcohol are ethylene glycol and glycerol.
Preferred cyclic alcohols have an —OH group attached to at least one carbon atom which is part of a ring of 1 to 10, more preferably 5-6 carbon atoms.
Preferred aromatic alcohols have at least one —OH group attached either to a benzene ring or to a carbon atom in a side chain.
Preferred reactants containing at least one aldehyde group (—CHO) are selected from the group consisting of compounds having the general formula (V), alkanedial compounds having the general formula (VI), and other derivatives of aldehydes.
Thus, in one embodiment preferred reactants are aldehydes having the general formula (V):
R3—CHO (V)
wherein R3 is selected from the group consisting of hydrogen and linear or branched C1-C20 alkyl and alkenyl groups, preferably methyl, ethyl, propyl, butyl, pentyl or hexyl groups. More preferably, R3 is selected from the group consisting of methyl or ethyl groups. Examples of preferred compounds according to formula (V) are formaldehyde, acetaldehyde and butyraldehyde.
In another embodiment preferred reactants are aldehydes having the general formula (VI):
OHC—R4—CHO (VI)
wherein R4 is a linear or branched C1-C20 saturated or unsaturated hydrocarbon. Alternatively, the aldehyde groups may be directly bonded to each other (R4 is null).
Organic reactants containing at least one —COOH group are preferably selected from the group consisting of compounds of the general formula (VII), polycarboxylic acids, and other derivatives of carboxylic acids.
Thus, in one embodiment, preferred organic reactants may be carboxylic acids having the general formula (VII):
R5—COOH (VII)
wherein R5 is hydrogen or linear or branched C1-C20 alkyl or alkenyl group, preferably methyl, ethyl, propyl, butyl, pentyl or hexyl, more preferably methyl or ethyl groups. In some embodiments, R5 is a linear or branched C1-C3 alkyl or alkenyl group. Examples of preferred compounds according to formula (VII) are formic acid, propanoic acid and acetic acid, most preferably formic acid (HCOOH).
In some embodiments, the organic reactant demonstrates desired vapor pressure such that the organic reactant may be volatized without heating the organic reactant. In some embodiments, such an organic reactant may comprise only one carboxyl group (—COOH).
In some embodiments, the organic reactant may be heated to volatize the organic reactant prior to delivering the volatized organic reactant to the substrate surface. In some embodiments, such an organic reactant may comprise a dicarboxylic acid, including an oxalic acid.
In some embodiments, the organic reactant may comprise less than about 15 weight % water (H2O). In some embodiments, the organic reactant may comprise less than about 5 weight % water, less than about 2 weight % or less than about 1 weight %. For example, the organic reactant may comprise less than about 0.5, less than about 0.1, or less than about 0.05 weight % water. In some embodiments, the organic reactant may not comprise metal. In some embodiments, the organic reactant may comprise only carbon, hydrogen, and oxygen.
As described herein, an organic reactant may decompose into two or more reactive components during the deposition. For example, some of the carboxylic acid delivered to a reaction space may decompose into carbon monoxide (CO) and hydrogen gas (Hz) during the deposition process, such that one or more of the carbon monoxide (CO) and hydrogen gas (H2) may help keep metal or metallic surfaces in its original state, i.e., prevent oxidation of the metal or metallic surfaces, or reduce them to elemental or metallic state. In this way, a substrate surface may be exposed to hydrogen gas (H2) even though no hydrogen gas (H2) is actively provided into the reaction space from an external source.
In some embodiments, the organic reactant may be stored in a liquid phase and subsequently volatized prior to being delivered to the substrate surface. In some embodiments, the organic reactant may be in vapor phase in the reaction space, such that the reaction space is substantially free of any liquid phase reactants. For example, the organic reactant may be in liquid phase during storage and may be subsequently volatized prior to delivery into a reaction chamber, such that only or substantially only organic reactant in the vapor phase is present within the reaction chamber.
In some embodiments, an organic reactant may be stored in a gas bubbler and can be supplied to the reaction chamber from the gas bubbler. In some embodiments, the organic reactant may be stored in a gas bubbler at around room temperature (e.g., from about 20° C. to about 25° C.). For example, the organic reactant gas may be pulsed into the reaction chamber from the gas bubbler during a cycle of the deposition process. In some embodiments, a mass flow rate of the organic reactant may be controlled by controlling the extent to which a valve for delivering the organic reactant into the reactor chamber is kept open (e.g., a needle valve). For example, a mass flow rate may be selected such that a quantity of the organic reactant may be flowed into the reaction chamber during a cycle of the deposition process to facilitate metal surface reduction or protecting the metal surface from being oxidized or facilitate increased selectivity.
Embodiments of the invention may be directed to selectively deposit metal or semi-metal oxide film using an organic reactant source on micrometer-scale (or smaller) features during integrated circuit fabrication. For example, process flows described herein may be used to manufacture features having a size less than 100 micrometers, less than 1 micrometer, or less than 200 nm. In the case of selective deposition of tungsten on copper for interconnects, the size of the feature or line width may be less than 1 micrometer, less than 200 nm, less than 100 nm, or less than 50 nm. One of ordinary skill in the art may recognize that selective deposition on larger features and in other contexts is possible using the disclosed methods.
As mentioned above, the selectivity may be expressed as the ratio of material formed on the first surface (A) minus the amount of material formed on the second surface (B) to amount of material formed on the first surface (A) (i.e., selectivity can be given as a percentage calculated by [(deposition on first surface)−(deposition on second surface)]/(deposition on the first surface) or [(A−B)/A]). Preferably, the selectivity is above about 70%, above about 80%, more preferably above 90%, even more preferably above 95%, or most preferably about 100%. In some cases, selectivity above 80% may be acceptable for certain applications. In some cases, selectivity above 50% may be acceptable for certain applications. In some embodiments, the deposition temperature may be selected such that the selectivity is above about 90%. In some embodiments, the deposition temperature may be selected such that a selectivity of about 100% is achieved.
In some embodiments, the thickness of the film that is selectively deposited may be less than about 100 nm, less than about 50 nm, about 25 nm or less than about 10 nm, in some embodiments, from about 0.5 nm to about 100 nm or from about 1 nm to about 50 nm. However, in some cases a desired level of selectivity, for example more than 50%, more preferably more than 80%, is achieved with the thicknesses of the selectively deposited film being over about 2.5 nm, about 5 nm, over about 10 nm, over about 25 nm or over about 50 nm.
The substrate may comprise various types of materials. When manufacturing integrated circuits, the substrate typically comprises a number of thin films with varying chemical and physical properties. For example and without limitation, the substrate may comprise a silicon-containing layer and a metal layer. In some embodiments, the substrate can comprise metal carbide. In some embodiments, the substrate can comprise a conductive oxide.
In at least one embodiment, the substrate may have a first surface comprising a metal, referred to herein as the first metal surface or first metallic surface. The first surface may be essentially an elemental metal, such as Cu or Co. In other embodiments, the first surface may comprise a metal nitride or a transition metal. The transition metal may be selected from the group: Ti, V, Cr, Mn, Nb, Mo, Ru, Rh, Pd, Ag, Au, Hf, Ta, W, Re, Os, Ir, and Pt. In some embodiments, the first surface may comprise a noble metal, such as Au, Pt, Ir, Pd, Os, Ag, Re, Rh, and Ru, for example. In other embodiments, the metal or semi-metal film deposited using one or more organic reactants as oxygen source may be selectively deposited on a metal oxide surface relative to other surfaces, where the metal oxide surface may be, for example a WOx, HfOx, TiOx, AlOx, or ZrOx surface. In some embodiments, a metal oxide surface may be an oxidized surface of a metallic material.
In at least one embodiment, the substrate may have a second surface which is preferably a silicon containing surface, referred to herein as the second silicon containing surface or second surface comprising silicon. In some embodiments, the silicon containing surface may comprise, for example, SiO2 or surface comprising Si—O bonds. In some embodiments, the second surface may comprise silicon oxide, silicon nitride, silicon carbide, silicon oxynitride, silicon dioxide, or mixtures thereof. In some embodiments, the material comprising the second surface may be a porous material. In some embodiments, the porous material may contain pores which are connected to each other, while in other embodiments, the pores are not connected to each other. In some embodiments, the second surface may comprise a low-k material, defined as an insulator with a dielectric value below about 4.0. In some embodiments, the dielectric value of the low-k material may be below about 3.5, below about 3.0, below about 2.5, or below about 2.3.
Many of the metal oxides that are listed above may be deposited using water as a precursor, but processes in accordance with the present invention may avoid the issues associated using water as a precursor.
The ALD method 200 includes a step of pulsing a metal or semi-metal precursor 210. Metal or semi-metal precursors that may be used in step 210 may include germanium alkylamide, such as germanium dialkylamine, like (Ge(NMe2)4). In some embodiments the metal or semi-metal precursor is a metal halide, such as transition metal halide or for example, aluminum halide, such as aluminum chloride. In some embodiments the metal or semi-metal precursor comprises halide, such as chlorine. In some embodiments the metal or semi-metal precursor is a metal chloride, such as transition metal chloride, such as TiCl4, HfCl4 or ZrCl4. In some embodiments the metal or semi-metal precursor is a metalorganic precursor, such as metalorganic precursor comprising transition metal. In some embodiments the metal or semi-metal precursor is a metal alkylamine precursor, such as Ti(NEtMe)4, Hf(NEtMe)4, or Zr(NEtMe)4. In some embodiments the metal or semi-metal precursor is organometallic precursor, such as alkylaluminum compounds, for example trimethylaluminum (TMA), or such as cyclopentadienyl compounds of Ti, Hf or Zr, for example, (pentamethylcyclopentadienyl)trimethoxytitanium (Me5Cp)Ti(OMe)3, bis(methylcyclopentadienyl)methoxymethylhafnium (MeCp)2Hf(OMe)Me or tris(dimethylamino)cyclopentadienylzirconium CpZr(NMe2)3. The pulse step 210 may take place for a time duration ranging between 0.01 and 60 seconds, from about 0.1 to about 30 seconds or from about 0.2 to about 10 seconds at temperatures ranging between about 0 to about 750° C., from about 50 to about 500° C., or from about 150 and 350° C. Step 210 may then be followed by a purge step 220, which would remove any excess metal or semi-metal precursors.
A number of different Ge precursors can be used in the deposition processes. In some embodiments the Ge precursor is tetravalent (i.e. Ge has an oxidation state of +IV). In some embodiments, the Ge precursor is not divalent (i.e., Ge has an oxidation state of +II). In some embodiments, the Ge precursor may comprise at least one alkoxide ligand. In some embodiments, the Ge precursor may comprise at least one amine or alkylamine ligand. In some embodiments the Ge precursor is a metal-organic or organometallic compound. In some embodiments the Ge precursor comprises at least one halide ligand. In some embodiments the Ge precursor does not comprise a halide ligand.
For example, Ge precursors from formulas VIII-X below may be used in some embodiments:
Ge(NRIRII)4 (VIII)
wherein RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and RII can be independently selected from the group consisting of alkyl and substituted alkyl;
Ge(NRIRII)x-A4-x (IX)
wherein the x is an integer from 1 to 4; RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and RII can be independently selected from the group consisting of alkyl and substituted alkyl; A can be independently selected from the group consisting of alkyl, alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines, halide, and hydrogen;
Gen(NRIRII)2n+2 (X)
wherein the n is an integer from 1 to 3; RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and RII can be independently selected from the group consisting of alkyl and substituted alkyl.
The ALD method 200 may also include a step of pulsing an organic reactant 230. Organic reactant may include formic acid (HCOOH), any simple carboxylic acid, or any precursor that might decompose into CO, CO2, or any other by-product species, and H2O, or any other organic precursor noted herein. For example, a step 230 pulsing formic acid (and/or another organic reactant) may use a purity of organic reactant, such as formic acid and/or other organic reactant of at least 90%, more preferably at least 95%, and more preferably at least 98%, in order to obtain a properly deposited layer. The pulse step 230 may take place for a time duration ranging between 0.01 and 60 seconds, from about 0.1 to about 30 seconds or from about 0.2 to about 10 seconds at a temperature range ranging between about 0 to about 750° C., from about 50 to about 500 C or from about 150 and 350° C. Step 230 may then be followed by a purge step 240, which would remove any excess organic reactant(s). The steps of the ALD method 200 may be repeated to form an oxide layer of a desired thickness. In some embodiments, the purge step of the organic reactant(s) may be less than about 10 seconds, less than about 5 seconds, less than about 2 seconds, less than about 1 second, less than about 0.5 seconds while still retaining selective deposition. In some embodiments, the same degree of selectivity may not be retained if a water or other oxygen source than an organic reactant is used. While the exemplary pulse and purge times mentioned above may be applicable to many different types of reactors, single wafer, or mini-batch reactors, pulse and purge times may be higher in case of batch reactors with high surface areas. Any of the purge steps as discussed herein can use an inert gas, such nitrogen and/or a noble gas, such as argon and/or helium.
The ALD method 200 enables selective deposition on a substrate comprising at least two different surfaces, for example, a first surface comprising metal, such as Cu, and second surface comprising silicon, such as silicon dioxide or low-k material. As a result, for example, a metal oxide film can be formed on the dielectric material, while the metal surface can remain uncovered or vice versa. In addition, there may be more efficient purging of the carboxylic acid or other organic reactant due to its lower polarity in comparison to water. The use of ozone (O3) or oxygen plasma or oxygen atoms or oxygen radicals may be avoided due to its tendency to oxidize metals or metallic materials or surfaces easily as well as destroying the selectivity. In some embodiments, plasma may not be used in the deposition process. Although described in connection with ALD processing, method 200 can similarly be performed using sequential/cyclic CVD.
In some embodiments, the selective deposited film using organic reactant may have a growth rate of less than about 5 Å/cycle, less than about 2.5 Å/cycle, less than about 1.5 Å/cycle or less than about 1.0 Å/cycle. In other embodiments the selective deposited film using organic reactant has a growth rate from about 0.01 to about 5 Å/cycle, from about 0.05 to about 2.5 Å/cycle or from about 0.1 to about 2 Å/cycle.
The ALD method 300 may include a step of pulsing an organic reactant 310. Organic reactants may include formic acid (HCOOH), any simple carboxylic acid, or any precursor that might decompose into CO, CO2, or any other by-product species and H2O, or other organic reactant as described herein. For example, a step 310 pulsing formic acid or other organic reactant may use a purity of formic acid or other organic reactant of at least 90%, at least 95%, and more preferably at least 98% in order to obtain a properly deposited layer. The pulse step 310 may take place for a time duration ranging between 0.01 and 60 seconds, from about 0.1 to about 30 seconds, or from about 0.2 to about 10 seconds at temperatures ranging between 0 and 750° C., between 50 and 500° C., or between 150 and 350° C. Step 310 may then be followed by a purge step 320, which would remove any excess organic reactants.
The steps of the ALD method 300 may be repeated to form an oxide layer of a desired thickness. In some embodiments, the purge step of the organic reactant may be less than about 10 seconds, less than about 5 seconds, less than about 2 seconds, less than about 1 second, less than about 0.5 seconds while still retaining selective deposition. In some embodiments, the same degree of selectivity may not be retained if a water or other oxygen source than the organic reactant is used. While the exemplary pulse and purge times mentioned above may be applicable to many different types of reactors, single wafer, or mini-batch reactors, pulse and purge times may be higher in case of batch reactors with high surface areas.
The ALD method 300 includes a step of pulsing a metal or semi-metal precursor 330. Metal or semi-metal precursors that may be used in step 330 may include germanium alkylamide, such as germanium dialkylamine like (Ge(NMe2)4), for example. The pulse step 330 may take place for a time duration ranging between 0.01 and 60 seconds, from about 0.1 to about 30 seconds, or from about 0.2 to about 10 seconds at temperatures ranging between about 0 to about 750° C., from about 50 to about 500° C., or from about 150 and 350° C. Step 330 may then be followed by a purge step 340, which would remove any excess metal or semi-metal precursors. The steps of the ALD method 300 may be repeated to form an oxide layer of a desired thickness.
The ALD method 300 enables selective deposition on a substrate comprising at least two different surfaces, for example, a first surface comprising metal, such as Cu, and second surface comprising silicon, such as silicon dioxide or low-k silicon. As a result, for example, a metal oxide film can be formed on the dielectric, while the metal surface can remain uncovered or vice versa. In addition, there may be more efficient purging of the carboxylic acid reactant due to its lower polarity in comparison to water. The use of ozone (O3), oxygen plasma, oxygen atoms, or oxygen radicals may be avoided due to its tendency to oxidize metals or metallic materials or surfaces easily as well as destroying the selectivity. In some embodiments, plasma may not be used in the deposition process.
The ALD method 300 may modify the metal surface of the substrate. For example, the carboxylic acid (or other organic reactant) may reduce a metallic surface or elemental metal, such as copper oxide (CuO), surface to metallic or elemental metal, such as elemental copper. In addition, the carboxylic acid may remove any remaining passivation layer on the metal surface, such as benzotriazole (BTA). Both of these effects are benefits because removal of the passivation layer or reduction to straight copper may both be capable of enabling selective growth. Similar to method 200, method 300 may be a cyclic CVC process, rather than an ALD process.
Quality of the metal oxide layer deposited through either ALD method 200 or ALD method 300 may be judged by a selectivity of a surface of the metal oxide layer. For example, the selectivity may be quantified by a thickness of the metal oxide layer in relation to thickness deposited on the desired layer.
The particular implementations shown and described are illustrative of the invention and its best mode and are not intended to otherwise limit the scope of the aspects and implementations in any way. Indeed, for the sake of brevity, conventional manufacturing, connection, preparation, and other functional aspects of the system may not be described in detail. Furthermore, the connecting lines shown in the various figures are intended to represent exemplary functional relationships and/or physical couplings between the various elements. Many alternative or additional functional relationship or physical connections may be present in the practical system, and/or may be absent in some embodiments.
It is to be understood that the configurations and/or approaches described herein are exemplary in nature, and that these specific embodiments or examples are not to be considered in a limiting sense, because numerous variations are possible. The specific routines or methods described herein may represent one or more of any number of processing strategies. Thus, the various acts illustrated may be performed in the sequence illustrated, in other sequences, or omitted in some cases.
The subject matter of the present disclosure includes all novel and nonobvious combinations and subcombinations of the various processes, systems, and configurations, and other features, functions, acts, and/or properties disclosed herein, as well as any and all equivalents thereof.
| Number | Name | Date | Kind |
|---|---|---|---|
| D30036 | Rhind | Jan 1899 | S |
| D31889 | Gill | Nov 1899 | S |
| D56051 | Cohn | Aug 1920 | S |
| 2059480 | Obermaier | Nov 1936 | A |
| 2161626 | Loughner et al. | Jun 1939 | A |
| 2266416 | Duclos | Dec 1941 | A |
| 2280778 | Anderson | Apr 1942 | A |
| 2410420 | Bennett | Nov 1946 | A |
| 2563931 | Harrison | Aug 1951 | A |
| 2660061 | Lewis | Nov 1953 | A |
| 2745640 | Cushman | May 1956 | A |
| 2990045 | Root | Sep 1959 | A |
| 3038951 | Mead | Jun 1962 | A |
| 3089507 | Drake et al. | May 1963 | A |
| 3094396 | Flugge et al. | Jun 1963 | A |
| 3232437 | Hultgren | Feb 1966 | A |
| 3263502 | Springfield | Aug 1966 | A |
| 3410349 | Troutman | Nov 1968 | A |
| 3588192 | Drutchas et al. | Jun 1971 | A |
| 3647387 | Benson | Mar 1972 | A |
| 3647716 | Koches | Mar 1972 | A |
| 3713899 | Sebestyen | Jan 1973 | A |
| 3718429 | Williamson | Feb 1973 | A |
| 3833492 | Bollyky | Sep 1974 | A |
| 3854443 | Baerg | Dec 1974 | A |
| 3862397 | Anderson et al. | Jan 1975 | A |
| 3867205 | Schley | Feb 1975 | A |
| 3885504 | Baermann | May 1975 | A |
| 3887790 | Ferguson | Jun 1975 | A |
| 3904371 | Neti | Sep 1975 | A |
| 3913058 | Nishio et al. | Oct 1975 | A |
| 3913617 | van Laar | Oct 1975 | A |
| 3947685 | Meinel | Mar 1976 | A |
| 3960559 | Suzuki | Jun 1976 | A |
| 3997638 | Manning et al. | Dec 1976 | A |
| 4054071 | Patejak | Oct 1977 | A |
| 4058430 | Suntola et al. | Nov 1977 | A |
| 4093491 | Whelpton et al. | Jun 1978 | A |
| D249341 | Mertz | Sep 1978 | S |
| 4126027 | Smith et al. | Nov 1978 | A |
| 4134425 | Gussefeld et al. | Jan 1979 | A |
| 4145699 | Hu et al. | Mar 1979 | A |
| 4164959 | Wurzburger | Aug 1979 | A |
| 4176630 | Elmer | Dec 1979 | A |
| 4181330 | Kojima | Jan 1980 | A |
| 4194536 | Stine et al. | Mar 1980 | A |
| 4217463 | Swearingen | Aug 1980 | A |
| 4234449 | Wolson et al. | Nov 1980 | A |
| 4322592 | Martin | Mar 1982 | A |
| 4333735 | Hardy | Jun 1982 | A |
| 4355912 | Haak | Oct 1982 | A |
| 4389973 | Suntola et al. | Jun 1983 | A |
| 4393013 | McMenamin | Jul 1983 | A |
| 4401507 | Engle | Aug 1983 | A |
| 4414492 | Hanlet | Nov 1983 | A |
| 4436674 | McMenamin | Mar 1984 | A |
| 4444990 | Villar | Apr 1984 | A |
| 4454370 | Voznick | Jun 1984 | A |
| 4455193 | Jeuch et al. | Jun 1984 | A |
| 4466766 | Geren et al. | Aug 1984 | A |
| 4479831 | Sandow | Oct 1984 | A |
| 4499354 | Hill et al. | Feb 1985 | A |
| 4512113 | Budinger | Apr 1985 | A |
| 4527005 | McKelvey et al. | Jul 1985 | A |
| 4537001 | Uppstrom | Aug 1985 | A |
| 4548688 | Mathews | Oct 1985 | A |
| 4570328 | Price et al. | Feb 1986 | A |
| 4575636 | Caprari | Mar 1986 | A |
| 4578560 | Tanaka et al. | Mar 1986 | A |
| 4579378 | Snyders | Apr 1986 | A |
| 4579623 | Suzuki et al. | Apr 1986 | A |
| 4590326 | Woldy | May 1986 | A |
| 4611966 | Johnson | Sep 1986 | A |
| 4620998 | Lalvani | Nov 1986 | A |
| D288556 | Wallgren | Mar 1987 | S |
| 4653541 | Oehlschlaeger et al. | Mar 1987 | A |
| 4654226 | Jackson et al. | Mar 1987 | A |
| 4664769 | Cuomo et al. | May 1987 | A |
| 4681134 | Paris | Jul 1987 | A |
| 4718637 | Contin | Jan 1988 | A |
| 4721533 | Phillippi et al. | Jan 1988 | A |
| 4722298 | Rubin et al. | Feb 1988 | A |
| 4724272 | Raniere et al. | Feb 1988 | A |
| 4735259 | Vincent | Apr 1988 | A |
| 4749416 | Greenspan | Jun 1988 | A |
| 4753192 | Goldsmith et al. | Jun 1988 | A |
| 4753856 | Haluska et al. | Jun 1988 | A |
| 4756794 | Yoder | Jul 1988 | A |
| 4771015 | Kanai | Sep 1988 | A |
| 4780169 | Stark et al. | Oct 1988 | A |
| 4789294 | Sato et al. | Dec 1988 | A |
| 4821674 | deBoer et al. | Apr 1989 | A |
| 4827430 | Aid et al. | May 1989 | A |
| 4830515 | Cortes | May 1989 | A |
| 4837113 | Luttmer et al. | Jun 1989 | A |
| 4837185 | Yau et al. | Jun 1989 | A |
| 4854263 | Chang et al. | Aug 1989 | A |
| 4854266 | Simson et al. | Aug 1989 | A |
| 4857137 | Tachi et al. | Aug 1989 | A |
| 4857382 | Liu et al. | Aug 1989 | A |
| 4882199 | Sadoway et al. | Nov 1989 | A |
| 4916091 | Freeman et al. | Apr 1990 | A |
| 4934831 | Volbrecht | Jun 1990 | A |
| 4949848 | Kos | Aug 1990 | A |
| D311126 | Crowley | Oct 1990 | S |
| 4976996 | Monkowski et al. | Dec 1990 | A |
| 4978567 | Miller | Dec 1990 | A |
| 4984904 | Nakano et al. | Jan 1991 | A |
| 4985114 | Okudaira | Jan 1991 | A |
| 4986215 | Yamada | Jan 1991 | A |
| 4987856 | Hey | Jan 1991 | A |
| 4989992 | Piai | Feb 1991 | A |
| 4991614 | Hammel | Feb 1991 | A |
| 5013691 | Lory et al. | May 1991 | A |
| 5027746 | Frijlink | Jul 1991 | A |
| 5028366 | Harakal et al. | Jul 1991 | A |
| 5057436 | Ball | Oct 1991 | A |
| 5060322 | Delepine | Oct 1991 | A |
| 5061083 | Grimm et al. | Oct 1991 | A |
| 5062386 | Christensen | Nov 1991 | A |
| 5065698 | Koike | Nov 1991 | A |
| 5071258 | Usher et al. | Dec 1991 | A |
| 5074017 | Toya et al. | Dec 1991 | A |
| 5098638 | Sawada | Mar 1992 | A |
| 5098865 | Machado | Mar 1992 | A |
| 5104514 | Quartarone | Apr 1992 | A |
| 5108192 | Mailliet et al. | Apr 1992 | A |
| 5116018 | Friemoth et al. | May 1992 | A |
| D327534 | Manville | Jun 1992 | S |
| 5119760 | McMillan et al. | Jun 1992 | A |
| 5130003 | Conrad | Jul 1992 | A |
| 5137286 | Whitford | Aug 1992 | A |
| 5154301 | Kos | Oct 1992 | A |
| 5158128 | Inoue et al. | Oct 1992 | A |
| 5167716 | Boitnott et al. | Dec 1992 | A |
| 5176451 | Sasada | Jan 1993 | A |
| 5178682 | Tsukamoto et al. | Jan 1993 | A |
| 5181779 | Shia et al. | Jan 1993 | A |
| 5183511 | Yamazaki et al. | Feb 1993 | A |
| 5192717 | Kawakami | Mar 1993 | A |
| 5194401 | Adams et al. | Mar 1993 | A |
| 5199603 | Prescott | Apr 1993 | A |
| 5213650 | Wang et al. | May 1993 | A |
| 5221556 | Hawkins et al. | Jun 1993 | A |
| 5225366 | Yoder et al. | Jul 1993 | A |
| 5226383 | Bhat | Jul 1993 | A |
| 5228114 | Suzuki | Jul 1993 | A |
| 5242539 | Kumihashi et al. | Sep 1993 | A |
| 5243195 | Nishi | Sep 1993 | A |
| 5243202 | Mori et al. | Sep 1993 | A |
| 5246218 | Yap et al. | Sep 1993 | A |
| 5246500 | Samata et al. | Sep 1993 | A |
| 5259881 | Edwards et al. | Nov 1993 | A |
| 5266526 | Aoyama | Nov 1993 | A |
| 5271967 | Kramer et al. | Dec 1993 | A |
| 5278494 | Obigane | Jan 1994 | A |
| 5284519 | Gadgil | Feb 1994 | A |
| 5288684 | Yamazaki et al. | Feb 1994 | A |
| 5294778 | Carman et al. | Mar 1994 | A |
| 5306666 | Izumi | Apr 1994 | A |
| 5306946 | Yamamoto | Apr 1994 | A |
| 5310456 | Kadomura | May 1994 | A |
| 5314570 | Ikegaya et al. | May 1994 | A |
| 5315092 | Takahashi et al. | May 1994 | A |
| 5326427 | Jerbic | Jul 1994 | A |
| 5336327 | Lee | Aug 1994 | A |
| 5354580 | Goela et al. | Oct 1994 | A |
| 5356478 | Chen et al. | Oct 1994 | A |
| 5356672 | Schmitt et al. | Oct 1994 | A |
| 5360269 | Ogawa et al. | Nov 1994 | A |
| 5364667 | Rhieu | Nov 1994 | A |
| D353452 | Groenhoff | Dec 1994 | S |
| 5374315 | Deboer et al. | Dec 1994 | A |
| 5380367 | Bertone | Jan 1995 | A |
| 5382311 | Ishikawa et al. | Jan 1995 | A |
| 5388945 | Garric et al. | Feb 1995 | A |
| 5404082 | Hernandez et al. | Apr 1995 | A |
| 5407449 | Zinger | Apr 1995 | A |
| 5413813 | Cruse et al. | May 1995 | A |
| 5414221 | Gardner | May 1995 | A |
| 5415753 | Hurwitt et al. | May 1995 | A |
| 5421893 | Perlov | Jun 1995 | A |
| 5422139 | Fischer | Jun 1995 | A |
| 5423942 | Robbins et al. | Jun 1995 | A |
| 5430011 | Tanaka et al. | Jul 1995 | A |
| 5444217 | Moore | Aug 1995 | A |
| 5453124 | Moslehi et al. | Sep 1995 | A |
| 5494494 | Mizuno et al. | Feb 1996 | A |
| 5496408 | Motoda et al. | Mar 1996 | A |
| 5501740 | Besen et al. | Mar 1996 | A |
| 5503875 | Imai et al. | Apr 1996 | A |
| 5504042 | Cho et al. | Apr 1996 | A |
| 5514439 | Sibley | May 1996 | A |
| 5518549 | Hellwig | May 1996 | A |
| 5523616 | Yasuhide | Jun 1996 | A |
| 5527111 | Lysen et al. | Jun 1996 | A |
| 5527417 | Iida et al. | Jun 1996 | A |
| 5531835 | Fodor et al. | Jul 1996 | A |
| 5540898 | Davidson | Jul 1996 | A |
| 5558717 | Zhao et al. | Sep 1996 | A |
| 5559046 | Oishi et al. | Sep 1996 | A |
| 5574247 | Nishitani et al. | Nov 1996 | A |
| 5576629 | Turner | Nov 1996 | A |
| 5577331 | Suzuki | Nov 1996 | A |
| 5583736 | Anderson et al. | Dec 1996 | A |
| 5589002 | Su | Dec 1996 | A |
| 5589110 | Motoda et al. | Dec 1996 | A |
| 5595606 | Fujikawa et al. | Jan 1997 | A |
| 5601641 | Stephens | Feb 1997 | A |
| 5604410 | Vollkommer et al. | Feb 1997 | A |
| 5616264 | Nishi et al. | Apr 1997 | A |
| 5616947 | Tamura | Apr 1997 | A |
| 5621982 | Yamashita | Apr 1997 | A |
| 5632919 | MacCracken et al. | May 1997 | A |
| D380527 | Velez | Jul 1997 | S |
| 5656093 | Burkhart et al. | Aug 1997 | A |
| 5663899 | Zvonar et al. | Sep 1997 | A |
| 5665608 | Chapple-Sokol et al. | Sep 1997 | A |
| 5679215 | Barnes et al. | Oct 1997 | A |
| 5681779 | Pasch et al. | Oct 1997 | A |
| 5683517 | Shan | Nov 1997 | A |
| 5695567 | Kordina | Dec 1997 | A |
| 5697706 | Ciaravino et al. | Dec 1997 | A |
| 5700729 | Lee et al. | Dec 1997 | A |
| 5708825 | Sotomayor | Jan 1998 | A |
| 5711811 | Suntola et al. | Jan 1998 | A |
| 5716133 | Hosokawa et al. | Feb 1998 | A |
| 5718574 | Shimazu | Feb 1998 | A |
| D392855 | Pillow | Mar 1998 | S |
| 5724748 | Brooks | Mar 1998 | A |
| 5728223 | Murakarni et al. | Mar 1998 | A |
| 5730801 | Tepman et al. | Mar 1998 | A |
| 5732744 | Barr et al. | Mar 1998 | A |
| 5736314 | Hayes et al. | Apr 1998 | A |
| 5753835 | Gustin | May 1998 | A |
| 5761328 | Solberg et al. | Jun 1998 | A |
| 5777838 | Tamagawa et al. | Jul 1998 | A |
| 5779203 | Edlinger | Jul 1998 | A |
| 5781693 | Balance et al. | Jul 1998 | A |
| 5782979 | Kaneno | Jul 1998 | A |
| 5791782 | Wooten et al. | Aug 1998 | A |
| 5792272 | Van Os et al. | Aug 1998 | A |
| 5796074 | Edelstein et al. | Aug 1998 | A |
| 5801104 | Schuegraf et al. | Sep 1998 | A |
| 5806980 | Berrian | Sep 1998 | A |
| 5813851 | Nakao | Sep 1998 | A |
| 5819092 | Ferguson et al. | Oct 1998 | A |
| 5819434 | Herchen et al. | Oct 1998 | A |
| 5827435 | Seiji | Oct 1998 | A |
| 5827757 | Robinson, Jr. et al. | Oct 1998 | A |
| 5836483 | Disel | Nov 1998 | A |
| 5837058 | Chen et al. | Nov 1998 | A |
| 5837320 | Hampden-Smith et al. | Nov 1998 | A |
| 5844683 | Pavloski et al. | Dec 1998 | A |
| 5846332 | Zhao et al. | Dec 1998 | A |
| 5851294 | Young et al. | Dec 1998 | A |
| 5852879 | Schumaier | Dec 1998 | A |
| 5853484 | Jeong | Dec 1998 | A |
| 5855680 | Soininen et al. | Jan 1999 | A |
| 5855681 | Maydan et al. | Jan 1999 | A |
| 5857777 | Schuh | Jan 1999 | A |
| 5863123 | Lee | Jan 1999 | A |
| 5865205 | Wilmer | Feb 1999 | A |
| 5873942 | Park | Feb 1999 | A |
| 5877095 | Tamura et al. | Mar 1999 | A |
| 5879128 | Tietz et al. | Mar 1999 | A |
| 5884640 | Fishkin et al. | Mar 1999 | A |
| D409894 | McClurg | May 1999 | S |
| 5908672 | Ryu | Jun 1999 | A |
| 5916365 | Sherman | Jun 1999 | A |
| D412270 | Fredrickson | Jul 1999 | S |
| 5920798 | Higuchi et al. | Jul 1999 | A |
| 5937323 | Orczyk et al. | Aug 1999 | A |
| 5947718 | Weaver | Sep 1999 | A |
| 5954375 | Trickle et al. | Sep 1999 | A |
| 5961775 | Fujimura | Oct 1999 | A |
| 5968275 | Lee et al. | Oct 1999 | A |
| 5970621 | Bazydola | Oct 1999 | A |
| 5975492 | Brenes | Nov 1999 | A |
| 5979506 | Aarseth | Nov 1999 | A |
| 5982931 | Ishimaru | Nov 1999 | A |
| 5984391 | Vanderpot et al. | Nov 1999 | A |
| 5987480 | Donohue et al. | Nov 1999 | A |
| 5997588 | Goodwin | Dec 1999 | A |
| 5997768 | Scully | Dec 1999 | A |
| 5998870 | Lee et al. | Dec 1999 | A |
| 6001267 | Van Os et al. | Dec 1999 | A |
| D419652 | Hall et al. | Jan 2000 | S |
| 6013553 | Wallace | Jan 2000 | A |
| 6013920 | Gordon et al. | Jan 2000 | A |
| 6015465 | Kholodenko et al. | Jan 2000 | A |
| 6017779 | Miyasaka | Jan 2000 | A |
| 6017818 | Lu | Jan 2000 | A |
| 6024799 | Chen | Feb 2000 | A |
| 6035101 | Sajoto et al. | Mar 2000 | A |
| 6042652 | Hyun | Mar 2000 | A |
| 6044860 | Nue | Apr 2000 | A |
| 6045260 | Schwartz et al. | Apr 2000 | A |
| 6048154 | Wytman | Apr 2000 | A |
| 6050506 | Guo et al. | Apr 2000 | A |
| 6054678 | Miyazaki | Apr 2000 | A |
| 6060691 | Minami et al. | May 2000 | A |
| 6060721 | Huang | May 2000 | A |
| 6068441 | Raaijmakers et al. | May 2000 | A |
| 6072163 | Armstrong | Jun 2000 | A |
| 6073973 | Boscaljon et al. | Jun 2000 | A |
| 6074443 | Venkatesh | Jun 2000 | A |
| 6083321 | Lei et al. | Jul 2000 | A |
| 6086677 | Umotoy et al. | Jul 2000 | A |
| 6091062 | Pfahnl et al. | Jul 2000 | A |
| 6093252 | Wengert et al. | Jul 2000 | A |
| 6093253 | Lofgren | Jul 2000 | A |
| 6096267 | Kishkovich | Aug 2000 | A |
| 6099302 | Hong et al. | Aug 2000 | A |
| 6102565 | Kita et al. | Aug 2000 | A |
| 6104011 | Juliano | Aug 2000 | A |
| 6104401 | Parsons | Aug 2000 | A |
| 6106678 | Shufflebotham | Aug 2000 | A |
| 6119710 | Brown | Sep 2000 | A |
| 6121061 | Van Bilsen et al. | Sep 2000 | A |
| 6121158 | Benchikha et al. | Sep 2000 | A |
| 6122036 | Yamasaki et al. | Sep 2000 | A |
| 6124600 | Moroishi et al. | Sep 2000 | A |
| 6125789 | Gupta et al. | Oct 2000 | A |
| 6126848 | Li et al. | Oct 2000 | A |
| 6129044 | Zhao et al. | Oct 2000 | A |
| 6129546 | Sada | Oct 2000 | A |
| 6134807 | Komino | Oct 2000 | A |
| 6137240 | Bogdan et al. | Oct 2000 | A |
| 6140252 | Cho et al. | Oct 2000 | A |
| 6148761 | Majewski et al. | Nov 2000 | A |
| 6158941 | Muka et al. | Dec 2000 | A |
| 6160244 | Ohashi | Dec 2000 | A |
| 6161500 | Kopacz et al. | Dec 2000 | A |
| 6162323 | Koshimizu et al. | Dec 2000 | A |
| 6174809 | Kang et al. | Jan 2001 | B1 |
| 6178918 | Van Os et al. | Jan 2001 | B1 |
| 6180979 | Hofman et al. | Jan 2001 | B1 |
| 6187672 | Zhao | Feb 2001 | B1 |
| 6187691 | Fukuda | Feb 2001 | B1 |
| 6190634 | Lieber et al. | Feb 2001 | B1 |
| 6191399 | Van Bilsen | Feb 2001 | B1 |
| 6194037 | Terasaki et al. | Feb 2001 | B1 |
| 6201999 | Jevtic | Mar 2001 | B1 |
| 6203613 | Gates et al. | Mar 2001 | B1 |
| 6207932 | Yoo | Mar 2001 | B1 |
| 6212789 | Kato | Apr 2001 | B1 |
| 6214122 | Thompson | Apr 2001 | B1 |
| 6217658 | Orczyk et al. | Apr 2001 | B1 |
| 6218288 | Li et al. | Apr 2001 | B1 |
| 6225020 | Jung et al. | May 2001 | B1 |
| 6235858 | Swarup et al. | May 2001 | B1 |
| 6242359 | Misra | Jun 2001 | B1 |
| 6243654 | Johnson et al. | Jun 2001 | B1 |
| 6245665 | Yokoyama | Jun 2001 | B1 |
| 6247245 | Ishii | Jun 2001 | B1 |
| 6250250 | Maishev et al. | Jun 2001 | B1 |
| 6257758 | Culbertson | Jul 2001 | B1 |
| 6264467 | Andreas et al. | Jul 2001 | B1 |
| 6271148 | Kao | Aug 2001 | B1 |
| 6274878 | Li et al. | Aug 2001 | B1 |
| 6281098 | Wang | Aug 2001 | B1 |
| 6281141 | Das et al. | Aug 2001 | B1 |
| 6284050 | Shi et al. | Sep 2001 | B1 |
| 6287965 | Kang et al. | Sep 2001 | B1 |
| 6293700 | Lund et al. | Sep 2001 | B1 |
| D449873 | Bronson | Oct 2001 | S |
| 6296909 | Spitsberg | Oct 2001 | B1 |
| 6299133 | Waragai et al. | Oct 2001 | B2 |
| 6302964 | Umotoy et al. | Oct 2001 | B1 |
| 6303523 | Cheung | Oct 2001 | B2 |
| 6305898 | Yamagishi et al. | Oct 2001 | B1 |
| 6311016 | Yanagawa et al. | Oct 2001 | B1 |
| 6312525 | Bright et al. | Nov 2001 | B1 |
| 6315512 | Tabrizi et al. | Nov 2001 | B1 |
| 6316162 | Jung et al. | Nov 2001 | B1 |
| 6321680 | Cook et al. | Nov 2001 | B2 |
| D451893 | Robson | Dec 2001 | S |
| D452220 | Robson | Dec 2001 | S |
| 6325858 | Wengert | Dec 2001 | B1 |
| 6326597 | Lubomirsky et al. | Dec 2001 | B1 |
| 6329297 | Balish | Dec 2001 | B1 |
| 6342427 | Choi et al. | Jan 2002 | B1 |
| 6344084 | Koinuma et al. | Feb 2002 | B1 |
| 6344232 | Jones et al. | Feb 2002 | B1 |
| 6347636 | Xia | Feb 2002 | B1 |
| 6350391 | Livshits et al. | Feb 2002 | B1 |
| 6352945 | Matsuki | Mar 2002 | B1 |
| D455024 | Mimick et al. | Apr 2002 | S |
| 6367410 | Leahey et al. | Apr 2002 | B1 |
| 6368773 | Jung et al. | Apr 2002 | B1 |
| 6368987 | Kopacz et al. | Apr 2002 | B1 |
| 6370796 | Zucker | Apr 2002 | B1 |
| 6372583 | Tyagi | Apr 2002 | B1 |
| 6374831 | Chandran | Apr 2002 | B1 |
| 6375312 | Ikeda et al. | Apr 2002 | B1 |
| 6375750 | Van Os et al. | Apr 2002 | B1 |
| D457609 | Piano | May 2002 | S |
| 6383566 | Zagdoun | May 2002 | B1 |
| 6383955 | Matsuki | May 2002 | B1 |
| 6387207 | Janakiraman | May 2002 | B1 |
| 6391803 | Kim et al. | May 2002 | B1 |
| 6395650 | Callegari et al. | May 2002 | B1 |
| 6398184 | Sowada et al. | Jun 2002 | B1 |
| 6410459 | Blalock et al. | Jun 2002 | B2 |
| 6413321 | Kim et al. | Jul 2002 | B1 |
| 6413583 | Moghadam et al. | Jul 2002 | B1 |
| 6420279 | Ono et al. | Jul 2002 | B1 |
| D461233 | Whalen | Aug 2002 | S |
| D461882 | Piano | Aug 2002 | S |
| 6432849 | Endo et al. | Aug 2002 | B1 |
| 6435798 | Satoh | Aug 2002 | B1 |
| 6435865 | Tseng et al. | Aug 2002 | B1 |
| 6436819 | Zhang | Aug 2002 | B1 |
| 6437444 | Andideh | Aug 2002 | B2 |
| 6438502 | Awtrey | Aug 2002 | B1 |
| 6441350 | Stoddard et al. | Aug 2002 | B1 |
| 6445574 | Saw et al. | Sep 2002 | B1 |
| 6446573 | Hirayama et al. | Sep 2002 | B2 |
| 6447232 | Davis et al. | Sep 2002 | B1 |
| 6447651 | Ishikawa et al. | Sep 2002 | B1 |
| 6448192 | Kaushik | Sep 2002 | B1 |
| 6450757 | Saeki | Sep 2002 | B1 |
| 6451713 | Tay et al. | Sep 2002 | B1 |
| 6454860 | Metzner et al. | Sep 2002 | B2 |
| 6455225 | Kong et al. | Sep 2002 | B1 |
| 6455445 | Matsuki | Sep 2002 | B2 |
| 6461435 | Littau et al. | Oct 2002 | B1 |
| 6461436 | Campbell et al. | Oct 2002 | B1 |
| 6468924 | Lee | Oct 2002 | B2 |
| 6471779 | Nishio et al. | Oct 2002 | B1 |
| 6472266 | Yu et al. | Oct 2002 | B1 |
| 6475276 | Elers et al. | Nov 2002 | B1 |
| 6475930 | Junker et al. | Nov 2002 | B1 |
| 6478872 | Chae et al. | Nov 2002 | B1 |
| 6482331 | Lu et al. | Nov 2002 | B2 |
| 6482663 | Buckland | Nov 2002 | B1 |
| 6483989 | Okada et al. | Nov 2002 | B1 |
| 6494065 | Babbitt | Dec 2002 | B2 |
| 6494998 | Brcka | Dec 2002 | B1 |
| 6496819 | Bello et al. | Dec 2002 | B1 |
| 6499533 | Yamada | Dec 2002 | B2 |
| 6503079 | Kogano et al. | Jan 2003 | B2 |
| 6503562 | Saito et al. | Jan 2003 | B1 |
| 6503826 | Oda | Jan 2003 | B1 |
| 6506253 | Sakuma | Jan 2003 | B2 |
| 6507410 | Robertson et al. | Jan 2003 | B1 |
| 6511539 | Raaijmakers | Jan 2003 | B1 |
| 6514313 | Spiegelman | Feb 2003 | B1 |
| 6514666 | Choi et al. | Feb 2003 | B1 |
| 6521295 | Remington | Feb 2003 | B1 |
| 6521547 | Chang et al. | Feb 2003 | B1 |
| 6528430 | Kwan | Mar 2003 | B2 |
| 6528767 | Bagley et al. | Mar 2003 | B2 |
| 6531193 | Fonash et al. | Mar 2003 | B2 |
| 6531412 | Conti et al. | Mar 2003 | B2 |
| 6534133 | Kaloyeros et al. | Mar 2003 | B1 |
| 6534395 | Werkhoven et al. | Mar 2003 | B2 |
| 6536950 | Green | Mar 2003 | B1 |
| 6540469 | Matsunaga et al. | Apr 2003 | B2 |
| 6544906 | Rotondaro et al. | Apr 2003 | B2 |
| 6552209 | Lei et al. | Apr 2003 | B1 |
| 6558755 | Berry et al. | May 2003 | B2 |
| 6559026 | Rossman et al. | May 2003 | B1 |
| 6566278 | Harvey et al. | May 2003 | B1 |
| 6569239 | Arai et al. | May 2003 | B2 |
| 6569971 | Roh et al. | May 2003 | B2 |
| 6573030 | Fairbairn et al. | Jun 2003 | B1 |
| 6574644 | Hsu et al. | Jun 2003 | B2 |
| 6576062 | Matsuse | Jun 2003 | B2 |
| 6576064 | Griffiths et al. | Jun 2003 | B2 |
| 6576300 | Berry et al. | Jun 2003 | B1 |
| 6576564 | Agarwal | Jun 2003 | B2 |
| 6578589 | Mayusumi | Jun 2003 | B1 |
| 6579833 | McNallan et al. | Jun 2003 | B1 |
| 6580050 | Miller et al. | Jun 2003 | B1 |
| 6583048 | Vincent et al. | Jun 2003 | B1 |
| 6589707 | Lee et al. | Jul 2003 | B2 |
| 6589868 | Rossman | Jul 2003 | B2 |
| 6590251 | Kang et al. | Jul 2003 | B2 |
| 6594550 | Okrah | Jul 2003 | B1 |
| 6596653 | Tan | Jul 2003 | B2 |
| 6598559 | Vellore et al. | Jul 2003 | B1 |
| 6607868 | Choi | Aug 2003 | B2 |
| 6607948 | Sugiyama et al. | Aug 2003 | B1 |
| 6608745 | Tsuruta et al. | Aug 2003 | B2 |
| 6620251 | Kitano | Sep 2003 | B2 |
| 6624064 | Sahin | Sep 2003 | B1 |
| 6627268 | Fair et al. | Sep 2003 | B1 |
| 6627503 | Ma et al. | Sep 2003 | B2 |
| 6632478 | Gaillard et al. | Oct 2003 | B2 |
| 6633364 | Hayashi | Oct 2003 | B2 |
| 6635117 | Kinnard et al. | Oct 2003 | B1 |
| 6638839 | Deng et al. | Oct 2003 | B2 |
| 6645304 | Yamaguchi | Nov 2003 | B2 |
| 6648974 | Ogliari et al. | Nov 2003 | B1 |
| 6649921 | Cekic et al. | Nov 2003 | B1 |
| 6652924 | Sherman | Nov 2003 | B2 |
| 6656281 | Ueda | Dec 2003 | B1 |
| 6660662 | Ishikawa et al. | Dec 2003 | B2 |
| 6662817 | Yamagishi | Dec 2003 | B2 |
| 6673196 | Oyabu | Jan 2004 | B1 |
| 6676290 | Lu | Jan 2004 | B1 |
| 6682971 | Tsuneda et al. | Jan 2004 | B2 |
| 6682973 | Paton et al. | Jan 2004 | B1 |
| D486891 | Cronce | Feb 2004 | S |
| 6684659 | Tanaka et al. | Feb 2004 | B1 |
| 6688784 | Templeton | Feb 2004 | B1 |
| 6689220 | Nguyen | Feb 2004 | B1 |
| 6692575 | Omstead et al. | Feb 2004 | B1 |
| 6692576 | Halpin et al. | Feb 2004 | B2 |
| 6699003 | Saeki | Mar 2004 | B2 |
| 6699399 | Qian et al. | Mar 2004 | B1 |
| 6709989 | Ramdani et al. | Mar 2004 | B2 |
| 6710364 | Guldi et al. | Mar 2004 | B2 |
| 6710857 | Kondo | Mar 2004 | B2 |
| 6713824 | Mikata | Mar 2004 | B1 |
| 6716571 | Gabriel | Apr 2004 | B2 |
| 6720260 | Fair et al. | Apr 2004 | B1 |
| 6722837 | Inui | Apr 2004 | B2 |
| 6723642 | Lim et al. | Apr 2004 | B1 |
| 6730614 | Lim et al. | May 2004 | B1 |
| 6732006 | Haanstra et al. | May 2004 | B2 |
| 6734090 | Agarwala et al. | May 2004 | B2 |
| 6740853 | Johnson et al. | May 2004 | B1 |
| 6743475 | Skarp et al. | Jun 2004 | B2 |
| 6743738 | Todd et al. | Jun 2004 | B2 |
| 6745095 | Ben-Dov | Jun 2004 | B1 |
| 6753507 | Fure et al. | Jun 2004 | B2 |
| 6755221 | Jeong et al. | Jun 2004 | B2 |
| 6756085 | Waldfried | Jun 2004 | B2 |
| 6756293 | Li et al. | Jun 2004 | B2 |
| 6756318 | Nguyen et al. | Jun 2004 | B2 |
| 6759098 | Han | Jul 2004 | B2 |
| 6760981 | Leap | Jul 2004 | B2 |
| 6784108 | Donohoe et al. | Aug 2004 | B1 |
| D497977 | Engelbrektsson | Nov 2004 | S |
| 6811960 | Lee et al. | Nov 2004 | B2 |
| 6815350 | Kim et al. | Nov 2004 | B2 |
| 6820570 | Kilpela et al. | Nov 2004 | B2 |
| 6821910 | Adomaitis et al. | Nov 2004 | B2 |
| 6824665 | Shelnut et al. | Nov 2004 | B2 |
| 6825134 | Law et al. | Nov 2004 | B2 |
| 6828235 | Takano | Dec 2004 | B2 |
| 6831004 | Byun | Dec 2004 | B2 |
| 6835039 | Van Den Berg | Dec 2004 | B2 |
| 6846146 | Inui | Jan 2005 | B2 |
| 6846515 | Vrtis | Jan 2005 | B2 |
| 6846742 | Rossman | Jan 2005 | B2 |
| 6847014 | Benjamin et al. | Jan 2005 | B1 |
| 6858524 | Haukka et al. | Feb 2005 | B2 |
| 6858547 | Metzner | Feb 2005 | B2 |
| 6863019 | Shamouilian | Mar 2005 | B2 |
| 6863281 | Endou et al. | Mar 2005 | B2 |
| 6864041 | Brown | Mar 2005 | B2 |
| 6872258 | Park et al. | Mar 2005 | B2 |
| 6872259 | Strang | Mar 2005 | B2 |
| 6874247 | Hsu | Apr 2005 | B1 |
| 6874480 | Ismailov | Apr 2005 | B1 |
| 6875677 | Conley, Jr. et al. | Apr 2005 | B1 |
| 6876017 | Goodner | Apr 2005 | B2 |
| 6878402 | Chiang et al. | Apr 2005 | B2 |
| 6884066 | Nguyen et al. | Apr 2005 | B2 |
| 6884295 | Ishii | Apr 2005 | B2 |
| 6884319 | Kim | Apr 2005 | B2 |
| D505590 | Greiner | May 2005 | S |
| 6889211 | Yoshiura et al. | May 2005 | B1 |
| 6889864 | Lindfors et al. | May 2005 | B2 |
| 6895158 | Alyward et al. | May 2005 | B2 |
| 6899507 | Yamagishi et al. | May 2005 | B2 |
| 6909839 | Wang et al. | Jun 2005 | B2 |
| 6911092 | Sneh | Jun 2005 | B2 |
| 6913152 | Zuk | Jul 2005 | B2 |
| 6913796 | Albano et al. | Jul 2005 | B2 |
| 6917755 | Nguyen et al. | Jul 2005 | B2 |
| 6924078 | Lee et al. | Aug 2005 | B2 |
| 6929700 | Tan et al. | Aug 2005 | B2 |
| 6930041 | Agarwal | Aug 2005 | B2 |
| 6930059 | Conley, Jr. et al. | Aug 2005 | B2 |
| 6935269 | Lee et al. | Aug 2005 | B2 |
| 6939817 | Sandhu et al. | Sep 2005 | B2 |
| 6942753 | Choi et al. | Sep 2005 | B2 |
| 6951587 | Narushima | Oct 2005 | B1 |
| 6953609 | Carollo | Oct 2005 | B2 |
| 6955836 | Kumagai et al. | Oct 2005 | B2 |
| 6972055 | Sferlazzo | Dec 2005 | B2 |
| 6972478 | Waite et al. | Dec 2005 | B1 |
| 6974781 | Timmermans et al. | Dec 2005 | B2 |
| 6975921 | Verhaar | Dec 2005 | B2 |
| 6976822 | Woodruff | Dec 2005 | B2 |
| 6981832 | Zinger et al. | Jan 2006 | B2 |
| 6982046 | Srivastava et al. | Jan 2006 | B2 |
| 6984595 | Yamazaki | Jan 2006 | B1 |
| 6985788 | Haanstra et al. | Jan 2006 | B2 |
| 6987155 | Roh et al. | Jan 2006 | B2 |
| 6990430 | Hosek | Jan 2006 | B2 |
| 7005227 | Yueh et al. | Feb 2006 | B2 |
| 7005391 | Min | Feb 2006 | B2 |
| 7010580 | Fu et al. | Mar 2006 | B1 |
| 7017514 | Shepherd et al. | Mar 2006 | B1 |
| 7018941 | Cui et al. | Mar 2006 | B2 |
| 7021881 | Yamagishi | Apr 2006 | B2 |
| 7036453 | Ishikawa et al. | May 2006 | B2 |
| 7041609 | Vaartstra | May 2006 | B2 |
| 7045430 | Ahn et al. | May 2006 | B2 |
| 7049247 | Gates et al. | May 2006 | B2 |
| 7053009 | Conley, Jr. et al. | May 2006 | B2 |
| 7055875 | Bonora | Jun 2006 | B2 |
| 7062161 | Kusuda et al. | Jun 2006 | B2 |
| 7070178 | Van Der Toorn et al. | Jul 2006 | B2 |
| 7071051 | Jeon et al. | Jul 2006 | B1 |
| 7073834 | Matsumoto et al. | Jul 2006 | B2 |
| 7080545 | Dimeo et al. | Jul 2006 | B2 |
| 7084060 | Furukawa | Aug 2006 | B1 |
| 7084079 | Conti et al. | Aug 2006 | B2 |
| 7085623 | Siegers | Aug 2006 | B2 |
| 7088003 | Gates et al. | Aug 2006 | B2 |
| 7090394 | Hashikura et al. | Aug 2006 | B2 |
| 7092287 | Beulens et al. | Aug 2006 | B2 |
| 7098149 | Lukas | Aug 2006 | B2 |
| 7101763 | Anderson et al. | Sep 2006 | B1 |
| 7109098 | Ramaswamy et al. | Sep 2006 | B1 |
| 7109114 | Chen et al. | Sep 2006 | B2 |
| 7111232 | Bascom | Sep 2006 | B1 |
| 7115305 | Bronikowski et al. | Oct 2006 | B2 |
| 7115838 | Kurara et al. | Oct 2006 | B2 |
| 7122085 | Shero et al. | Oct 2006 | B2 |
| 7122222 | Xiao et al. | Oct 2006 | B2 |
| 7129165 | Basol et al. | Oct 2006 | B2 |
| 7132360 | Schaeffer et al. | Nov 2006 | B2 |
| 7135421 | Ahn et al. | Nov 2006 | B2 |
| 7143897 | Guzman et al. | Dec 2006 | B1 |
| 7147766 | Uzoh et al. | Dec 2006 | B2 |
| 7153542 | Nguyen et al. | Dec 2006 | B2 |
| 7156380 | Soininen | Jan 2007 | B2 |
| 7163393 | Adachi et al. | Jan 2007 | B2 |
| 7163721 | Zhang et al. | Jan 2007 | B2 |
| 7163900 | Weber | Jan 2007 | B2 |
| 7168852 | Linnarsson | Jan 2007 | B2 |
| 7172497 | Basol et al. | Feb 2007 | B2 |
| 7186648 | Rozbicki | Mar 2007 | B1 |
| 7192824 | Ahn et al. | Mar 2007 | B2 |
| 7192892 | Ahn et al. | Mar 2007 | B2 |
| 7195693 | Cowans | Mar 2007 | B2 |
| 7198447 | Morimitsu et al. | Apr 2007 | B2 |
| 7201943 | Park et al. | Apr 2007 | B2 |
| 7204887 | Kawamura et al. | Apr 2007 | B2 |
| 7205246 | MacNeil et al. | Apr 2007 | B2 |
| 7205247 | Lee et al. | Apr 2007 | B2 |
| 7207763 | Lee | Apr 2007 | B2 |
| 7208389 | Tipton et al. | Apr 2007 | B1 |
| 7210925 | Adachi | May 2007 | B2 |
| 7211524 | Ryu et al. | May 2007 | B2 |
| 7211525 | Shanker | May 2007 | B1 |
| 7214630 | Varadarajan et al. | May 2007 | B1 |
| 7223014 | Lojen | May 2007 | B2 |
| 7208413 | Byun et al. | Jun 2007 | B2 |
| 7234476 | Arai | Jun 2007 | B2 |
| 7235137 | Kitayama et al. | Jun 2007 | B2 |
| 7235482 | Wu | Jun 2007 | B2 |
| 7235501 | Ahn et al. | Jun 2007 | B2 |
| 7238596 | Kouvetakis et al. | Jul 2007 | B2 |
| 7238616 | Agarwal | Jul 2007 | B2 |
| 7238653 | Lee et al. | Jul 2007 | B2 |
| 7265061 | Cho et al. | Sep 2007 | B1 |
| 7274867 | Peukert | Sep 2007 | B2 |
| D553104 | Oohashi et al. | Oct 2007 | S |
| 7279256 | Son | Oct 2007 | B2 |
| 7290813 | Bonora | Nov 2007 | B2 |
| 7294581 | Haverkort et al. | Nov 2007 | B2 |
| 7296460 | Dimeo et al. | Nov 2007 | B2 |
| 7297641 | Todd et al. | Nov 2007 | B2 |
| 7298009 | Yan et al. | Nov 2007 | B2 |
| D557226 | Uchino et al. | Dec 2007 | S |
| 7307028 | Goto et al. | Dec 2007 | B2 |
| 7307178 | Kiyomori et al. | Dec 2007 | B2 |
| 7312148 | Ramaswamy et al. | Dec 2007 | B2 |
| 7312162 | Ramaswamy et al. | Dec 2007 | B2 |
| 7312494 | Ahn et al. | Dec 2007 | B2 |
| 7320544 | Hsieh | Jan 2008 | B2 |
| 7323401 | Ramaswamy et al. | Jan 2008 | B2 |
| 7326657 | Xia et al. | Feb 2008 | B2 |
| 7327948 | Shrinivasan | Feb 2008 | B1 |
| 7329947 | Adachi et al. | Feb 2008 | B2 |
| 7335611 | Ramaswamy et al. | Feb 2008 | B2 |
| 7351057 | Berenbak et al. | Apr 2008 | B2 |
| 7354847 | Chan et al. | Apr 2008 | B2 |
| 7354873 | Fukazawa et al. | Apr 2008 | B2 |
| 7356762 | van Driel | Apr 2008 | B2 |
| 7357138 | Ji et al. | Apr 2008 | B2 |
| 7361447 | Jung | Apr 2008 | B2 |
| 7376520 | Wong | May 2008 | B2 |
| 7379785 | Higashi et al. | May 2008 | B2 |
| 7381644 | Soubramonium et al. | Jun 2008 | B1 |
| 7387685 | Choi et al. | Jun 2008 | B2 |
| 7393207 | Imai | Jul 2008 | B2 |
| 7393418 | Yokogawa | Jul 2008 | B2 |
| 7393736 | Ahn et al. | Jul 2008 | B2 |
| 7393765 | Hanawa et al. | Jul 2008 | B2 |
| 7396491 | Marking et al. | Jul 2008 | B2 |
| 7399388 | Moghadam et al. | Jul 2008 | B2 |
| 7399570 | Lee et al. | Jul 2008 | B2 |
| 7402534 | Mahajani | Jul 2008 | B2 |
| 7405166 | Liang et al. | Jul 2008 | B2 |
| 7405454 | Ahn et al. | Jul 2008 | B2 |
| D575713 | Ratcliffe | Aug 2008 | S |
| 7410290 | Tanaka | Aug 2008 | B2 |
| 7410666 | Elers | Aug 2008 | B2 |
| 7411352 | Madocks | Aug 2008 | B2 |
| 7414281 | Fastow | Aug 2008 | B1 |
| D576001 | Brunderman | Sep 2008 | S |
| 7422635 | Zheng et al. | Sep 2008 | B2 |
| 7422653 | Blahnik et al. | Sep 2008 | B2 |
| 7422775 | Ramaswamy et al. | Sep 2008 | B2 |
| 7429532 | Ramaswamy et al. | Sep 2008 | B2 |
| 7431966 | Derderian et al. | Oct 2008 | B2 |
| 7432476 | Morita et al. | Oct 2008 | B2 |
| 7437060 | Wang et al. | Oct 2008 | B2 |
| 7442275 | Cowans | Oct 2008 | B2 |
| 7467632 | Lee et al. | Dec 2008 | B2 |
| 7475588 | Dimeo et al. | Jan 2009 | B2 |
| 7476291 | Wang et al. | Jan 2009 | B2 |
| 7479198 | Guffrey | Jan 2009 | B2 |
| 7482247 | Papasouliotis | Jan 2009 | B1 |
| 7482283 | Yamasaki et al. | Jan 2009 | B2 |
| D585968 | Elkins et al. | Feb 2009 | S |
| 7489389 | Shibazaki et al. | Feb 2009 | B2 |
| 7494882 | Vitale | Feb 2009 | B2 |
| 7497614 | Gaff | Mar 2009 | B2 |
| 7498242 | Kumar et al. | Mar 2009 | B2 |
| 7501292 | Matsushita et al. | Mar 2009 | B2 |
| 7501355 | Bhatia et al. | Mar 2009 | B2 |
| 7503980 | Kida et al. | Mar 2009 | B2 |
| D590933 | Vansell | Apr 2009 | S |
| 7514375 | Shanker et al. | Apr 2009 | B1 |
| D593969 | Li | Jun 2009 | S |
| 7541297 | Mallick et al. | Jun 2009 | B2 |
| 7547363 | Tomiyasu et al. | Jun 2009 | B2 |
| 7547633 | Ranish et al. | Jun 2009 | B2 |
| 7550396 | Frohberg et al. | Jun 2009 | B2 |
| 7561982 | Rund et al. | Jul 2009 | B2 |
| 7563715 | Haukka et al. | Jul 2009 | B2 |
| 7566891 | Rocha-Alvarez et al. | Jul 2009 | B2 |
| 7575968 | Sadaka et al. | Aug 2009 | B2 |
| 7579285 | Zimmerman et al. | Aug 2009 | B2 |
| 7579785 | Shinmen et al. | Aug 2009 | B2 |
| D600223 | Aggarwal | Sep 2009 | S |
| 7582555 | Lang | Sep 2009 | B1 |
| 7582575 | Fukazawa et al. | Sep 2009 | B2 |
| 7589003 | Kouvetakis et al. | Sep 2009 | B2 |
| 7589029 | Derderian et al. | Sep 2009 | B2 |
| 7591601 | Matsuoka et al. | Sep 2009 | B2 |
| D602575 | Breda | Oct 2009 | S |
| 7598513 | Kouvetakis et al. | Oct 2009 | B2 |
| 7601223 | Lindfors et al. | Oct 2009 | B2 |
| 7601225 | Tuominen et al. | Oct 2009 | B2 |
| 7601652 | Singh et al. | Oct 2009 | B2 |
| 7611751 | Elers | Nov 2009 | B2 |
| 7611980 | Wells et al. | Nov 2009 | B2 |
| 7618226 | Takizawa | Nov 2009 | B2 |
| 7621672 | Ripley | Nov 2009 | B2 |
| 7622369 | Lee et al. | Nov 2009 | B1 |
| 7622378 | Liu et al. | Nov 2009 | B2 |
| 7623940 | Huskamp et al. | Nov 2009 | B2 |
| D606952 | Lee | Dec 2009 | S |
| 7625820 | Papasouliotis | Dec 2009 | B1 |
| 7629277 | Ghatnagar | Dec 2009 | B2 |
| 7632549 | Goundar | Dec 2009 | B2 |
| 7640142 | Tachikawa et al. | Dec 2009 | B2 |
| 7645341 | Kennedy et al. | Jan 2010 | B2 |
| 7645484 | Ishizaka | Jan 2010 | B2 |
| 7648927 | Singh et al. | Jan 2010 | B2 |
| 7651269 | Comendant | Jan 2010 | B2 |
| 7651583 | Kent et al. | Jan 2010 | B2 |
| 7651955 | Ravish et al. | Jan 2010 | B2 |
| 7651959 | Fukazawa et al. | Jan 2010 | B2 |
| 7651961 | Clark | Jan 2010 | B2 |
| D609652 | Nagasaka | Feb 2010 | S |
| D609655 | Sugimoto | Feb 2010 | S |
| 7661299 | Kusunoki | Feb 2010 | B2 |
| 7678197 | Maki | Mar 2010 | B2 |
| 7678715 | Mungekar et al. | Mar 2010 | B2 |
| 7682454 | Sneh | Mar 2010 | B2 |
| 7682657 | Sherman | Mar 2010 | B2 |
| D613829 | Griffin et al. | Apr 2010 | S |
| D614153 | Fondurulia et al. | Apr 2010 | S |
| D614267 | Breda | Apr 2010 | S |
| D614268 | Breda | Apr 2010 | S |
| D614593 | Lee | Apr 2010 | S |
| 7690881 | Yamagishi | Apr 2010 | B2 |
| 7691205 | Ikedo | Apr 2010 | B2 |
| 7692171 | Kaszuba et al. | Apr 2010 | B2 |
| 7695808 | Tuma | Apr 2010 | B2 |
| 7713874 | Milligan | May 2010 | B2 |
| 7716993 | Ozawa et al. | May 2010 | B2 |
| 7720560 | Menser et al. | May 2010 | B2 |
| 7723648 | Tsukamoto et al. | May 2010 | B2 |
| 7727864 | Elers | Jun 2010 | B2 |
| 7732343 | Niroomand et al. | Jun 2010 | B2 |
| 7736437 | Cadwell et al. | Jun 2010 | B2 |
| 7736528 | Okita et al. | Jun 2010 | B2 |
| 7740437 | de Ridder et al. | Jun 2010 | B2 |
| 7740705 | Li | Jun 2010 | B2 |
| 7745346 | Hausmann et al. | Jun 2010 | B2 |
| 7748760 | Kushida | Jul 2010 | B2 |
| 7749563 | Zheng et al. | Jul 2010 | B2 |
| 7753584 | Gambino et al. | Jul 2010 | B2 |
| 7754621 | Putjkonen | Jul 2010 | B2 |
| 7763869 | Matsushita et al. | Jul 2010 | B2 |
| 7767262 | Clark | Aug 2010 | B2 |
| 7771796 | Kohno et al. | Aug 2010 | B2 |
| 7780440 | Shibagaki et al. | Aug 2010 | B2 |
| 7781352 | Fukazawa et al. | Aug 2010 | B2 |
| 7789559 | Waser et al. | Sep 2010 | B2 |
| 7789965 | Matsushita et al. | Sep 2010 | B2 |
| 7790633 | Tarafdar et al. | Sep 2010 | B1 |
| 7798096 | Mahajani et al. | Sep 2010 | B2 |
| 7803722 | Liang | Sep 2010 | B2 |
| 7806587 | Kobayashi | Oct 2010 | B2 |
| 7807566 | Tsuji et al. | Oct 2010 | B2 |
| 7807578 | Bencher et al. | Oct 2010 | B2 |
| 7816278 | Reed et al. | Oct 2010 | B2 |
| 7824492 | Tois et al. | Nov 2010 | B2 |
| 7825040 | Fukazawa et al. | Nov 2010 | B1 |
| 7829460 | Streck et al. | Nov 2010 | B2 |
| 7833353 | Furukawahara et al. | Nov 2010 | B2 |
| 7838084 | Derderian et al. | Nov 2010 | B2 |
| 7842518 | Miyajima | Nov 2010 | B2 |
| 7842622 | Lee et al. | Nov 2010 | B1 |
| D629874 | Hermans | Dec 2010 | S |
| 7850449 | Yang et al. | Dec 2010 | B2 |
| 7851019 | Tuominen et al. | Dec 2010 | B2 |
| 7851232 | van Schravendijk et al. | Dec 2010 | B2 |
| 7858519 | Liu et al. | Dec 2010 | B2 |
| 7858533 | Liu et al. | Dec 2010 | B2 |
| 7865070 | Nakamura | Jan 2011 | B2 |
| 7871198 | Rempe et al. | Jan 2011 | B2 |
| 7874726 | Jacobs et al. | Jan 2011 | B2 |
| 7884918 | Hattori | Feb 2011 | B2 |
| 7888233 | Gauri | Feb 2011 | B1 |
| D634329 | Wastrom | Mar 2011 | S |
| D634719 | Yasuda et al. | Mar 2011 | S |
| 7897215 | Fair et al. | Mar 2011 | B1 |
| 7897217 | Faguet | Mar 2011 | B2 |
| 7902582 | Forbes et al. | Mar 2011 | B2 |
| 7906174 | Wu et al. | Mar 2011 | B1 |
| 7910288 | Abatchev et al. | Mar 2011 | B2 |
| 7915139 | Lang | Mar 2011 | B1 |
| 7915667 | Knoefler et al. | Mar 2011 | B2 |
| 7919416 | Lee et al. | Apr 2011 | B2 |
| 7925378 | Gilchrist et al. | Apr 2011 | B2 |
| 7935940 | Smargiassi | May 2011 | B1 |
| 7939447 | Bauer et al. | May 2011 | B2 |
| 7942969 | Riker et al. | May 2011 | B2 |
| 7946762 | Yednak | May 2011 | B2 |
| 7951262 | Koshiishi et al. | May 2011 | B2 |
| 7955516 | Chandrachood et al. | Jun 2011 | B2 |
| 7955650 | Tsuji | Jun 2011 | B2 |
| 7957708 | Karschnia et al. | Jun 2011 | B2 |
| 7963736 | Takizawa et al. | Jun 2011 | B2 |
| 7967913 | Hua et al. | Jun 2011 | B2 |
| 7972980 | Lee et al. | Jul 2011 | B2 |
| 7977256 | Liu et al. | Jul 2011 | B2 |
| 7981751 | Zhu et al. | Jul 2011 | B2 |
| D643055 | Takahashi | Aug 2011 | S |
| 7989736 | Park et al. | Aug 2011 | B2 |
| 7992318 | Kawaji | Aug 2011 | B2 |
| 7994721 | Espiau et al. | Aug 2011 | B2 |
| 7997795 | Schwagerman et al. | Aug 2011 | B2 |
| 7998875 | DeYoung | Aug 2011 | B2 |
| 8003174 | Fukazawa | Aug 2011 | B2 |
| 8003919 | Goto et al. | Aug 2011 | B2 |
| 8004198 | Bakre et al. | Aug 2011 | B2 |
| 8020315 | Nishimura | Sep 2011 | B2 |
| 8030129 | Jeong | Oct 2011 | B2 |
| 8033771 | Gage et al. | Oct 2011 | B1 |
| 8038835 | Hayashi et al. | Oct 2011 | B2 |
| 8041197 | Kasai et al. | Oct 2011 | B2 |
| 8041450 | Takizawa et al. | Oct 2011 | B2 |
| 8043972 | Liu et al. | Oct 2011 | B1 |
| 8046193 | Yetter et al. | Oct 2011 | B2 |
| 8048783 | Chung et al. | Nov 2011 | B2 |
| 8055378 | Numakura | Nov 2011 | B2 |
| 8060252 | Gage et al. | Nov 2011 | B2 |
| 8083853 | Choi et al. | Nov 2011 | B2 |
| D651291 | Liebson et al. | Dec 2011 | S |
| 8071451 | Berry | Dec 2011 | B2 |
| 8071452 | Raisanen | Dec 2011 | B2 |
| 8072578 | Yasuda et al. | Dec 2011 | B2 |
| 8076230 | Wei | Dec 2011 | B2 |
| 8076237 | Uzoh | Dec 2011 | B2 |
| 8076250 | Rajagopalan | Dec 2011 | B1 |
| 8076251 | Akae et al. | Dec 2011 | B2 |
| 8078310 | Nishimoto et al. | Dec 2011 | B2 |
| 8082946 | Laverdiere et al. | Dec 2011 | B2 |
| 8084104 | Shinriki et al. | Dec 2011 | B2 |
| 8084372 | You et al. | Dec 2011 | B2 |
| D652896 | Gether | Jan 2012 | S |
| 8092604 | Tomiyasu et al. | Jan 2012 | B2 |
| 8100583 | Aggarwal | Jan 2012 | B2 |
| D653734 | Sisk | Feb 2012 | S |
| D654884 | Honma | Feb 2012 | S |
| D655055 | Toll | Feb 2012 | S |
| 8110099 | Hersey et al. | Feb 2012 | B2 |
| 8114734 | Yang et al. | Feb 2012 | B2 |
| 8119466 | Avouris | Feb 2012 | B2 |
| 8129290 | Balseanu et al. | Mar 2012 | B2 |
| 8137462 | Fondurulia et al. | Mar 2012 | B2 |
| 8137465 | Shrinivasan et al. | Mar 2012 | B1 |
| 8138104 | Balseanu et al. | Mar 2012 | B2 |
| 8138676 | Mills | Mar 2012 | B2 |
| 8142862 | Lee et al. | Mar 2012 | B2 |
| 8143174 | Xia et al. | Mar 2012 | B2 |
| 8147242 | Shibagaki et al. | Apr 2012 | B2 |
| 8158512 | Ji et al. | Apr 2012 | B2 |
| 8172947 | Shibata et al. | May 2012 | B2 |
| 8173554 | Lee et al. | May 2012 | B2 |
| 8178436 | King et al. | May 2012 | B2 |
| 8187679 | Dickey et al. | May 2012 | B2 |
| 8187951 | Wang | May 2012 | B1 |
| 8192901 | Kageyama | Jun 2012 | B2 |
| 8196234 | Glunk | Jun 2012 | B2 |
| 8197915 | Oka et al. | Jun 2012 | B2 |
| 8198168 | Tanioku | Jun 2012 | B2 |
| 8216380 | White et al. | Jul 2012 | B2 |
| 8231799 | Bera et al. | Jul 2012 | B2 |
| D665055 | Yanagisawa et al. | Aug 2012 | S |
| 8241991 | Hsieh et al. | Aug 2012 | B2 |
| 8242028 | van Schravendijk | Aug 2012 | B1 |
| 8242031 | Mallick et al. | Aug 2012 | B2 |
| 8246900 | Kasai et al. | Aug 2012 | B2 |
| 8252114 | Vukovic | Aug 2012 | B2 |
| 8252659 | Huyghabaert et al. | Aug 2012 | B2 |
| 8252691 | Beynet et al. | Aug 2012 | B2 |
| 8267633 | Obikane | Sep 2012 | B2 |
| 8272516 | Salvador | Sep 2012 | B2 |
| 8278176 | Bauer et al. | Oct 2012 | B2 |
| 8282769 | Iizuka | Oct 2012 | B2 |
| 8282847 | Romano | Oct 2012 | B2 |
| 8287648 | Reed et al. | Oct 2012 | B2 |
| 8293016 | Bahng et al. | Oct 2012 | B2 |
| 8293642 | Kim | Oct 2012 | B2 |
| 8298951 | Nakano | Oct 2012 | B1 |
| 8307472 | Saxon et al. | Nov 2012 | B1 |
| 8309173 | Tuominen et al. | Nov 2012 | B2 |
| 8323413 | Son | Dec 2012 | B2 |
| 8328939 | Choi et al. | Dec 2012 | B2 |
| 8329599 | Fukazawa et al. | Dec 2012 | B2 |
| 8334219 | Lee et al. | Dec 2012 | B2 |
| 8349083 | Takasuka et al. | Jan 2013 | B2 |
| D676943 | Kluss | Feb 2013 | S |
| 8367528 | Bauer et al. | Feb 2013 | B2 |
| 8372204 | Nakamura | Feb 2013 | B2 |
| 8378464 | Kato et al. | Feb 2013 | B2 |
| 8393091 | Kawamoto | Mar 2013 | B2 |
| 8394466 | Hong et al. | Mar 2013 | B2 |
| 8398773 | Jdira et al. | Mar 2013 | B2 |
| 8404499 | Moffatt | Mar 2013 | B2 |
| 8415258 | Akae | Apr 2013 | B2 |
| 8415259 | Lee et al. | Apr 2013 | B2 |
| 8440259 | Chiang et al. | May 2013 | B2 |
| 8444120 | Gregg et al. | May 2013 | B2 |
| 8445075 | Xu et al. | May 2013 | B2 |
| 8450191 | Wang | May 2013 | B2 |
| 8465811 | Ueda | Jun 2013 | B2 |
| 8466411 | Arai | Jun 2013 | B2 |
| 8470187 | Ha | Jun 2013 | B2 |
| 8484846 | Dhindsa | Jul 2013 | B2 |
| 8492170 | Xie et al. | Jul 2013 | B2 |
| 8496377 | Harr et al. | Jul 2013 | B2 |
| 8496756 | Cruse et al. | Jul 2013 | B2 |
| 8497213 | Yasui et al. | Jul 2013 | B2 |
| 8501599 | Ueno et al. | Aug 2013 | B2 |
| 8506162 | Schick et al. | Aug 2013 | B2 |
| 8506713 | Takagi | Aug 2013 | B2 |
| 8529701 | Morita | Sep 2013 | B2 |
| 8535767 | Kimura | Sep 2013 | B1 |
| D691974 | Osada et al. | Oct 2013 | S |
| 8551892 | Nakano | Oct 2013 | B2 |
| 8562272 | Lenz | Oct 2013 | B2 |
| 8563443 | Fukazawa | Oct 2013 | B2 |
| 8569184 | Oka | Oct 2013 | B2 |
| 8586484 | Matsuyama et al. | Nov 2013 | B2 |
| 8591659 | Fang et al. | Nov 2013 | B1 |
| 8592005 | Ueda | Nov 2013 | B2 |
| D695240 | Iida et al. | Dec 2013 | S |
| 8608885 | Goto et al. | Dec 2013 | B2 |
| 8614047 | Ayothi et al. | Dec 2013 | B2 |
| 8616765 | Darabnia et al. | Dec 2013 | B2 |
| 8617411 | Singh | Dec 2013 | B2 |
| 8633115 | Chang et al. | Jan 2014 | B2 |
| D698904 | Milligan et al. | Feb 2014 | S |
| 8642488 | Liu et al. | Feb 2014 | B2 |
| 8647722 | Kobayashi et al. | Feb 2014 | B2 |
| 8664627 | Ishikawa et al. | Mar 2014 | B1 |
| 8667654 | Gros-Jean | Mar 2014 | B2 |
| 8668957 | Dussarrat et al. | Mar 2014 | B2 |
| 8669185 | Onizawa | Mar 2014 | B2 |
| 8679958 | Takamure et al. | Mar 2014 | B2 |
| D702188 | Jacobs | Apr 2014 | S |
| 8683943 | Onodera et al. | Apr 2014 | B2 |
| 8710580 | Sakuma et al. | Apr 2014 | B2 |
| 8711338 | Liu et al. | Apr 2014 | B2 |
| D705745 | Kurs et al. | May 2014 | S |
| D705762 | Yu | May 2014 | S |
| 8664127 | Bhatia et al. | May 2014 | B2 |
| 8720965 | Hino et al. | May 2014 | B2 |
| 8721791 | Choi et al. | May 2014 | B2 |
| 8722510 | Watanabe et al. | May 2014 | B2 |
| 8722546 | Fukazawa et al. | May 2014 | B2 |
| 8726837 | Patalay et al. | May 2014 | B2 |
| 8728832 | Raisanen et al. | May 2014 | B2 |
| 8742668 | Nakano et al. | Jun 2014 | B2 |
| 8759223 | Sapre et al. | Jun 2014 | B2 |
| 8764085 | Urabe | Jul 2014 | B2 |
| 8771807 | Xiao et al. | Jul 2014 | B2 |
| 8779502 | Sakuma et al. | Jul 2014 | B2 |
| 8784950 | Fukazawa et al. | Jul 2014 | B2 |
| 8784951 | Fukazawa et al. | Jul 2014 | B2 |
| 8785215 | Kobayashi et al. | Jul 2014 | B2 |
| 8785311 | Miyoshi | Jul 2014 | B2 |
| 8790743 | Omari | Jul 2014 | B1 |
| 8790749 | Omori et al. | Jul 2014 | B2 |
| 8802201 | Raisanen et al. | Aug 2014 | B2 |
| 8820809 | Ando et al. | Sep 2014 | B2 |
| 8821640 | Cleary et al. | Sep 2014 | B2 |
| 8841182 | Chen et al. | Sep 2014 | B1 |
| 8845806 | Aida et al. | Sep 2014 | B2 |
| 8846502 | Haukka et al. | Sep 2014 | B2 |
| D715410 | Lohmann | Oct 2014 | S |
| 8864202 | Schrameyer | Oct 2014 | B1 |
| D716742 | Jang et al. | Nov 2014 | S |
| 8877655 | Shero et al. | Nov 2014 | B2 |
| 8882923 | Saido et al. | Nov 2014 | B2 |
| 8883270 | Shero et al. | Nov 2014 | B2 |
| 8901016 | Ha et al. | Dec 2014 | B2 |
| 8911553 | Baluja et al. | Dec 2014 | B2 |
| 8911826 | Adachi et al. | Dec 2014 | B2 |
| 8912101 | Tsuji et al. | Dec 2014 | B2 |
| D720838 | Yamagishi et al. | Jan 2015 | S |
| 8927906 | Tadokoro et al. | Jan 2015 | B2 |
| 8933375 | Dunn et al. | Jan 2015 | B2 |
| 8940646 | Chandrasekharan | Jan 2015 | B1 |
| D723153 | Borkholder | Feb 2015 | S |
| 8945305 | Marsh | Feb 2015 | B2 |
| 8945306 | Tsuda | Feb 2015 | B2 |
| 8945339 | Kakimoto | Feb 2015 | B2 |
| 8946830 | Jung et al. | Feb 2015 | B2 |
| 8956971 | Huakka | Feb 2015 | B2 |
| 8956983 | Swaminathan | Feb 2015 | B2 |
| D723330 | York | Mar 2015 | S |
| D724553 | Choi | Mar 2015 | S |
| D724701 | Yamagishi et al. | Mar 2015 | S |
| D725168 | Yamagishi | Mar 2015 | S |
| 8967608 | Mitsumori et al. | Mar 2015 | B2 |
| 8974868 | Ishikawa et al. | Mar 2015 | B2 |
| 8986456 | Fondurulia et al. | Mar 2015 | B2 |
| 8991214 | Hoshino et al. | Mar 2015 | B2 |
| 8991887 | Shin et al. | Mar 2015 | B2 |
| 8993054 | Jung et al. | Mar 2015 | B2 |
| 8993457 | Ramkumar et al. | Mar 2015 | B1 |
| D726365 | Weigensberg | Apr 2015 | S |
| D726884 | Yamagishi et al. | Apr 2015 | S |
| 8999102 | Miyoshi et al. | Apr 2015 | B2 |
| 9005539 | Halpin et al. | Apr 2015 | B2 |
| 9017481 | Pettinger et al. | Apr 2015 | B1 |
| 9017933 | Liu et al. | Apr 2015 | B2 |
| 9018093 | Tsuji et al. | Apr 2015 | B2 |
| 9018111 | Milligan et al. | Apr 2015 | B2 |
| 9018567 | de Ridder et al. | Apr 2015 | B2 |
| 9021985 | Alokozai et al. | May 2015 | B2 |
| 9023737 | Beynet et al. | May 2015 | B2 |
| 9023738 | Kato et al. | May 2015 | B2 |
| 9029253 | Milligan et al. | May 2015 | B2 |
| 9029272 | Nakano | May 2015 | B1 |
| D732145 | Yamagishi | Jun 2015 | S |
| D732644 | Yamagishi et al. | Jun 2015 | S |
| D733261 | Yamagishi et al. | Jun 2015 | S |
| D733262 | Yamagishi et al. | Jul 2015 | S |
| D733843 | Yamagishi | Jul 2015 | S |
| D734377 | Hirakida | Jul 2015 | S |
| D735836 | Yamagishi et al. | Aug 2015 | S |
| 9096931 | Yednak et al. | Aug 2015 | B2 |
| 9099505 | Kusakabe et al. | Aug 2015 | B2 |
| 9111972 | Takeshita et al. | Aug 2015 | B2 |
| 9117657 | Nakano et al. | Aug 2015 | B2 |
| 9117866 | Marquardt et al. | Aug 2015 | B2 |
| D739222 | Chadbourne | Sep 2015 | S |
| 9123510 | Nakano et al. | Sep 2015 | B2 |
| 9123577 | Fujimoto et al. | Sep 2015 | B2 |
| 9129897 | Pore et al. | Sep 2015 | B2 |
| 9136108 | Matsushita et al. | Sep 2015 | B2 |
| 9136180 | Machkaoutsan | Sep 2015 | B2 |
| 9142393 | Okabe et al. | Sep 2015 | B2 |
| 9142437 | Fosnight et al. | Sep 2015 | B2 |
| 9153441 | Takamure et al. | Oct 2015 | B2 |
| 9166012 | Sim et al. | Oct 2015 | B2 |
| 9169975 | Sarin et al. | Oct 2015 | B2 |
| 9171714 | Mori | Oct 2015 | B2 |
| 9171716 | Fukuda | Oct 2015 | B2 |
| D742202 | Cyphers et al. | Nov 2015 | S |
| D743357 | Vyne | Nov 2015 | S |
| D743513 | Yamagishi | Nov 2015 | S |
| 9174178 | Yudovsky et al. | Nov 2015 | B2 |
| 9175394 | Berger et al. | Nov 2015 | B2 |
| 9177784 | Raisanen et al. | Nov 2015 | B2 |
| 9184047 | Liu et al. | Nov 2015 | B2 |
| 9190263 | Ishikawa et al. | Nov 2015 | B2 |
| 9190264 | Yuasa et al. | Nov 2015 | B2 |
| 9196483 | Lee et al. | Nov 2015 | B1 |
| 9202727 | Dunn et al. | Dec 2015 | B2 |
| 9214333 | Sims et al. | Dec 2015 | B1 |
| 9228259 | Haukka et al. | Jan 2016 | B2 |
| 9240412 | Xie et al. | Jan 2016 | B2 |
| 9245742 | Haukka | Jan 2016 | B2 |
| 9252024 | Lam et al. | Feb 2016 | B2 |
| 9257274 | Kang et al. | Feb 2016 | B2 |
| 9263298 | Matsumoto et al. | Feb 2016 | B2 |
| 9267850 | Aggarwal | Feb 2016 | B2 |
| 9281277 | Baek et al. | Mar 2016 | B2 |
| 9284642 | Nakano | Mar 2016 | B2 |
| 9297705 | Aggarwal | Mar 2016 | B2 |
| 9299557 | Tolle et al. | Mar 2016 | B2 |
| 9299595 | Dunn et al. | Mar 2016 | B2 |
| D753269 | Yamagishi et al. | Apr 2016 | S |
| D753629 | Plattard | Apr 2016 | S |
| 9305836 | Gates et al. | Apr 2016 | B1 |
| 9312155 | Mori | Apr 2016 | B2 |
| 9315897 | Byun | Apr 2016 | B2 |
| 9324811 | Weeks | Apr 2016 | B2 |
| 9324846 | Camillo | Apr 2016 | B1 |
| 9337054 | Hunks et al. | May 2016 | B2 |
| 9341296 | Yednak | May 2016 | B2 |
| 9343297 | Fukazawa et al. | May 2016 | B1 |
| 9343308 | Isii | May 2016 | B2 |
| 9343343 | Mori | May 2016 | B2 |
| 9343350 | Arai | May 2016 | B2 |
| 9349620 | Kamata et al. | May 2016 | B2 |
| 9353441 | Chung | May 2016 | B2 |
| 9355876 | Rejuter et al. | May 2016 | B2 |
| 9365924 | Nonaka | Jun 2016 | B2 |
| 9368352 | Takamure et al. | Jun 2016 | B2 |
| 9370863 | Tsuji et al. | Jun 2016 | B2 |
| 9384987 | Jung et al. | Jul 2016 | B2 |
| 9390909 | Pasquale et al. | Jul 2016 | B2 |
| 9394608 | Shero et al. | Jul 2016 | B2 |
| 9396934 | Tolle | Jul 2016 | B2 |
| 9396956 | Fukazawa | Jul 2016 | B1 |
| 9404587 | Shugrue | Aug 2016 | B2 |
| 9412564 | Milligan | Aug 2016 | B2 |
| 9412582 | Sasaki et al. | Aug 2016 | B2 |
| 9425078 | Tang et al. | Aug 2016 | B2 |
| 9443725 | Liu et al. | Sep 2016 | B2 |
| 9447498 | Shiba et al. | Sep 2016 | B2 |
| 9449793 | Shaji et al. | Sep 2016 | B2 |
| 9455138 | Fukazawa | Sep 2016 | B1 |
| 9464352 | Nakano et al. | Oct 2016 | B2 |
| 9478414 | Kobayashi et al. | Oct 2016 | B2 |
| 9478415 | Kimura | Oct 2016 | B2 |
| D770993 | Yoshida et al. | Nov 2016 | S |
| 9484191 | Winkler | Nov 2016 | B2 |
| 9514927 | Tolle et al. | Dec 2016 | B2 |
| 9514932 | Mallick et al. | Dec 2016 | B2 |
| 9543180 | Kamiya | Jan 2017 | B2 |
| 9556516 | Takamure | Jan 2017 | B2 |
| 9558931 | Tang | Jan 2017 | B2 |
| 9564314 | Takamure et al. | Feb 2017 | B2 |
| 9574268 | Dunn et al. | Feb 2017 | B1 |
| 9589770 | Winkler | Mar 2017 | B2 |
| 9605342 | Alokozai et al. | Mar 2017 | B2 |
| 9605343 | Winkler | Mar 2017 | B2 |
| 9607837 | Namba | Mar 2017 | B1 |
| D783351 | Fujino et al. | Apr 2017 | S |
| 9613801 | Carcasi et al. | Apr 2017 | B2 |
| 9627221 | Zaitsu et al. | Apr 2017 | B1 |
| D785766 | Sato | May 2017 | S |
| D787458 | Kim et al. | May 2017 | S |
| 9640416 | Arai | May 2017 | B2 |
| 9640448 | Ikegawa et al. | May 2017 | B2 |
| 9647114 | Margetis | May 2017 | B2 |
| 9657845 | Shugrue | May 2017 | B2 |
| 9659799 | Lawson | May 2017 | B2 |
| 9663857 | Nakano et al. | May 2017 | B2 |
| D789888 | Jang et al. | Jun 2017 | S |
| 9685320 | Kang et al. | Jun 2017 | B2 |
| 9691771 | Lansalot-Matras | Jun 2017 | B2 |
| 9698031 | Kobayashi et al. | Jul 2017 | B2 |
| 9708707 | Ditizio et al. | Jul 2017 | B2 |
| 9708708 | Isobe et al. | Jul 2017 | B2 |
| 9711345 | Shiba et al. | Jul 2017 | B2 |
| D793352 | Hill | Aug 2017 | S |
| D793572 | Kozuka et al. | Aug 2017 | S |
| 9735024 | Zaitsu | Aug 2017 | B2 |
| 9741559 | Shimura et al. | Aug 2017 | B2 |
| 9748145 | Kannan et al. | Aug 2017 | B1 |
| D796458 | Jang et al. | Sep 2017 | S |
| 9754779 | Ishikawa | Sep 2017 | B1 |
| 9754818 | Shin et al. | Sep 2017 | B2 |
| 9759489 | Kaneko | Sep 2017 | B2 |
| 9790595 | Jung et al. | Oct 2017 | B2 |
| 9793115 | Tolle | Oct 2017 | B2 |
| 9793135 | Zaitsu et al. | Oct 2017 | B1 |
| 9793148 | Yamagishi et al. | Oct 2017 | B2 |
| D802546 | Jang et al. | Nov 2017 | S |
| 9808246 | Shelton et al. | Nov 2017 | B2 |
| 9812319 | Fukazawa et al. | Nov 2017 | B1 |
| 9812320 | Pore et al. | Nov 2017 | B1 |
| 9859151 | Niskanen | Jan 2018 | B1 |
| 9875891 | Henri et al. | Jan 2018 | B2 |
| 9887082 | Pore et al. | Feb 2018 | B1 |
| 9890456 | Tolle et al. | Feb 2018 | B2 |
| 9891521 | Kang et al. | Feb 2018 | B2 |
| 9892908 | Pettinger et al. | Feb 2018 | B2 |
| 9892913 | Margetis et al. | Feb 2018 | B2 |
| 9895715 | Haukka et al. | Feb 2018 | B2 |
| 9899291 | Kato | Feb 2018 | B2 |
| 9899405 | Kim | Feb 2018 | B2 |
| 9905420 | Margetis et al. | Feb 2018 | B2 |
| 9909492 | Tang | Feb 2018 | B2 |
| 9909214 | Suemori | Mar 2018 | B2 |
| 9911676 | Tang | Mar 2018 | B2 |
| 9916980 | Knaepen | Mar 2018 | B1 |
| 9929011 | Hawryluk et al. | Mar 2018 | B2 |
| 9960072 | Coomer | May 2018 | B2 |
| 9984869 | Blanquart | May 2018 | B1 |
| 10032628 | Xie et al. | Jun 2018 | B2 |
| 10023960 | Alokozai | Jul 2018 | B2 |
| 10032792 | Kim et al. | Jul 2018 | B2 |
| 10043661 | Kato et al. | Aug 2018 | B2 |
| 10053774 | Tolle et al. | Aug 2018 | B2 |
| 10083836 | Milligan | Sep 2018 | B2 |
| D830981 | Jeong et al. | Oct 2018 | S |
| 10087522 | Raisanen et al. | Oct 2018 | B2 |
| 10087525 | Schmotzer et al. | Oct 2018 | B2 |
| 10090316 | Ootsuka | Oct 2018 | B2 |
| 10103040 | Oosterlaken et al. | Oct 2018 | B1 |
| 10134757 | Chun et al. | Nov 2018 | B2 |
| RE47170 | Beynet et al. | Dec 2018 | E |
| 10167557 | Hawkins et al. | Jan 2019 | B2 |
| 20010001953 | Griffiths et al. | May 2001 | A1 |
| 20010003191 | Kovacs et al. | Jun 2001 | A1 |
| 20010006070 | Shang | Jul 2001 | A1 |
| 20010007645 | Honma | Jul 2001 | A1 |
| 20010014514 | Geusic | Aug 2001 | A1 |
| 20010017103 | Takeshita et al. | Aug 2001 | A1 |
| 20010018267 | Shinriki et al. | Aug 2001 | A1 |
| 20010019777 | Tanaka et al. | Sep 2001 | A1 |
| 20010019900 | Hasegawa | Sep 2001 | A1 |
| 20010020715 | Yamasaki | Sep 2001 | A1 |
| 20010028924 | Sherman | Oct 2001 | A1 |
| 20010031535 | Agnello et al. | Oct 2001 | A1 |
| 20010038783 | Nakashima et al. | Nov 2001 | A1 |
| 20010040511 | Bushner et al. | Nov 2001 | A1 |
| 20010046765 | Cappellani et al. | Nov 2001 | A1 |
| 20010048981 | Suzuki | Dec 2001 | A1 |
| 20010049080 | Asano | Dec 2001 | A1 |
| 20010049202 | Maeda et al. | Dec 2001 | A1 |
| 20020001974 | Chan | Jan 2002 | A1 |
| 20020001976 | Danek | Jan 2002 | A1 |
| 20020005400 | Gat et al. | Jan 2002 | A1 |
| 20020009119 | Matthew et al. | Jan 2002 | A1 |
| 20020011210 | Satoh et al. | Jan 2002 | A1 |
| 20020011211 | Halpin | Jan 2002 | A1 |
| 20020013792 | Imielinski et al. | Jan 2002 | A1 |
| 20020014204 | Pyo | Feb 2002 | A1 |
| 20020014483 | Suzuki et al. | Feb 2002 | A1 |
| 20020016829 | Defosse | Feb 2002 | A1 |
| 20020023677 | Zheng | Feb 2002 | A1 |
| 20020031644 | Malofsky et al. | Mar 2002 | A1 |
| 20020041931 | Suntola et al. | Apr 2002 | A1 |
| 20020043337 | Goodman et al. | Apr 2002 | A1 |
| 20020081826 | Rotondaro et al. | Apr 2002 | A1 |
| 20020064592 | Datta et al. | May 2002 | A1 |
| 20020064598 | Wang et al. | May 2002 | A1 |
| 20020069222 | McNeely | Jun 2002 | A1 |
| 20020076507 | Chiang et al. | Jun 2002 | A1 |
| 20020078893 | Van Os et al. | Jun 2002 | A1 |
| 20020079714 | Soucy et al. | Jun 2002 | A1 |
| 20020088542 | Nishikawa et al. | Jul 2002 | A1 |
| 20020096211 | Zheng | Jul 2002 | A1 |
| 20020098627 | Pomarede et al. | Jul 2002 | A1 |
| 20020108670 | Baker et al. | Aug 2002 | A1 |
| 20020109115 | Cederstav et al. | Aug 2002 | A1 |
| 20020110695 | Yang et al. | Aug 2002 | A1 |
| 20020110991 | Li | Aug 2002 | A1 |
| 20020112114 | Blair et al. | Aug 2002 | A1 |
| 20020114886 | Chou et al. | Aug 2002 | A1 |
| 20020115252 | Haukka et al. | Aug 2002 | A1 |
| 20020124883 | Zheng | Sep 2002 | A1 |
| 20020127350 | Ishikawa et al. | Sep 2002 | A1 |
| 20020134511 | Ushioda et al. | Sep 2002 | A1 |
| 20020136214 | Do et al. | Sep 2002 | A1 |
| 20020136909 | Yang | Sep 2002 | A1 |
| 20020139775 | Chang | Oct 2002 | A1 |
| 20020146512 | Rossman | Oct 2002 | A1 |
| 20020151327 | Levitt | Oct 2002 | A1 |
| 20020152244 | Dean et al. | Oct 2002 | A1 |
| 20020155219 | Wang et al. | Oct 2002 | A1 |
| 20020164420 | Derderian et al. | Nov 2002 | A1 |
| 20020172768 | Endo et al. | Nov 2002 | A1 |
| 20020174106 | Martin | Nov 2002 | A1 |
| 20020179011 | Jonnalagadda et al. | Dec 2002 | A1 |
| 20020184111 | Swanson | Dec 2002 | A1 |
| 20020187650 | Blalock et al. | Dec 2002 | A1 |
| 20020187656 | Tan et al. | Dec 2002 | A1 |
| 20020197849 | Mandal | Dec 2002 | A1 |
| 20030002562 | Yerlikaya et al. | Jan 2003 | A1 |
| 20030003607 | Kagoshima | Jan 2003 | A1 |
| 20030003635 | Paranjpe et al. | Jan 2003 | A1 |
| 20030003696 | Gelatos et al. | Jan 2003 | A1 |
| 20030010451 | Tzu | Jan 2003 | A1 |
| 20030010452 | Park et al. | Jan 2003 | A1 |
| 20030012632 | Saeki | Jan 2003 | A1 |
| 20030015294 | Wang | Jan 2003 | A1 |
| 20030015596 | Evans | Jan 2003 | A1 |
| 20030017268 | Hu | Jan 2003 | A1 |
| 20030019428 | Ku et al. | Jan 2003 | A1 |
| 20030019580 | Strang | Jan 2003 | A1 |
| 20030022468 | Shioya et al. | Jan 2003 | A1 |
| 20030022523 | Irino et al. | Jan 2003 | A1 |
| 20030023338 | Chin et al. | Jan 2003 | A1 |
| 20030024901 | Ishikawa | Feb 2003 | A1 |
| 20030025146 | Narwankar et al. | Feb 2003 | A1 |
| 20030029303 | Hasegawa et al. | Feb 2003 | A1 |
| 20030029381 | Nishibayashi | Feb 2003 | A1 |
| 20030029475 | Hua et al. | Feb 2003 | A1 |
| 20030035002 | Moles | Feb 2003 | A1 |
| 20030036272 | Shamouilian et al. | Feb 2003 | A1 |
| 20030040158 | Saitoh | Feb 2003 | A1 |
| 20030040841 | Nasr et al. | Feb 2003 | A1 |
| 20030042419 | Katsumata et al. | Mar 2003 | A1 |
| 20030049372 | Cook et al. | Mar 2003 | A1 |
| 20030049375 | Nguyen et al. | Mar 2003 | A1 |
| 20030049937 | Suzuki | Mar 2003 | A1 |
| 20030054670 | Wang et al. | Mar 2003 | A1 |
| 20030059535 | Luo | Mar 2003 | A1 |
| 20030059980 | Chen et al. | Mar 2003 | A1 |
| 20030065413 | Liteplo et al. | Apr 2003 | A1 |
| 20030066541 | Sun et al. | Apr 2003 | A1 |
| 20030066826 | Lee et al. | Apr 2003 | A1 |
| 20030071015 | Chinn et al. | Apr 2003 | A1 |
| 20030075925 | Lindfors et al. | Apr 2003 | A1 |
| 20030082296 | Elers et al. | May 2003 | A1 |
| 20030082307 | Chung et al. | May 2003 | A1 |
| 20030091938 | Fairbairn et al. | May 2003 | A1 |
| 20030094133 | Yoshidome et al. | May 2003 | A1 |
| 20030109107 | Hsieh et al. | Jun 2003 | A1 |
| 20030109951 | Hsiung et al. | Jun 2003 | A1 |
| 20030111963 | Tolmachev et al. | Jun 2003 | A1 |
| 20030116087 | Nguyen | Jun 2003 | A1 |
| 20030168750 | Basceri et al. | Jun 2003 | A1 |
| 20030121608 | Chen | Jul 2003 | A1 |
| 20030133854 | Tabata et al. | Jul 2003 | A1 |
| 20030134038 | Paranjpe | Jul 2003 | A1 |
| 20030141820 | White et al. | Jul 2003 | A1 |
| 20030143328 | Chen | Jul 2003 | A1 |
| 20030157436 | Manger et al. | Aug 2003 | A1 |
| 20030159656 | Tan | Aug 2003 | A1 |
| 20030162412 | Chung | Aug 2003 | A1 |
| 20030168001 | Sneh | Sep 2003 | A1 |
| 20030168699 | Honda | Sep 2003 | A1 |
| 20030170583 | Nakashima | Sep 2003 | A1 |
| 20030173490 | Lappen | Sep 2003 | A1 |
| 20030180458 | Sneh | Sep 2003 | A1 |
| 20030183156 | Dando | Oct 2003 | A1 |
| 20030183856 | Wieczorek et al. | Oct 2003 | A1 |
| 20030188685 | Wang | Oct 2003 | A1 |
| 20030192875 | Bieker et al. | Oct 2003 | A1 |
| 20030198587 | Kaloyeros | Oct 2003 | A1 |
| 20030201541 | Kim | Oct 2003 | A1 |
| 20030205202 | Funaki et al. | Nov 2003 | A1 |
| 20030209323 | Yokogaki | Nov 2003 | A1 |
| 20030209326 | Lee et al. | Nov 2003 | A1 |
| 20030209746 | Horii | Nov 2003 | A1 |
| 20030211735 | Rossman | Nov 2003 | A1 |
| 20030217915 | Ouellet | Nov 2003 | A1 |
| 20030219972 | Green | Nov 2003 | A1 |
| 20030226840 | Dalton | Dec 2003 | A1 |
| 20030228772 | Cowans | Dec 2003 | A1 |
| 20030231698 | Yamaguchi | Dec 2003 | A1 |
| 20030232138 | Tuominen et al. | Dec 2003 | A1 |
| 20030232491 | Yamaguchi | Dec 2003 | A1 |
| 20040002224 | Chono et al. | Jan 2004 | A1 |
| 20040009307 | Koh et al. | Jan 2004 | A1 |
| 20040009679 | Yeo et al. | Jan 2004 | A1 |
| 20040010772 | McKenna et al. | Jan 2004 | A1 |
| 20040013577 | Ganguli et al. | Jan 2004 | A1 |
| 20040013818 | Moon et al. | Jan 2004 | A1 |
| 20040016637 | Yang | Jan 2004 | A1 |
| 20040018304 | Chung et al. | Jan 2004 | A1 |
| 20040018307 | Park et al. | Jan 2004 | A1 |
| 20040018723 | Byun et al. | Jan 2004 | A1 |
| 20040018750 | Sophie et al. | Jan 2004 | A1 |
| 20040023516 | Londergan et al. | Feb 2004 | A1 |
| 20040026372 | Takenaka et al. | Feb 2004 | A1 |
| 20040029052 | Park et al. | Feb 2004 | A1 |
| 20040036129 | Forbes et al. | Feb 2004 | A1 |
| 20040037675 | Zinger et al. | Feb 2004 | A1 |
| 20040048439 | Soman | Mar 2004 | A1 |
| 20040048492 | Ishikawa et al. | Mar 2004 | A1 |
| 20040050325 | Samoilov | Mar 2004 | A1 |
| 20040062081 | Drewes | Apr 2004 | A1 |
| 20040063289 | Ohta | Apr 2004 | A1 |
| 20040071897 | Verplancken et al. | Apr 2004 | A1 |
| 20040077182 | Lim et al. | Apr 2004 | A1 |
| 20040079960 | Shakuda | Apr 2004 | A1 |
| 20040080697 | Song | Apr 2004 | A1 |
| 20040082171 | Shin et al. | Apr 2004 | A1 |
| 20040087141 | Ramanathan et al. | May 2004 | A1 |
| 20040094402 | Gopalraja | May 2004 | A1 |
| 20040099213 | Adomaitis et al. | May 2004 | A1 |
| 20040101622 | Park et al. | May 2004 | A1 |
| 20040103914 | Cheng et al. | Jun 2004 | A1 |
| 20040106249 | Huotari | Jun 2004 | A1 |
| 20040124131 | Aitchison | Jul 2004 | A1 |
| 20040124549 | Curran | Jul 2004 | A1 |
| 20040126990 | Ohta | Jul 2004 | A1 |
| 20040129211 | Blonigan et al. | Jul 2004 | A1 |
| 20040129671 | Ji et al. | Jul 2004 | A1 |
| 20040134429 | Yamanaka | Jul 2004 | A1 |
| 20040144311 | Chen | Jul 2004 | A1 |
| 20040144980 | Ahn et al. | Jul 2004 | A1 |
| 20040146644 | Xia et al. | Jul 2004 | A1 |
| 20040151844 | Zhang et al. | Aug 2004 | A1 |
| 20040151845 | Nguyen et al. | Aug 2004 | A1 |
| 20040152287 | Sherrill et al. | Aug 2004 | A1 |
| 20040159343 | Shimbara et al. | Aug 2004 | A1 |
| 20040168627 | Conley et al. | Sep 2004 | A1 |
| 20040169032 | Murayama et al. | Sep 2004 | A1 |
| 20040187777 | Okamoto et al. | Sep 2004 | A1 |
| 20040187790 | Bader | Sep 2004 | A1 |
| 20040187928 | Ambrosina | Sep 2004 | A1 |
| 20040198069 | Metzner | Oct 2004 | A1 |
| 20040200499 | Harvey et al. | Oct 2004 | A1 |
| 20040203251 | Kawaguchi et al. | Oct 2004 | A1 |
| 20040206305 | Choi et al. | Oct 2004 | A1 |
| 20040209477 | Buxbaum et al. | Oct 2004 | A1 |
| 20040211357 | Gadgil | Oct 2004 | A1 |
| 20040212947 | Nguyen | Oct 2004 | A1 |
| 20040213921 | Leu | Oct 2004 | A1 |
| 20040214399 | Ahn et al. | Oct 2004 | A1 |
| 20040214445 | Shimizu et al. | Oct 2004 | A1 |
| 20040217217 | Han et al. | Nov 2004 | A1 |
| 20040219793 | Hishiya et al. | Nov 2004 | A1 |
| 20040221807 | Verghese et al. | Nov 2004 | A1 |
| 20040231600 | Lee | Nov 2004 | A1 |
| 20040238523 | Kuibira et al. | Dec 2004 | A1 |
| 20040241998 | Hanson | Dec 2004 | A1 |
| 20040247779 | Selvamanickam et al. | Dec 2004 | A1 |
| 20040250600 | Bevers et al. | Dec 2004 | A1 |
| 20040253867 | Matsumoto | Dec 2004 | A1 |
| 20040261712 | Hayashi et al. | Dec 2004 | A1 |
| 20040266011 | Lee et al. | Dec 2004 | A1 |
| 20050000428 | Shero et al. | Jan 2005 | A1 |
| 20050003662 | Jurisch et al. | Jan 2005 | A1 |
| 20050008799 | Tomiyasu et al. | Jan 2005 | A1 |
| 20050019026 | Wang et al. | Jan 2005 | A1 |
| 20050019494 | Moghadam et al. | Jan 2005 | A1 |
| 20050020071 | Sonobe et al. | Jan 2005 | A1 |
| 20050023624 | Ahn et al. | Feb 2005 | A1 |
| 20050034674 | Ono | Feb 2005 | A1 |
| 20050037154 | Koh et al. | Feb 2005 | A1 |
| 20050037610 | Cha | Feb 2005 | A1 |
| 20050042778 | Peukert | Feb 2005 | A1 |
| 20050048797 | Fukazawa | Mar 2005 | A1 |
| 20050051093 | Makino et al. | Mar 2005 | A1 |
| 20050054228 | March | Mar 2005 | A1 |
| 20050059262 | Yin et al. | Mar 2005 | A1 |
| 20050064207 | Senzaki et al. | Mar 2005 | A1 |
| 20050064719 | Liu | Mar 2005 | A1 |
| 20050066893 | Soininen | Mar 2005 | A1 |
| 20050069651 | Miyoshi | Mar 2005 | A1 |
| 20050070123 | Hirano | Mar 2005 | A1 |
| 20050070729 | Kiyomori et al. | Mar 2005 | A1 |
| 20050072357 | Shero et al. | Apr 2005 | A1 |
| 20050074983 | Shinriki et al. | Apr 2005 | A1 |
| 20050092247 | Schmidt | May 2005 | A1 |
| 20050092249 | Kilpela et al. | May 2005 | A1 |
| 20050092733 | Ito et al. | May 2005 | A1 |
| 20050095770 | Kumagai et al. | May 2005 | A1 |
| 20050098107 | Du Bois et al. | May 2005 | A1 |
| 20050100669 | Kools et al. | May 2005 | A1 |
| 20050101154 | Huang | May 2005 | A1 |
| 20050101843 | Quinn et al. | May 2005 | A1 |
| 20050106893 | Wilk | May 2005 | A1 |
| 20050110069 | Kil et al. | May 2005 | A1 |
| 20050118804 | Byun et al. | Jun 2005 | A1 |
| 20050118837 | Todd | Jun 2005 | A1 |
| 20050120805 | Lane | Jun 2005 | A1 |
| 20050120962 | Ushioda et al. | Jun 2005 | A1 |
| 20050123690 | Derderian et al. | Jun 2005 | A1 |
| 20050130427 | Seok-Jun | Jun 2005 | A1 |
| 20050132957 | El-Raghy | Jun 2005 | A1 |
| 20050133161 | Carpenter et al. | Jun 2005 | A1 |
| 20050141591 | Sakano | Jun 2005 | A1 |
| 20050142361 | Nakanishi | Jun 2005 | A1 |
| 20050145338 | Park et al. | Jul 2005 | A1 |
| 20050153571 | Senzaki | Jul 2005 | A1 |
| 20050172895 | Kijima et al. | Aug 2005 | A1 |
| 20050173003 | Laverdiere et al. | Aug 2005 | A1 |
| 20050175789 | Helms | Aug 2005 | A1 |
| 20050181535 | Yun et al. | Aug 2005 | A1 |
| 20050181555 | Haukka et al. | Aug 2005 | A1 |
| 20050187647 | Wang et al. | Aug 2005 | A1 |
| 20050191828 | Al-Bayati et al. | Sep 2005 | A1 |
| 20050199013 | Vandroux et al. | Sep 2005 | A1 |
| 20050208718 | Lim et al. | Sep 2005 | A1 |
| 20050211167 | Gunji | Sep 2005 | A1 |
| 20050212119 | Shero | Sep 2005 | A1 |
| 20050214457 | Schmitt et al. | Sep 2005 | A1 |
| 20050214458 | Meiere | Sep 2005 | A1 |
| 20050208778 | Li | Oct 2005 | A1 |
| 20050218462 | Ahn et al. | Oct 2005 | A1 |
| 20050221021 | Strang | Oct 2005 | A1 |
| 20050221618 | AmRhein et al. | Oct 2005 | A1 |
| 20050223982 | Park et al. | Oct 2005 | A1 |
| 20050223994 | Blomiley et al. | Oct 2005 | A1 |
| 20050227502 | Schmitt et al. | Oct 2005 | A1 |
| 20050229848 | Shinriki | Oct 2005 | A1 |
| 20050229849 | Silvetti et al. | Oct 2005 | A1 |
| 20050229972 | Hoshi et al. | Oct 2005 | A1 |
| 20050233477 | Yamazaki et al. | Oct 2005 | A1 |
| 20050241176 | Shero et al. | Nov 2005 | A1 |
| 20050241763 | Huang et al. | Nov 2005 | A1 |
| 20050245058 | Lee et al. | Nov 2005 | A1 |
| 20050249876 | Kawahara et al. | Nov 2005 | A1 |
| 20050250340 | Chen et al. | Nov 2005 | A1 |
| 20050251990 | Choi | Nov 2005 | A1 |
| 20050252449 | Nguyen et al. | Nov 2005 | A1 |
| 20050255257 | Choi et al. | Nov 2005 | A1 |
| 20050258280 | Goto et al. | Nov 2005 | A1 |
| 20050260347 | Narwankar et al. | Nov 2005 | A1 |
| 20050260850 | Loke | Nov 2005 | A1 |
| 20050263072 | Balasubramanian et al. | Dec 2005 | A1 |
| 20050263075 | Wang et al. | Dec 2005 | A1 |
| 20050263932 | Heugel | Dec 2005 | A1 |
| 20050271813 | Kher et al. | Dec 2005 | A1 |
| 20050274323 | Seidel et al. | Dec 2005 | A1 |
| 20050277271 | Beintner | Dec 2005 | A1 |
| 20050282101 | Adachi | Dec 2005 | A1 |
| 20050285097 | Shang et al. | Dec 2005 | A1 |
| 20050287725 | Kitagawa | Dec 2005 | A1 |
| 20050287771 | Seamons et al. | Dec 2005 | A1 |
| 20060000411 | Seo | Jan 2006 | A1 |
| 20060013674 | Elliott et al. | Jan 2006 | A1 |
| 20060013946 | Park et al. | Jan 2006 | A1 |
| 20060014384 | Lee et al. | Jan 2006 | A1 |
| 20060014397 | Seamons et al. | Jan 2006 | A1 |
| 20060016783 | Wu et al. | Jan 2006 | A1 |
| 20060019033 | Muthukrishnan et al. | Jan 2006 | A1 |
| 20060019502 | Park et al. | Jan 2006 | A1 |
| 20060021572 | Wolden | Feb 2006 | A1 |
| 20060021703 | Umotoy et al. | Feb 2006 | A1 |
| 20060024439 | Tuominen et al. | Feb 2006 | A2 |
| 20060026314 | Franchuk et al. | Feb 2006 | A1 |
| 20060040054 | Pearlstein et al. | Feb 2006 | A1 |
| 20060040508 | Ji | Feb 2006 | A1 |
| 20060046518 | Hill et al. | Mar 2006 | A1 |
| 20060051520 | Behle et al. | Mar 2006 | A1 |
| 20060051925 | Ahn et al. | Mar 2006 | A1 |
| 20060057828 | Omura | Mar 2006 | A1 |
| 20060060930 | Metz et al. | Mar 2006 | A1 |
| 20060062910 | Meiere | Mar 2006 | A1 |
| 20060063346 | Lee et al. | Mar 2006 | A1 |
| 20060068104 | Ishizaka | Mar 2006 | A1 |
| 20060068121 | Lee et al. | Mar 2006 | A1 |
| 20060068125 | Radhakrishnan | Mar 2006 | A1 |
| 20060087638 | Hirayanagi | Apr 2006 | A1 |
| 20060096540 | Choi | May 2006 | A1 |
| 20060099782 | Ritenour | May 2006 | A1 |
| 20060105566 | Waldfried et al. | May 2006 | A1 |
| 20060107898 | Blomberg | May 2006 | A1 |
| 20060110934 | Fukuchi | May 2006 | A1 |
| 20060113675 | Chang et al. | Jun 2006 | A1 |
| 20060113806 | Tsuji et al. | Jun 2006 | A1 |
| 20060128142 | Whelan et al. | Jun 2006 | A1 |
| 20060128168 | Ahn et al. | Jun 2006 | A1 |
| 20060130767 | Herchen | Jun 2006 | A1 |
| 20060137609 | Puchacz et al. | Jun 2006 | A1 |
| 20060147626 | Blomberg | Jul 2006 | A1 |
| 20060148180 | Ahn et al. | Jul 2006 | A1 |
| 20060154424 | Yang et al. | Jul 2006 | A1 |
| 20060156981 | Fondurulia | Jul 2006 | A1 |
| 20060163612 | Kouvetakis et al. | Jul 2006 | A1 |
| 20060166428 | Kamioka | Jul 2006 | A1 |
| 20060172531 | Lin et al. | Aug 2006 | A1 |
| 20060175669 | Kim et al. | Aug 2006 | A1 |
| 20060177855 | Utermohlen | Aug 2006 | A1 |
| 20060182885 | Lei et al. | Aug 2006 | A1 |
| 20060188360 | Bonora et al. | Aug 2006 | A1 |
| 20060191555 | Yoshida et al. | Aug 2006 | A1 |
| 20060193979 | Meiere et al. | Aug 2006 | A1 |
| 20060196420 | Ushakov et al. | Sep 2006 | A1 |
| 20060199357 | Wan et al. | Sep 2006 | A1 |
| 20060205223 | Smayling | Sep 2006 | A1 |
| 20060205231 | Chou et al. | Sep 2006 | A1 |
| 20060208215 | Metzner et al. | Sep 2006 | A1 |
| 20060211243 | Ishizaka et al. | Sep 2006 | A1 |
| 20060211259 | Maes | Sep 2006 | A1 |
| 20060213439 | Ishizaka | Sep 2006 | A1 |
| 20060216942 | Kim et al. | Sep 2006 | A1 |
| 20060219169 | Chen et al. | Oct 2006 | A1 |
| 20060223301 | Vanhaelemeersch et al. | Oct 2006 | A1 |
| 20060226117 | Bertram et al. | Oct 2006 | A1 |
| 20060228496 | Choi | Oct 2006 | A1 |
| 20060228863 | Zhang et al. | Oct 2006 | A1 |
| 20060228888 | Lee et al. | Oct 2006 | A1 |
| 20060236934 | Choi et al. | Oct 2006 | A1 |
| 20060240574 | Yoshie | Oct 2006 | A1 |
| 20060240662 | Conley et al. | Oct 2006 | A1 |
| 20060249253 | Dando | Nov 2006 | A1 |
| 20060251827 | Nowak | Nov 2006 | A1 |
| 20060252228 | Jeng | Nov 2006 | A1 |
| 20060252351 | Kundracik | Nov 2006 | A1 |
| 20060257563 | Doh et al. | Nov 2006 | A1 |
| 20060257584 | Derderian et al. | Nov 2006 | A1 |
| 20060258078 | Lee et al. | Nov 2006 | A1 |
| 20060258173 | Xiao et al. | Nov 2006 | A1 |
| 20060260545 | Ramaswamy et al. | Nov 2006 | A1 |
| 20060263522 | Byun | Nov 2006 | A1 |
| 20060264060 | Ramaswamy et al. | Nov 2006 | A1 |
| 20060264066 | Bartholomew | Nov 2006 | A1 |
| 20060266289 | Verghese et al. | Nov 2006 | A1 |
| 20060269690 | Watanabe et al. | Nov 2006 | A1 |
| 20060269692 | Balseanu | Nov 2006 | A1 |
| 20060275933 | Du Bois et al. | Dec 2006 | A1 |
| 20060278524 | Stowell | Dec 2006 | A1 |
| 20060283629 | Kikuchi et al. | Dec 2006 | A1 |
| 20060286774 | Singh et al. | Dec 2006 | A1 |
| 20060286775 | Singh et al. | Dec 2006 | A1 |
| 20060286817 | Kato et al. | Dec 2006 | A1 |
| 20060286818 | Wang et al. | Dec 2006 | A1 |
| 20060286819 | Seutter | Dec 2006 | A1 |
| 20060291982 | Tanaka | Dec 2006 | A1 |
| 20070006806 | Imai | Jan 2007 | A1 |
| 20070010072 | Bailey et al. | Jan 2007 | A1 |
| 20070012402 | Sneh | Jan 2007 | A1 |
| 20070020167 | Han et al. | Jan 2007 | A1 |
| 20070020830 | Speranza | Jan 2007 | A1 |
| 20070020953 | Tsai et al. | Jan 2007 | A1 |
| 20070022954 | Iizuka et al. | Feb 2007 | A1 |
| 20070026148 | Arai et al. | Feb 2007 | A1 |
| 20070028842 | Inagawa et al. | Feb 2007 | A1 |
| 20070031598 | Okuyama et al. | Feb 2007 | A1 |
| 20070031599 | Gschwandtner et al. | Feb 2007 | A1 |
| 20070032045 | Kasahara et al. | Feb 2007 | A1 |
| 20070032082 | Ramaswamy et al. | Feb 2007 | A1 |
| 20070034477 | Inui | Feb 2007 | A1 |
| 20070037343 | Colombo et al. | Feb 2007 | A1 |
| 20070037412 | Dip et al. | Feb 2007 | A1 |
| 20070042117 | Kupurao et al. | Feb 2007 | A1 |
| 20070049053 | Mahajani | Mar 2007 | A1 |
| 20070054499 | Jang | Mar 2007 | A1 |
| 20070056843 | Ye et al. | Mar 2007 | A1 |
| 20070056850 | Ye et al. | Mar 2007 | A1 |
| 20070059948 | Metzner et al. | Mar 2007 | A1 |
| 20070062439 | Wada et al. | Mar 2007 | A1 |
| 20070062453 | Ishikawa | Mar 2007 | A1 |
| 20070065578 | McDougall | Mar 2007 | A1 |
| 20070066010 | Ando | Mar 2007 | A1 |
| 20070066079 | Kolster et al. | Mar 2007 | A1 |
| 20070066084 | Wajda et al. | Mar 2007 | A1 |
| 20070077355 | Chacin et al. | Apr 2007 | A1 |
| 20070082132 | Shinriki | Apr 2007 | A1 |
| 20070082500 | Norman et al. | Apr 2007 | A1 |
| 20070084405 | Kim | Apr 2007 | A1 |
| 20070087579 | Kitayama et al. | Apr 2007 | A1 |
| 20070089670 | Ikedo | Apr 2007 | A1 |
| 20070096194 | Streck et al. | May 2007 | A1 |
| 20070098527 | Hall et al. | May 2007 | A1 |
| 20070107845 | Ishizawa et al. | May 2007 | A1 |
| 20070111470 | Smythe | May 2007 | A1 |
| 20070111545 | Lee et al. | May 2007 | A1 |
| 20070116873 | Li et al. | May 2007 | A1 |
| 20070116888 | Faguet | May 2007 | A1 |
| 20070119370 | Ma et al. | May 2007 | A1 |
| 20070123037 | Lee et al. | May 2007 | A1 |
| 20070123189 | Saito et al. | May 2007 | A1 |
| 20070125762 | Cui et al. | Jun 2007 | A1 |
| 20070128538 | Fairbairn et al. | Jun 2007 | A1 |
| 20070128876 | Fukiage | Jun 2007 | A1 |
| 20070128888 | Goto et al. | Jun 2007 | A1 |
| 20070129621 | Kellogg et al. | Jun 2007 | A1 |
| 20070134942 | Ahn et al. | Jun 2007 | A1 |
| 20070137794 | Qiu et al. | Jun 2007 | A1 |
| 20070146621 | Yeom | Jun 2007 | A1 |
| 20070148350 | Rahtu | Jun 2007 | A1 |
| 20070148990 | Deboer et al. | Jun 2007 | A1 |
| 20070155138 | Tomasini et al. | Jul 2007 | A1 |
| 20070157466 | Kida et al. | Jul 2007 | A1 |
| 20070158026 | Amikura | Jul 2007 | A1 |
| 20070163440 | Kim et al. | Jul 2007 | A1 |
| 20070163625 | Lee | Jul 2007 | A1 |
| 20070166457 | Yamoto et al. | Jul 2007 | A1 |
| 20070166966 | Todd et al. | Jul 2007 | A1 |
| 20070166999 | Vaarstra | Jul 2007 | A1 |
| 20070173071 | Afzali-Ardakani et al. | Jul 2007 | A1 |
| 20070175393 | Nishimura et al. | Aug 2007 | A1 |
| 20070175397 | Tomiyasu et al. | Aug 2007 | A1 |
| 20070178235 | Yamada | Aug 2007 | A1 |
| 20070186849 | Furuya | Aug 2007 | A1 |
| 20070186952 | Honda et al. | Aug 2007 | A1 |
| 20070187363 | Oka et al. | Aug 2007 | A1 |
| 20070202678 | Plombon et al. | Aug 2007 | A1 |
| 20070207275 | Nowak et al. | Sep 2007 | A1 |
| 20070209590 | Li | Sep 2007 | A1 |
| 20070210890 | Hsu et al. | Sep 2007 | A1 |
| 20070215048 | Suzuki et al. | Sep 2007 | A1 |
| 20070218200 | Suzuki et al. | Sep 2007 | A1 |
| 20070218705 | Matsuki et al. | Sep 2007 | A1 |
| 20070224777 | Hamelin | Sep 2007 | A1 |
| 20070224833 | Morisada et al. | Sep 2007 | A1 |
| 20070232031 | Singh et al. | Oct 2007 | A1 |
| 20070232071 | Balseanu et al. | Oct 2007 | A1 |
| 20070232501 | Tonomura | Oct 2007 | A1 |
| 20070234955 | Suzuki et al. | Oct 2007 | A1 |
| 20070237697 | Clark | Oct 2007 | A1 |
| 20070237698 | Clark | Oct 2007 | A1 |
| 20070237699 | Clark | Oct 2007 | A1 |
| 20070241688 | DeVancentis et al. | Oct 2007 | A1 |
| 20070248767 | Okura | Oct 2007 | A1 |
| 20070249131 | Allen et al. | Oct 2007 | A1 |
| 20070251444 | Gros-Jean et al. | Nov 2007 | A1 |
| 20070251456 | Herchen et al. | Nov 2007 | A1 |
| 20070252244 | Srividya et al. | Nov 2007 | A1 |
| 20070252532 | DeVancentis et al. | Nov 2007 | A1 |
| 20070258506 | Schwagerman et al. | Nov 2007 | A1 |
| 20070264807 | Leone et al. | Nov 2007 | A1 |
| 20070266945 | Shuto et al. | Nov 2007 | A1 |
| 20070269983 | Sneh | Nov 2007 | A1 |
| 20070275166 | Thridandam et al. | Nov 2007 | A1 |
| 20070277735 | Mokhesi et al. | Dec 2007 | A1 |
| 20070281082 | Mokhesi et al. | Dec 2007 | A1 |
| 20070281105 | Mokhesi et al. | Dec 2007 | A1 |
| 20070281496 | Ingle et al. | Dec 2007 | A1 |
| 20070298362 | Rocha-Alvarez et al. | Dec 2007 | A1 |
| 20080003824 | Padhi et al. | Jan 2008 | A1 |
| 20080003838 | Haukka et al. | Jan 2008 | A1 |
| 20080006208 | Ueno et al. | Jan 2008 | A1 |
| 20080018004 | Steidl | Jan 2008 | A1 |
| 20080020591 | Balseanu et al. | Jan 2008 | A1 |
| 20080020593 | Wang et al. | Jan 2008 | A1 |
| 20080023436 | Gros-Jean et al. | Jan 2008 | A1 |
| 20080026574 | Brcka | Jan 2008 | A1 |
| 20080026597 | Munro et al. | Jan 2008 | A1 |
| 20080029790 | Ahn et al. | Feb 2008 | A1 |
| 20080031708 | Bonora et al. | Feb 2008 | A1 |
| 20080036354 | Letz et al. | Feb 2008 | A1 |
| 20080038485 | Fukazawa et al. | Feb 2008 | A1 |
| 20080038934 | Vrtis et al. | Feb 2008 | A1 |
| 20080042165 | Sugizaki | Feb 2008 | A1 |
| 20080043803 | Bandoh | Feb 2008 | A1 |
| 20080050536 | Aing et al. | Feb 2008 | A1 |
| 20080050538 | Hirata | Feb 2008 | A1 |
| 20080054332 | Kim et al. | Mar 2008 | A1 |
| 20080054813 | Espiau et al. | Mar 2008 | A1 |
| 20080056860 | Natume | Mar 2008 | A1 |
| 20080057659 | Forbes et al. | Mar 2008 | A1 |
| 20080061667 | Gaertner et al. | Mar 2008 | A1 |
| 20080066778 | Matsushita et al. | Mar 2008 | A1 |
| 20080069955 | Hong et al. | Mar 2008 | A1 |
| 20080075562 | Maria et al. | Mar 2008 | A1 |
| 20080075881 | Won et al. | Mar 2008 | A1 |
| 20080076070 | Koh et al. | Mar 2008 | A1 |
| 20080076266 | Fukazawa et al. | Mar 2008 | A1 |
| 20080081104 | Hasebe et al. | Apr 2008 | A1 |
| 20080081113 | Clark | Apr 2008 | A1 |
| 20080081121 | Morita et al. | Apr 2008 | A1 |
| 20080085226 | Fondurulia et al. | Apr 2008 | A1 |
| 20080092815 | Chen et al. | Apr 2008 | A1 |
| 20080102203 | Wu | May 2008 | A1 |
| 20080113094 | Casper | May 2008 | A1 |
| 20080113096 | Mahajani | May 2008 | A1 |
| 20080113097 | Mahajani et al. | May 2008 | A1 |
| 20080118334 | Bonora | May 2008 | A1 |
| 20080121177 | Bang et al. | May 2008 | A1 |
| 20080121626 | Thomas et al. | May 2008 | A1 |
| 20080124197 | van der Meulen et al. | May 2008 | A1 |
| 20080124908 | Forbes et al. | May 2008 | A1 |
| 20080124946 | Xiao et al. | May 2008 | A1 |
| 20080132046 | Walther | Jun 2008 | A1 |
| 20080133154 | Krauss et al. | Jun 2008 | A1 |
| 20080142483 | Hua | Jun 2008 | A1 |
| 20080149031 | Chu et al. | Jun 2008 | A1 |
| 20080149593 | Bai et al. | Jun 2008 | A1 |
| 20080152463 | Chidambaram et al. | Jun 2008 | A1 |
| 20080153311 | Padhi et al. | Jun 2008 | A1 |
| 20080157157 | Tonomura | Jul 2008 | A1 |
| 20080157365 | Ott et al. | Jul 2008 | A1 |
| 20080173237 | Collins | Jul 2008 | A1 |
| 20080173238 | Nakashima et al. | Jul 2008 | A1 |
| 20080173240 | Furukawahara | Jul 2008 | A1 |
| 20080173326 | Gu et al. | Jul 2008 | A1 |
| 20080176375 | Erben et al. | Jul 2008 | A1 |
| 20080178805 | Paterson et al. | Jul 2008 | A1 |
| 20080179104 | Zhang | Jul 2008 | A1 |
| 20080179715 | Coppa | Jul 2008 | A1 |
| 20080182075 | Chopra | Jul 2008 | A1 |
| 20080182390 | Lemmi et al. | Jul 2008 | A1 |
| 20080191193 | Li et al. | Aug 2008 | A1 |
| 20080199977 | Weigel et al. | Aug 2008 | A1 |
| 20080202416 | Provencher | Aug 2008 | A1 |
| 20080202689 | Kim | Aug 2008 | A1 |
| 20080203487 | Hohage et al. | Aug 2008 | A1 |
| 20080205483 | Rempe et al. | Aug 2008 | A1 |
| 20080211423 | Shinmen et al. | Sep 2008 | A1 |
| 20080211526 | Shinma | Sep 2008 | A1 |
| 20080216077 | Emani et al. | Sep 2008 | A1 |
| 20080216742 | Takebayashi | Sep 2008 | A1 |
| 20080220619 | Matsushita et al. | Sep 2008 | A1 |
| 20080224240 | Ahn et al. | Sep 2008 | A1 |
| 20080228306 | Yetter et al. | Sep 2008 | A1 |
| 20080233288 | Clark | Sep 2008 | A1 |
| 20080237572 | Chui et al. | Oct 2008 | A1 |
| 20080241384 | Jeong | Oct 2008 | A1 |
| 20080241387 | Keto | Oct 2008 | A1 |
| 20080242116 | Clark | Oct 2008 | A1 |
| 20080248310 | Kim et al. | Oct 2008 | A1 |
| 20080257494 | Hayashi et al. | Oct 2008 | A1 |
| 20080260963 | Yoon et al. | Oct 2008 | A1 |
| 20080261413 | Mahajani | Oct 2008 | A1 |
| 20080264337 | Sano et al. | Oct 2008 | A1 |
| 20080267598 | Nakamura | Oct 2008 | A1 |
| 20080268635 | Yu et al. | Oct 2008 | A1 |
| 20080277715 | Ohmi et al. | Nov 2008 | A1 |
| 20080282970 | Heys et al. | Nov 2008 | A1 |
| 20080283962 | Dyer | Nov 2008 | A1 |
| 20080289574 | Jacobs et al. | Nov 2008 | A1 |
| 20080291964 | Shrimpling | Nov 2008 | A1 |
| 20080295872 | Riker et al. | Dec 2008 | A1 |
| 20080298945 | Cox | Dec 2008 | A1 |
| 20080299326 | Fukazawa | Dec 2008 | A1 |
| 20080299758 | Harada et al. | Dec 2008 | A1 |
| 20080302303 | Choi et al. | Dec 2008 | A1 |
| 20080305014 | Honda | Dec 2008 | A1 |
| 20080305246 | Choi et al. | Dec 2008 | A1 |
| 20080305443 | Nakamura | Dec 2008 | A1 |
| 20080315292 | Ji et al. | Dec 2008 | A1 |
| 20080317972 | Hendriks | Dec 2008 | A1 |
| 20090000550 | Tran et al. | Jan 2009 | A1 |
| 20090000551 | Choi et al. | Jan 2009 | A1 |
| 20090011145 | Yun | Jan 2009 | A1 |
| 20090011608 | Nabatame | Jan 2009 | A1 |
| 20090017631 | Bencher | Jan 2009 | A1 |
| 20090020072 | Mizunaga et al. | Jan 2009 | A1 |
| 20090023229 | Matsushita | Jan 2009 | A1 |
| 20090029503 | Arai | Jan 2009 | A1 |
| 20090029528 | Sanchez et al. | Jan 2009 | A1 |
| 20090029564 | Yamashita et al. | Jan 2009 | A1 |
| 20090033907 | Watson | Feb 2009 | A1 |
| 20090035947 | Horii | Feb 2009 | A1 |
| 20090041952 | Yoon et al. | Feb 2009 | A1 |
| 20090041984 | Mayers et al. | Feb 2009 | A1 |
| 20090042344 | Ye et al. | Feb 2009 | A1 |
| 20090042408 | Maeda | Feb 2009 | A1 |
| 20090045829 | Awazu | Feb 2009 | A1 |
| 20090050621 | Awazu | Feb 2009 | A1 |
| 20090052498 | Halpin et al. | Feb 2009 | A1 |
| 20090053023 | Wakabayashi | Feb 2009 | A1 |
| 20090053906 | Miya et al. | Feb 2009 | A1 |
| 20090056629 | Katz et al. | Mar 2009 | A1 |
| 20090057269 | Katz et al. | Mar 2009 | A1 |
| 20090061083 | Chiang et al. | Mar 2009 | A1 |
| 20090061644 | Chiang et al. | Mar 2009 | A1 |
| 20090061647 | Mallick et al. | Mar 2009 | A1 |
| 20090075491 | Liu et al. | Mar 2009 | A1 |
| 20090084317 | Wu | Apr 2009 | A1 |
| 20090085156 | Dewey et al. | Apr 2009 | A1 |
| 20090090382 | Morisada | Apr 2009 | A1 |
| 20090093094 | Ye et al. | Apr 2009 | A1 |
| 20090095221 | Tam et al. | Apr 2009 | A1 |
| 20090104351 | Kakegawa | Apr 2009 | A1 |
| 20090104789 | Mallick et al. | Apr 2009 | A1 |
| 20090107404 | Ogliari et al. | Apr 2009 | A1 |
| 20090108308 | Yang et al. | Apr 2009 | A1 |
| 20090112458 | Nakai | Apr 2009 | A1 |
| 20090115064 | Sandhu et al. | May 2009 | A1 |
| 20090120580 | Kagoshima et al. | May 2009 | A1 |
| 20090122293 | Shibazaki | May 2009 | A1 |
| 20090122458 | Lischer et al. | May 2009 | A1 |
| 20090124131 | Breunsbach et al. | May 2009 | A1 |
| 20090130331 | Asai | May 2009 | A1 |
| 20090130859 | Itatani et al. | May 2009 | A1 |
| 20090136668 | Gregg et al. | May 2009 | A1 |
| 20090136683 | Fukasawa et al. | May 2009 | A1 |
| 20090139657 | Lee et al. | Jun 2009 | A1 |
| 20090142905 | Yamazaki | Jun 2009 | A1 |
| 20090142935 | Fukazawa et al. | Jun 2009 | A1 |
| 20090146322 | Weling et al. | Jun 2009 | A1 |
| 20090156015 | Park et al. | Jun 2009 | A1 |
| 20090159000 | Aggarwal et al. | Jun 2009 | A1 |
| 20090159424 | Liu et al. | Jun 2009 | A1 |
| 20090162996 | Ramaswarmy et al. | Jun 2009 | A1 |
| 20090163038 | Miyoshi | Jun 2009 | A1 |
| 20090165715 | Oh | Jul 2009 | A1 |
| 20090179365 | Lerner et al. | Jul 2009 | A1 |
| 20090186571 | Haro | Jul 2009 | A1 |
| 20090197015 | Kudela et al. | Aug 2009 | A1 |
| 20090200494 | Hatem | Aug 2009 | A1 |
| 20090204403 | Hollander et al. | Aug 2009 | A1 |
| 20090206056 | Xu | Aug 2009 | A1 |
| 20090209081 | Matero | Aug 2009 | A1 |
| 20090211523 | Kuppurao et al. | Aug 2009 | A1 |
| 20090211525 | Sarigiannis et al. | Aug 2009 | A1 |
| 20090227094 | Bateman | Sep 2009 | A1 |
| 20090230211 | Kobayashi et al. | Sep 2009 | A1 |
| 20090236014 | Wilson | Sep 2009 | A1 |
| 20090236276 | Kurth et al. | Sep 2009 | A1 |
| 20090239386 | Suzaki et al. | Sep 2009 | A1 |
| 20090242957 | Ma et al. | Oct 2009 | A1 |
| 20090246374 | Vukovic | Oct 2009 | A1 |
| 20090246399 | Goundar | Oct 2009 | A1 |
| 20090246971 | Reid et al. | Oct 2009 | A1 |
| 20090250955 | Aoki | Oct 2009 | A1 |
| 20090255901 | Okita | Oct 2009 | A1 |
| 20090261331 | Yang et al. | Oct 2009 | A1 |
| 20090269506 | Okura et al. | Oct 2009 | A1 |
| 20090269941 | Raisanen | Oct 2009 | A1 |
| 20090275205 | Kiehlbauch et al. | Nov 2009 | A1 |
| 20090277510 | Shikata | Nov 2009 | A1 |
| 20090283041 | Tomiyasu et al. | Nov 2009 | A1 |
| 20090283217 | Lubomirsky et al. | Nov 2009 | A1 |
| 20090284156 | Banna et al. | Nov 2009 | A1 |
| 20090286400 | Heo et al. | Nov 2009 | A1 |
| 20090286402 | Xia et al. | Nov 2009 | A1 |
| 20090289300 | Sasaki et al. | Nov 2009 | A1 |
| 20090302434 | Pallem et al. | Dec 2009 | A1 |
| 20090304558 | Patton | Dec 2009 | A1 |
| 20090308315 | de Ridder | Dec 2009 | A1 |
| 20090308425 | Yednak | Dec 2009 | A1 |
| 20090311857 | Todd et al. | Dec 2009 | A1 |
| 20090315093 | Li et al. | Dec 2009 | A1 |
| 20090320754 | Oya | Dec 2009 | A1 |
| 20090324971 | De Vries et al. | Dec 2009 | A1 |
| 20090325391 | De Vusser et al. | Dec 2009 | A1 |
| 20090325469 | Koo et al. | Dec 2009 | A1 |
| 20100001409 | Humbert et al. | Jan 2010 | A1 |
| 20100003406 | Lam et al. | Jan 2010 | A1 |
| 20100006031 | Choi et al. | Jan 2010 | A1 |
| 20100006923 | Fujitsuka | Jan 2010 | A1 |
| 20100014479 | Kim | Jan 2010 | A1 |
| 20100015813 | McGinnis et al. | Jan 2010 | A1 |
| 20100018460 | Singh et al. | Jan 2010 | A1 |
| 20100024727 | Kim et al. | Feb 2010 | A1 |
| 20100024872 | Kishimoto | Feb 2010 | A1 |
| 20100025796 | Dabiran | Feb 2010 | A1 |
| 20100032587 | Hosch et al. | Feb 2010 | A1 |
| 20100032842 | Herdt et al. | Feb 2010 | A1 |
| 20100040441 | Obikane | Feb 2010 | A1 |
| 20100041179 | Lee | Feb 2010 | A1 |
| 20100041243 | Cheng et al. | Feb 2010 | A1 |
| 20100050943 | Kato et al. | Mar 2010 | A1 |
| 20100051597 | Morita et al. | Mar 2010 | A1 |
| 20100055312 | Kato et al. | Mar 2010 | A1 |
| 20100055442 | Kellock | Mar 2010 | A1 |
| 20100058984 | Marubayashi | Mar 2010 | A1 |
| 20100065758 | Liu et al. | Mar 2010 | A1 |
| 20100068009 | Kimura | Mar 2010 | A1 |
| 20100068891 | Hatanaka et al. | Mar 2010 | A1 |
| 20100075037 | Marsh et al. | Mar 2010 | A1 |
| 20100075507 | Chang et al. | Mar 2010 | A1 |
| 20100081094 | Hasebe et al. | Apr 2010 | A1 |
| 20100089320 | Kim | Apr 2010 | A1 |
| 20100089870 | Hiroshima et al. | Apr 2010 | A1 |
| 20100090149 | Thompson et al. | Apr 2010 | A1 |
| 20100092696 | Shinriki | Apr 2010 | A1 |
| 20100093187 | Lee et al. | Apr 2010 | A1 |
| 20100098862 | Xu et al. | Apr 2010 | A1 |
| 20100102417 | Ganguli et al. | Apr 2010 | A1 |
| 20100105936 | Tada et al. | Apr 2010 | A1 |
| 20100112496 | Nakajima et al. | May 2010 | A1 |
| 20100116207 | Givens | May 2010 | A1 |
| 20100116209 | Kato | May 2010 | A1 |
| 20100124610 | Aikawa et al. | May 2010 | A1 |
| 20100124618 | Kobayashi et al. | May 2010 | A1 |
| 20100124621 | Kobayashi et al. | May 2010 | A1 |
| 20100126415 | Ishino et al. | May 2010 | A1 |
| 20100126539 | Lee et al. | May 2010 | A1 |
| 20100126605 | Stones | May 2010 | A1 |
| 20100129990 | Nishizawa et al. | May 2010 | A1 |
| 20100130015 | Nakajima et al. | May 2010 | A1 |
| 20100130017 | Luo et al. | May 2010 | A1 |
| 20100130105 | Lee | May 2010 | A1 |
| 20100134023 | Mills | Jun 2010 | A1 |
| 20100136216 | Tsuei et al. | Jun 2010 | A1 |
| 20100140221 | Kikuchi et al. | Jun 2010 | A1 |
| 20100143609 | Fukazawa et al. | Jun 2010 | A1 |
| 20100144162 | Lee et al. | Jun 2010 | A1 |
| 20100144968 | Lee et al. | Jun 2010 | A1 |
| 20100145547 | Darabnia et al. | Jun 2010 | A1 |
| 20100151206 | Wu et al. | Jun 2010 | A1 |
| 20100159638 | Jeong | Jun 2010 | A1 |
| 20100162752 | Tabata et al. | Jul 2010 | A1 |
| 20100162956 | Murakami et al. | Jul 2010 | A1 |
| 20100163524 | Arai | Jul 2010 | A1 |
| 20100163937 | Clendenning | Jul 2010 | A1 |
| 20100168404 | Girolami et al. | Jul 2010 | A1 |
| 20100170441 | Won et al. | Jul 2010 | A1 |
| 20100170868 | Lin et al. | Jul 2010 | A1 |
| 20100173432 | White et al. | Jul 2010 | A1 |
| 20100178137 | Chintalapati et al. | Jul 2010 | A1 |
| 20100178423 | Shimizu et al. | Jul 2010 | A1 |
| 20100180819 | Hatanaka et al. | Jul 2010 | A1 |
| 20100183825 | Becker et al. | Jul 2010 | A1 |
| 20100184302 | Lee et al. | Jul 2010 | A1 |
| 20100186669 | Shin et al. | Jul 2010 | A1 |
| 20100193501 | Zucker et al. | Aug 2010 | A1 |
| 20100195392 | Freeman | Aug 2010 | A1 |
| 20100202860 | Reed | Aug 2010 | A1 |
| 20100221452 | Kang | Sep 2010 | A1 |
| 20100229795 | Tanabe | Sep 2010 | A1 |
| 20100230051 | Iizuka | Sep 2010 | A1 |
| 20100230863 | Moench et al. | Sep 2010 | A1 |
| 20100233885 | Kushibiki et al. | Sep 2010 | A1 |
| 20100233886 | Yang et al. | Sep 2010 | A1 |
| 20100236691 | Yamazaki | Sep 2010 | A1 |
| 20100243166 | Hayashi et al. | Sep 2010 | A1 |
| 20100244688 | Braun et al. | Sep 2010 | A1 |
| 20100248465 | Yi et al. | Sep 2010 | A1 |
| 20100255198 | Cleary et al. | Oct 2010 | A1 |
| 20100255218 | Oka et al. | Oct 2010 | A1 |
| 20100255625 | De Vries | Oct 2010 | A1 |
| 20100255658 | Aggarwal | Oct 2010 | A1 |
| 20100259152 | Yasuda et al. | Oct 2010 | A1 |
| 20100266765 | White et al. | Oct 2010 | A1 |
| 20100267248 | Ma et al. | Oct 2010 | A1 |
| 20100270675 | Harada | Oct 2010 | A1 |
| 20100246630 | Kaszynski et al. | Nov 2010 | A1 |
| 20100275846 | Kitagawa | Nov 2010 | A1 |
| 20100282163 | Aggarwal et al. | Nov 2010 | A1 |
| 20100282170 | Nishizawa | Nov 2010 | A1 |
| 20100282645 | Wang | Nov 2010 | A1 |
| 20100285237 | Ditizio et al. | Nov 2010 | A1 |
| 20100285319 | Kwak et al. | Nov 2010 | A1 |
| 20100294199 | Tran et al. | Nov 2010 | A1 |
| 20100297391 | Kley | Nov 2010 | A1 |
| 20100301752 | Bakre et al. | Dec 2010 | A1 |
| 20100304047 | Yang et al. | Dec 2010 | A1 |
| 20100307415 | Shero et al. | Dec 2010 | A1 |
| 20100317198 | Antonelli | Dec 2010 | A1 |
| 20100322604 | Fondurulia et al. | Dec 2010 | A1 |
| 20100326358 | Choi | Dec 2010 | A1 |
| 20110000619 | Suh | Jan 2011 | A1 |
| 20110006402 | Zhou | Jan 2011 | A1 |
| 20110006406 | Urbanowicz et al. | Jan 2011 | A1 |
| 20110014359 | Hashim | Jan 2011 | A1 |
| 20110014795 | Lee | Jan 2011 | A1 |
| 20110027725 | Tsutsumi et al. | Feb 2011 | A1 |
| 20110027999 | Sparks et al. | Feb 2011 | A1 |
| 20110034039 | Liang et al. | Feb 2011 | A1 |
| 20110045610 | van Schravendijk | Feb 2011 | A1 |
| 20110046314 | Klipp et al. | Feb 2011 | A1 |
| 20110048642 | Mihara et al. | Mar 2011 | A1 |
| 20110048769 | Fujwara | Mar 2011 | A1 |
| 20110049100 | Han et al. | Mar 2011 | A1 |
| 20110052833 | Hanawa et al. | Mar 2011 | A1 |
| 20110053383 | Shero et al. | Mar 2011 | A1 |
| 20110056513 | Hombach et al. | Mar 2011 | A1 |
| 20110056626 | Brown et al. | Mar 2011 | A1 |
| 20110057248 | Ma et al. | Mar 2011 | A1 |
| 20110061810 | Ganguly et al. | Mar 2011 | A1 |
| 20110070380 | Shero et al. | Mar 2011 | A1 |
| 20110081519 | Dillingh | Apr 2011 | A1 |
| 20110083496 | Lin et al. | Apr 2011 | A1 |
| 20110086516 | Lee et al. | Apr 2011 | A1 |
| 20110089469 | Merckling | Apr 2011 | A1 |
| 20110097901 | Banna et al. | Apr 2011 | A1 |
| 20110107512 | Gilbert | May 2011 | A1 |
| 20110108194 | Yoshioka et al. | May 2011 | A1 |
| 20110108741 | Ingram | May 2011 | A1 |
| 20110108929 | Meng | May 2011 | A1 |
| 20110117490 | Bae et al. | May 2011 | A1 |
| 20110117737 | Agarwala et al. | May 2011 | A1 |
| 20110117749 | Sheu | May 2011 | A1 |
| 20110124196 | Lee | May 2011 | A1 |
| 20110139272 | Matsumoto et al. | Jun 2011 | A1 |
| 20110139748 | Donnelly et al. | Jun 2011 | A1 |
| 20110140172 | Chu | Jun 2011 | A1 |
| 20110143032 | Vrtis et al. | Jun 2011 | A1 |
| 20110143461 | Fish et al. | Jun 2011 | A1 |
| 20110159202 | Matsushita | Jun 2011 | A1 |
| 20110159673 | Hanawa et al. | Jun 2011 | A1 |
| 20110159680 | Yoo | Jun 2011 | A1 |
| 20110168330 | Sakaue et al. | Jul 2011 | A1 |
| 20110171775 | Yamamoto et al. | Jul 2011 | A1 |
| 20110175011 | Ehrne et al. | Jul 2011 | A1 |
| 20110180233 | Bera et al. | Jul 2011 | A1 |
| 20110183079 | Jackson et al. | Jul 2011 | A1 |
| 20110183269 | Zhu | Jul 2011 | A1 |
| 20110183527 | Cho | Jul 2011 | A1 |
| 20110192820 | Yeom et al. | Aug 2011 | A1 |
| 20110198417 | Detmar et al. | Aug 2011 | A1 |
| 20110198736 | Shero et al. | Aug 2011 | A1 |
| 20110210468 | Shannon et al. | Sep 2011 | A1 |
| 20110220874 | Hanrath | Sep 2011 | A1 |
| 20110236600 | Fox et al. | Sep 2011 | A1 |
| 20110237040 | Ng et al. | Sep 2011 | A1 |
| 20110239936 | Suzaki et al. | Oct 2011 | A1 |
| 20110253044 | Tam et al. | Oct 2011 | A1 |
| 20110254052 | Kouvetakis | Oct 2011 | A1 |
| 20110256675 | Avouris | Oct 2011 | A1 |
| 20110256726 | Lavoie et al. | Oct 2011 | A1 |
| 20110256727 | Beynet et al. | Oct 2011 | A1 |
| 20110256734 | Hausmann et al. | Oct 2011 | A1 |
| 20110263107 | Chung et al. | Oct 2011 | A1 |
| 20110265549 | Cruse et al. | Nov 2011 | A1 |
| 20110265715 | Keller | Nov 2011 | A1 |
| 20110265725 | Tsuji | Nov 2011 | A1 |
| 20110265951 | Xu et al. | Nov 2011 | A1 |
| 20110275018 | Matteo et al. | Nov 2011 | A1 |
| 20110275166 | Shero et al. | Nov 2011 | A1 |
| 20110277690 | Rozenzon et al. | Nov 2011 | A1 |
| 20110281417 | Gordon et al. | Nov 2011 | A1 |
| 20110283933 | Makarov et al. | Nov 2011 | A1 |
| 20110291243 | Seamons | Dec 2011 | A1 |
| 20110294075 | Chen et al. | Dec 2011 | A1 |
| 20110294288 | Lee et al. | Dec 2011 | A1 |
| 20110298062 | Ganguli et al. | Dec 2011 | A1 |
| 20110300720 | Fu | Dec 2011 | A1 |
| 20110308453 | Su et al. | Dec 2011 | A1 |
| 20110308460 | Hong et al. | Dec 2011 | A1 |
| 20110312191 | Ohkura et al. | Dec 2011 | A1 |
| 20120003500 | Yoshida et al. | Jan 2012 | A1 |
| 20120006489 | Okita | Jan 2012 | A1 |
| 20120009802 | Lavoie | Jan 2012 | A1 |
| 20120024227 | Takasuka et al. | Feb 2012 | A1 |
| 20120024479 | Palagashvili et al. | Feb 2012 | A1 |
| 20120028454 | Swaminathan et al. | Feb 2012 | A1 |
| 20120031333 | Kurita et al. | Feb 2012 | A1 |
| 20120032311 | Gates | Feb 2012 | A1 |
| 20120033695 | Hayashi et al. | Feb 2012 | A1 |
| 20120036732 | Varadarajan | Feb 2012 | A1 |
| 20120040528 | Kim et al. | Feb 2012 | A1 |
| 20120043556 | Dube et al. | Feb 2012 | A1 |
| 20120046421 | Darling et al. | Feb 2012 | A1 |
| 20120052681 | Marsh | Mar 2012 | A1 |
| 20120058630 | Quinn | Mar 2012 | A1 |
| 20120064690 | Hirota et al. | Mar 2012 | A1 |
| 20120068242 | Shin et al. | Mar 2012 | A1 |
| 20120070136 | Koelmel et al. | Mar 2012 | A1 |
| 20120070997 | Larson | Mar 2012 | A1 |
| 20120074533 | Aoyama | Mar 2012 | A1 |
| 20120077349 | Li et al. | Mar 2012 | A1 |
| 20120080756 | Suzuki | Apr 2012 | A1 |
| 20120090704 | Laverdiere et al. | Apr 2012 | A1 |
| 20120098107 | Raisanen et al. | Apr 2012 | A1 |
| 20120100464 | Kageyama | Apr 2012 | A1 |
| 20120103264 | Choi et al. | May 2012 | A1 |
| 20120103522 | Hohenwater | May 2012 | A1 |
| 20120103939 | Wu et al. | May 2012 | A1 |
| 20120107607 | Takaki et al. | May 2012 | A1 |
| 20120108039 | Zajaji | May 2012 | A1 |
| 20120114877 | Lee | May 2012 | A1 |
| 20120115250 | Ariga et al. | May 2012 | A1 |
| 20120115257 | Matsuyam et al. | May 2012 | A1 |
| 20120119337 | Sasaki et al. | May 2012 | A1 |
| 20120121823 | Chhabra | May 2012 | A1 |
| 20120122275 | Koo et al. | May 2012 | A1 |
| 20120122302 | Weisman et al. | May 2012 | A1 |
| 20120128897 | Xiao et al. | May 2012 | A1 |
| 20120135145 | Je et al. | May 2012 | A1 |
| 20120149213 | Nittala | Jun 2012 | A1 |
| 20120156108 | Fondurulia et al. | Jun 2012 | A1 |
| 20120156890 | Yim et al. | Jun 2012 | A1 |
| 20120160172 | Wamura et al. | Jun 2012 | A1 |
| 20120161405 | Mohn | Jun 2012 | A1 |
| 20120164327 | Sato | Jun 2012 | A1 |
| 20120164837 | Tan et al. | Jun 2012 | A1 |
| 20120164842 | Watanabe | Jun 2012 | A1 |
| 20120170170 | Gros-Jean | Jul 2012 | A1 |
| 20120171391 | Won | Jul 2012 | A1 |
| 20120171874 | Thridandam et al. | Jul 2012 | A1 |
| 20120175751 | Gatineau | Jul 2012 | A1 |
| 20120180954 | Yang et al. | Jul 2012 | A1 |
| 20120183689 | Suzuki et al. | Jul 2012 | A1 |
| 20120187083 | Hashizume | Jul 2012 | A1 |
| 20120187305 | Elam et al. | Jul 2012 | A1 |
| 20120190178 | Wang et al. | Jul 2012 | A1 |
| 20120190185 | Rogers | Jul 2012 | A1 |
| 20120196048 | Ueda | Aug 2012 | A1 |
| 20120196450 | Balseanu et al. | Aug 2012 | A1 |
| 20120207456 | Kim et al. | Aug 2012 | A1 |
| 20120212121 | Lin | Aug 2012 | A1 |
| 20120214318 | Fukazawa et al. | Aug 2012 | A1 |
| 20120216743 | Itoh et al. | Aug 2012 | A1 |
| 20120219824 | Prolier | Aug 2012 | A1 |
| 20120220139 | Lee et al. | Aug 2012 | A1 |
| 20120225561 | Watanabe | Sep 2012 | A1 |
| 20120231771 | Marcus | Sep 2012 | A1 |
| 20120238074 | Santhanam et al. | Sep 2012 | A1 |
| 20120240858 | Taniyama et al. | Sep 2012 | A1 |
| 20120241411 | Darling et al. | Sep 2012 | A1 |
| 20120252229 | Timans et al. | Oct 2012 | A1 |
| 20120263876 | Haukka et al. | Oct 2012 | A1 |
| 20120264051 | Angelov et al. | Oct 2012 | A1 |
| 20120270339 | Xie et al. | Oct 2012 | A1 |
| 20120270393 | Pore et al. | Oct 2012 | A1 |
| 20120289053 | Holland et al. | Nov 2012 | A1 |
| 20120289057 | DeDontney | Nov 2012 | A1 |
| 20120295427 | Bauer | Nov 2012 | A1 |
| 20120304935 | Oosterlaken et al. | Dec 2012 | A1 |
| 20120305026 | Nomura et al. | Dec 2012 | A1 |
| 20120305196 | Mori et al. | Dec 2012 | A1 |
| 20120305987 | Hirler et al. | Dec 2012 | A1 |
| 20120310440 | Darabnia et al. | Dec 2012 | A1 |
| 20120315113 | Hiroki | Dec 2012 | A1 |
| 20120318334 | Bedell et al. | Dec 2012 | A1 |
| 20120321786 | Satitpunwaycha et al. | Dec 2012 | A1 |
| 20120322252 | Son et al. | Dec 2012 | A1 |
| 20120325148 | Yamagishi et al. | Dec 2012 | A1 |
| 20120328780 | Yamagishi et al. | Dec 2012 | A1 |
| 20130005122 | Schwarzenbach et al. | Jan 2013 | A1 |
| 20130011983 | Tsai | Jan 2013 | A1 |
| 20130014697 | Kanayama | Jan 2013 | A1 |
| 20130014896 | Shoji et al. | Jan 2013 | A1 |
| 20130019944 | Hekmatshoar-Tabai et al. | Jan 2013 | A1 |
| 20130019945 | Hekmatshoar-Tabai et al. | Jan 2013 | A1 |
| 20130020246 | Hoots et al. | Jan 2013 | A1 |
| 20130023129 | Reed | Jan 2013 | A1 |
| 20130025786 | Davidkovich et al. | Jan 2013 | A1 |
| 20130026451 | Bangsaruntip et al. | Jan 2013 | A1 |
| 20130037858 | Hong et al. | Feb 2013 | A1 |
| 20130037886 | Tsai et al. | Feb 2013 | A1 |
| 20130048606 | Mao et al. | Feb 2013 | A1 |
| 20130052585 | Ayothi et al. | Feb 2013 | A1 |
| 20130061755 | Frederick | Mar 2013 | A1 |
| 20130064973 | Chen et al. | Mar 2013 | A1 |
| 20130065189 | Yoshii et al. | Mar 2013 | A1 |
| 20130068727 | Okita | Mar 2013 | A1 |
| 20130068970 | Matsushita | Mar 2013 | A1 |
| 20130069052 | Sandhu | Mar 2013 | A1 |
| 20130078392 | Xiao et al. | Mar 2013 | A1 |
| 20130081702 | Mohammed et al. | Apr 2013 | A1 |
| 20130082274 | Yang | Apr 2013 | A1 |
| 20130084156 | Shimamoto | Apr 2013 | A1 |
| 20130084714 | Oka et al. | Apr 2013 | A1 |
| 20130089716 | Krishnamurthy et al. | Apr 2013 | A1 |
| 20130095664 | Matero et al. | Apr 2013 | A1 |
| 20130095973 | Kroneberger et al. | Apr 2013 | A1 |
| 20130104988 | Yednak et al. | May 2013 | A1 |
| 20130104992 | Yednak et al. | May 2013 | A1 |
| 20130115383 | Lu et al. | May 2013 | A1 |
| 20130115763 | Takamure et al. | May 2013 | A1 |
| 20130115768 | Pore et al. | May 2013 | A1 |
| 20130119018 | Kanarik et al. | May 2013 | A1 |
| 20130122712 | Kim et al. | May 2013 | A1 |
| 20130126515 | Shero et al. | May 2013 | A1 |
| 20130129577 | Halpin et al. | May 2013 | A1 |
| 20130134148 | Tachikawa | May 2013 | A1 |
| 20130143401 | Yu et al. | Jun 2013 | A1 |
| 20130157409 | Vaidya | Jun 2013 | A1 |
| 20130160709 | White | Jun 2013 | A1 |
| 20130161629 | Han et al. | Jun 2013 | A1 |
| 20130168354 | Kanarik | Jul 2013 | A1 |
| 20130171818 | Kim et al. | Jul 2013 | A1 |
| 20130175596 | Cheng et al. | Jul 2013 | A1 |
| 20130180448 | Sakaue et al. | Jul 2013 | A1 |
| 20130183814 | Huang et al. | Jul 2013 | A1 |
| 20130189854 | Hausmann et al. | Jul 2013 | A1 |
| 20130196507 | Ma et al. | Aug 2013 | A1 |
| 20130203266 | Hintze | Aug 2013 | A1 |
| 20130209940 | Sakamoto et al. | Aug 2013 | A1 |
| 20130210241 | Lavoie et al. | Aug 2013 | A1 |
| 20130214232 | Tendulkar et al. | Aug 2013 | A1 |
| 20130217239 | Mallick et al. | Aug 2013 | A1 |
| 20130217240 | Mallick et al. | Aug 2013 | A1 |
| 20130217241 | Underwood et al. | Aug 2013 | A1 |
| 20130217243 | Underwood et al. | Aug 2013 | A1 |
| 20130224964 | Fukazawa | Aug 2013 | A1 |
| 20130230814 | Dunn et al. | Sep 2013 | A1 |
| 20130256265 | Darling et al. | Oct 2013 | A1 |
| 20130256838 | Sanchez et al. | Oct 2013 | A1 |
| 20130256962 | Ranish | Oct 2013 | A1 |
| 20130264659 | Jung | Oct 2013 | A1 |
| 20130269612 | Cheng et al. | Oct 2013 | A1 |
| 20130270676 | Lindert et al. | Oct 2013 | A1 |
| 20130276978 | Bluck et al. | Oct 2013 | A1 |
| 20130285155 | Glass | Oct 2013 | A1 |
| 20130287526 | Bluck et al. | Oct 2013 | A1 |
| 20130288427 | Hung | Oct 2013 | A1 |
| 20130288480 | Sanchez et al. | Oct 2013 | A1 |
| 20130288485 | Liang et al. | Oct 2013 | A1 |
| 20130292047 | Tian et al. | Nov 2013 | A1 |
| 20130292676 | Milligan et al. | Nov 2013 | A1 |
| 20130292807 | Raisanen et al. | Nov 2013 | A1 |
| 20130295779 | Chandra et al. | Nov 2013 | A1 |
| 20130302999 | Won et al. | Nov 2013 | A1 |
| 20130303803 | Doerr et al. | Nov 2013 | A1 |
| 20130313656 | Tong | Nov 2013 | A1 |
| 20130319290 | Xiao et al. | Dec 2013 | A1 |
| 20130320429 | Thomas | Dec 2013 | A1 |
| 20130323435 | Xiao et al. | Dec 2013 | A1 |
| 20130330165 | Wimplinger | Dec 2013 | A1 |
| 20130330911 | Huang et al. | Dec 2013 | A1 |
| 20130330933 | Fukazawa et al. | Dec 2013 | A1 |
| 20130333619 | Omari | Dec 2013 | A1 |
| 20130337583 | Kobayashi et al. | Dec 2013 | A1 |
| 20130337653 | Kovalgin et al. | Dec 2013 | A1 |
| 20130340619 | Tammera | Dec 2013 | A1 |
| 20130344248 | Clark | Dec 2013 | A1 |
| 20140000843 | Dunn et al. | Jan 2014 | A1 |
| 20140001520 | Glass | Jan 2014 | A1 |
| 20140004274 | Thompson | Jan 2014 | A1 |
| 20140014642 | Elliot et al. | Jan 2014 | A1 |
| 20140014644 | Akiba et al. | Jan 2014 | A1 |
| 20140015186 | Wessel et al. | Jan 2014 | A1 |
| 20140020619 | Vincent et al. | Jan 2014 | A1 |
| 20140023794 | Mahajani et al. | Jan 2014 | A1 |
| 20140027884 | Tang et al. | Jan 2014 | A1 |
| 20140033978 | Adachi et al. | Feb 2014 | A1 |
| 20140036274 | Marquardt et al. | Feb 2014 | A1 |
| 20140047705 | Singh | Feb 2014 | A1 |
| 20140048765 | Ma et al. | Feb 2014 | A1 |
| 20140056679 | Yamabe et al. | Feb 2014 | A1 |
| 20140056770 | Bedard et al. | Feb 2014 | A1 |
| 20140057454 | Subramonium | Feb 2014 | A1 |
| 20140058179 | Stevens et al. | Feb 2014 | A1 |
| 20140060147 | Sarin et al. | Mar 2014 | A1 |
| 20140061770 | Lee | Mar 2014 | A1 |
| 20140062304 | Nakano et al. | Mar 2014 | A1 |
| 20140065841 | Matero | Mar 2014 | A1 |
| 20140067110 | Lawson et al. | Mar 2014 | A1 |
| 20140073143 | Alokozai et al. | Mar 2014 | A1 |
| 20140076861 | Cornelius et al. | Mar 2014 | A1 |
| 20140077240 | Roucka et al. | Mar 2014 | A1 |
| 20140084341 | Weeks | Mar 2014 | A1 |
| 20140087544 | Tolle | Mar 2014 | A1 |
| 20140094027 | Azumo et al. | Apr 2014 | A1 |
| 20140096716 | Chung et al. | Apr 2014 | A1 |
| 20140097468 | Okita | Apr 2014 | A1 |
| 20140099798 | Tsuji | Apr 2014 | A1 |
| 20140103145 | White et al. | Apr 2014 | A1 |
| 20140106574 | Kang et al. | Apr 2014 | A1 |
| 20140110798 | Cai | Apr 2014 | A1 |
| 20140113457 | Sims | Apr 2014 | A1 |
| 20140116335 | Tsuji et al. | May 2014 | A1 |
| 20140117380 | Loboda et al. | May 2014 | A1 |
| 20140120487 | Kaneko | May 2014 | A1 |
| 20140120723 | Fu et al. | May 2014 | A1 |
| 20140120738 | Jung | May 2014 | A1 |
| 20140127907 | Yang | May 2014 | A1 |
| 20140138779 | Xie et al. | May 2014 | A1 |
| 20140141625 | Fukazawa et al. | May 2014 | A1 |
| 20140144500 | Cao et al. | May 2014 | A1 |
| 20140158786 | Santo | Jun 2014 | A1 |
| 20140159170 | Raisanen et al. | Jun 2014 | A1 |
| 20140167187 | Kuo et al. | Jun 2014 | A1 |
| 20140174354 | Arai | Jun 2014 | A1 |
| 20140175054 | Carlson et al. | Jun 2014 | A1 |
| 20140182053 | Huang | Jul 2014 | A1 |
| 20140191389 | Lee et al. | Jul 2014 | A1 |
| 20140193983 | Lavoie | Jul 2014 | A1 |
| 20140202386 | Taga | Jul 2014 | A1 |
| 20140202388 | Um et al. | Jul 2014 | A1 |
| 20140209976 | Yang et al. | Jul 2014 | A1 |
| 20140217065 | Winkler et al. | Aug 2014 | A1 |
| 20140220247 | Haukka et al. | Aug 2014 | A1 |
| 20140225065 | Rachmady et al. | Aug 2014 | A1 |
| 20140227072 | Lee et al. | Aug 2014 | A1 |
| 20140227861 | Wu et al. | Aug 2014 | A1 |
| 20140227881 | Lubomirsky et al. | Aug 2014 | A1 |
| 20140234550 | Winter et al. | Aug 2014 | A1 |
| 20140245948 | Nguyen et al. | Sep 2014 | A1 |
| 20140251953 | Winkler et al. | Sep 2014 | A1 |
| 20140251954 | Winkler et al. | Sep 2014 | A1 |
| 20140252134 | Chen | Sep 2014 | A1 |
| 20140252479 | Utomo et al. | Sep 2014 | A1 |
| 20140260684 | Christmann | Sep 2014 | A1 |
| 20140264902 | Ting et al. | Sep 2014 | A1 |
| 20140272194 | Xiao et al. | Sep 2014 | A1 |
| 20140273428 | Shero | Sep 2014 | A1 |
| 20140273477 | Niskanen | Sep 2014 | A1 |
| 20140273510 | Chen et al. | Sep 2014 | A1 |
| 20140273528 | Niskanen | Sep 2014 | A1 |
| 20140273530 | Nguyen | Sep 2014 | A1 |
| 20140273531 | Niskanen | Sep 2014 | A1 |
| 20140283747 | Kasai et al. | Sep 2014 | A1 |
| 20140346142 | Chapuis et al. | Nov 2014 | A1 |
| 20140346650 | Raisanen et al. | Nov 2014 | A1 |
| 20140349033 | Nonaka et al. | Nov 2014 | A1 |
| 20140363980 | Kawamata et al. | Dec 2014 | A1 |
| 20140363983 | Nakano et al. | Dec 2014 | A1 |
| 20140363985 | Jang et al. | Dec 2014 | A1 |
| 20140367043 | Bishara et al. | Dec 2014 | A1 |
| 20140367642 | Guo | Dec 2014 | A1 |
| 20140377960 | Koiwa | Dec 2014 | A1 |
| 20150004316 | Thompson et al. | Jan 2015 | A1 |
| 20150004317 | Dussarrat et al. | Jan 2015 | A1 |
| 20150004798 | Chandrasekharan et al. | Jan 2015 | A1 |
| 20150007770 | Chandrasekharan et al. | Jan 2015 | A1 |
| 20150010381 | Cai | Jan 2015 | A1 |
| 20150014632 | Kim et al. | Jan 2015 | A1 |
| 20150014823 | Mallikarjunan et al. | Jan 2015 | A1 |
| 20150017794 | Takamure | Jan 2015 | A1 |
| 20150021599 | Ridgeway | Jan 2015 | A1 |
| 20150024609 | Milligan et al. | Jan 2015 | A1 |
| 20150041431 | Zafiropoulo et al. | Feb 2015 | A1 |
| 20150048485 | Tolle | Feb 2015 | A1 |
| 20150056815 | Fernandez | Feb 2015 | A1 |
| 20150072509 | Chi et al. | Mar 2015 | A1 |
| 20150078874 | Sansoni | Mar 2015 | A1 |
| 20150079311 | Nakano | Mar 2015 | A1 |
| 20150086316 | Greenberg | Mar 2015 | A1 |
| 20150087154 | Guha et al. | Mar 2015 | A1 |
| 20150091057 | Xie et al. | Apr 2015 | A1 |
| 20150096973 | Dunn et al. | Apr 2015 | A1 |
| 20150099065 | Canizares et al. | Apr 2015 | A1 |
| 20150099072 | Takamure et al. | Apr 2015 | A1 |
| 20150099342 | Tsai | Apr 2015 | A1 |
| 20150102466 | Colinge | Apr 2015 | A1 |
| 20150111374 | Bao | Apr 2015 | A1 |
| 20150111395 | Hashimoto et al. | Apr 2015 | A1 |
| 20150122180 | Chang et al. | May 2015 | A1 |
| 20150132212 | Winkler et al. | May 2015 | A1 |
| 20150140210 | Jung et al. | May 2015 | A1 |
| 20150147483 | Fukazawa | May 2015 | A1 |
| 20150147488 | Choi et al. | May 2015 | A1 |
| 20150147877 | Jung | May 2015 | A1 |
| 20150162168 | Oehrlien | Jun 2015 | A1 |
| 20150162185 | Pore | Jun 2015 | A1 |
| 20150162214 | Thompson | Jun 2015 | A1 |
| 20150167159 | Halpin et al. | Jun 2015 | A1 |
| 20150170914 | Haukka et al. | Jun 2015 | A1 |
| 20150170947 | Bluck | Jun 2015 | A1 |
| 20150170954 | Agarwal | Jun 2015 | A1 |
| 20150171177 | Cheng et al. | Jun 2015 | A1 |
| 20150174768 | Rodnick | Jun 2015 | A1 |
| 20150179501 | Jhaveri et al. | Jun 2015 | A1 |
| 20150179564 | Lee et al. | Jun 2015 | A1 |
| 20150184291 | Alokozai et al. | Jul 2015 | A1 |
| 20150187559 | Sano | Jul 2015 | A1 |
| 20150187568 | Pettinger et al. | Jul 2015 | A1 |
| 20150217330 | Haukka | Aug 2015 | A1 |
| 20150217456 | Tsuji et al. | Aug 2015 | A1 |
| 20150218695 | Odedra | Aug 2015 | A1 |
| 20150225850 | Arora et al. | Aug 2015 | A1 |
| 20150228572 | Yang et al. | Aug 2015 | A1 |
| 20150240359 | Jdira et al. | Aug 2015 | A1 |
| 20150243542 | Yoshihara et al. | Aug 2015 | A1 |
| 20150243545 | Tang | Aug 2015 | A1 |
| 20150243658 | Joshi et al. | Aug 2015 | A1 |
| 20150255385 | Lee et al. | Sep 2015 | A1 |
| 20150259790 | Newman | Sep 2015 | A1 |
| 20150263033 | Aoyama | Sep 2015 | A1 |
| 20150267295 | Hill et al. | Sep 2015 | A1 |
| 20150267297 | Shiba | Sep 2015 | A1 |
| 20150267298 | Saitou et al. | Sep 2015 | A1 |
| 20150267299 | Hawkins | Sep 2015 | A1 |
| 20150267301 | Hill et al. | Sep 2015 | A1 |
| 20150270140 | Gupta et al. | Sep 2015 | A1 |
| 20150270146 | Yoshihara et al. | Sep 2015 | A1 |
| 20150279681 | Knoops | Oct 2015 | A1 |
| 20150279708 | Kobayashi et al. | Oct 2015 | A1 |
| 20150284848 | Nakano et al. | Oct 2015 | A1 |
| 20150287626 | Arai | Oct 2015 | A1 |
| 20150287710 | Yun et al. | Oct 2015 | A1 |
| 20150292088 | Canizares | Oct 2015 | A1 |
| 20150299848 | Haukka | Oct 2015 | A1 |
| 20150308586 | Shugrue et al. | Oct 2015 | A1 |
| 20150303056 | Varadarajan et al. | Nov 2015 | A1 |
| 20150315704 | Nakano et al. | Nov 2015 | A1 |
| 20150340247 | Balakrishnan et al. | Nov 2015 | A1 |
| 20150340500 | Brunco | Nov 2015 | A1 |
| 20150343741 | Shibata et al. | Dec 2015 | A1 |
| 20150348755 | Han et al. | Dec 2015 | A1 |
| 20150361553 | Murakawa | Dec 2015 | A1 |
| 20150364371 | Yen | Dec 2015 | A1 |
| 20150367253 | Kanyal et al. | Dec 2015 | A1 |
| 20150376211 | Girard | Dec 2015 | A1 |
| 20150376785 | Knaapen et al. | Dec 2015 | A1 |
| 20150380296 | Antonelli et al. | Dec 2015 | A1 |
| 20160013022 | Ayoub | Jan 2016 | A1 |
| 20160013024 | Milligan et al. | Jan 2016 | A1 |
| 20160020092 | Kang | Jan 2016 | A1 |
| 20160024656 | White et al. | Jan 2016 | A1 |
| 20160035566 | LaVoie | Feb 2016 | A1 |
| 20160051964 | Tolle et al. | Feb 2016 | A1 |
| 20160056074 | Na | Feb 2016 | A1 |
| 20160079054 | Chen et al. | Mar 2016 | A1 |
| 20160097123 | Shugrue et al. | Apr 2016 | A1 |
| 20160099150 | Tsai | Apr 2016 | A1 |
| 20160102214 | Dietz et al. | Apr 2016 | A1 |
| 20160111272 | Girard | Apr 2016 | A1 |
| 20160111438 | Tsutsumi et al. | Apr 2016 | A1 |
| 20160115590 | Haukka et al. | Apr 2016 | A1 |
| 20160133307 | Lee et al. | May 2016 | A1 |
| 20160133628 | Xie | May 2016 | A1 |
| 20160141172 | Kang | May 2016 | A1 |
| 20160145738 | Liu et al. | May 2016 | A1 |
| 20160148811 | Nakatani et al. | May 2016 | A1 |
| 20160148821 | Singh | May 2016 | A1 |
| 20160155629 | Hawryluk et al. | Jun 2016 | A1 |
| 20160163556 | Briggs et al. | Jun 2016 | A1 |
| 20160163561 | Hudson et al. | Jun 2016 | A1 |
| 20160163711 | Arndt et al. | Jun 2016 | A1 |
| 20160168699 | Fukazawa et al. | Jun 2016 | A1 |
| 20160181128 | Mori | Jun 2016 | A1 |
| 20160181368 | Weeks | Jun 2016 | A1 |
| 20160190137 | Tsai et al. | Jun 2016 | A1 |
| 20160211135 | Noda et al. | Jul 2016 | A1 |
| 20160211147 | Fukazawa | Jul 2016 | A1 |
| 20160217857 | Paudel | Jul 2016 | A1 |
| 20160225607 | Yamamoto et al. | Aug 2016 | A1 |
| 20160245704 | Osaka et al. | Aug 2016 | A1 |
| 20160256187 | Shelton et al. | Sep 2016 | A1 |
| 20160268102 | White | Sep 2016 | A1 |
| 20160268107 | White | Sep 2016 | A1 |
| 20160276148 | Qian et al. | Sep 2016 | A1 |
| 20160284542 | Noda et al. | Sep 2016 | A1 |
| 20160289828 | Shero et al. | Oct 2016 | A1 |
| 20160293398 | Danek et al. | Oct 2016 | A1 |
| 20160307766 | Jongbloed et al. | Oct 2016 | A1 |
| 20160312360 | Rasheed et al. | Oct 2016 | A1 |
| 20160314962 | Higashino | Oct 2016 | A1 |
| 20160314964 | Tang et al. | Oct 2016 | A1 |
| 20160334709 | Huli et al. | Nov 2016 | A1 |
| 20160358772 | Xie | Dec 2016 | A1 |
| 20160362783 | Tolle et al. | Dec 2016 | A1 |
| 20160362813 | Bao et al. | Dec 2016 | A1 |
| 20160365280 | Brink et al. | Dec 2016 | A1 |
| 20160372365 | Tang et al. | Dec 2016 | A1 |
| 20160372744 | Essaki et al. | Dec 2016 | A1 |
| 20160376700 | Haukka | Dec 2016 | A1 |
| 20160376704 | Raisanen | Dec 2016 | A1 |
| 20160379851 | Swaminathan et al. | Dec 2016 | A1 |
| 20160381732 | Moench et al. | Dec 2016 | A1 |
| 20170011889 | Winkler et al. | Jan 2017 | A1 |
| 20170011950 | Schmotzer | Jan 2017 | A1 |
| 20170018477 | Kato | Jan 2017 | A1 |
| 20170025280 | Milligan | Jan 2017 | A1 |
| 20170025291 | Lin | Jan 2017 | A1 |
| 20170029945 | Kamakura | Feb 2017 | A1 |
| 20170033004 | Siew et al. | Feb 2017 | A1 |
| 20170037513 | Haukka | Feb 2017 | A1 |
| 20170040164 | Wang et al. | Feb 2017 | A1 |
| 20170040206 | Schmotzer et al. | Feb 2017 | A1 |
| 20170047446 | Margetis et al. | Feb 2017 | A1 |
| 20170051408 | Kosuke et al. | Feb 2017 | A1 |
| 20170053811 | Fung et al. | Feb 2017 | A1 |
| 20170062204 | Suzuki et al. | Mar 2017 | A1 |
| 20170062209 | Shiba | Mar 2017 | A1 |
| 20170062258 | Bluck | Mar 2017 | A1 |
| 20170091320 | Psota et al. | Mar 2017 | A1 |
| 20170092469 | Kurita et al. | Mar 2017 | A1 |
| 20170092531 | Coomer | Mar 2017 | A1 |
| 20170092847 | Kim et al. | Mar 2017 | A1 |
| 20170100742 | Pore et al. | Apr 2017 | A1 |
| 20170103907 | Chu et al. | Apr 2017 | A1 |
| 20170107621 | Suemori | Apr 2017 | A1 |
| 20170110313 | Tang et al. | Apr 2017 | A1 |
| 20170114464 | Iriuda et al. | Apr 2017 | A1 |
| 20170117141 | Zhu et al. | Apr 2017 | A1 |
| 20170117202 | Tang et al. | Apr 2017 | A1 |
| 20170117203 | Tang et al. | Apr 2017 | A1 |
| 20170117222 | Kim et al. | Apr 2017 | A1 |
| 20170130332 | Stumpf | May 2017 | A1 |
| 20170136578 | Yoshimura | May 2017 | A1 |
| 20170154757 | Winkler et al. | Jun 2017 | A1 |
| 20170173696 | Sheinman | Jun 2017 | A1 |
| 20170178899 | Kabansky et al. | Jun 2017 | A1 |
| 20170186754 | Blomberg et al. | Jun 2017 | A1 |
| 20170191164 | Alokozai et al. | Jul 2017 | A1 |
| 20170196562 | Shelton | Jul 2017 | A1 |
| 20170216762 | Shugrue et al. | Aug 2017 | A1 |
| 20170232457 | Toshiki et al. | Aug 2017 | A1 |
| 20170243734 | Ishikawa et al. | Aug 2017 | A1 |
| 20170250068 | Ishikawa et al. | Aug 2017 | A1 |
| 20170250075 | Caymax et al. | Aug 2017 | A1 |
| 20170256429 | Lawson et al. | Sep 2017 | A1 |
| 20170260649 | Coomer | Sep 2017 | A1 |
| 20170263437 | Li et al. | Sep 2017 | A1 |
| 20170267527 | Kim et al. | Sep 2017 | A1 |
| 20170267531 | Huakka | Sep 2017 | A1 |
| 20170271256 | Inatsuka | Sep 2017 | A1 |
| 20170271501 | Avci et al. | Sep 2017 | A1 |
| 20170278707 | Margetis et al. | Sep 2017 | A1 |
| 20170287681 | Nitadori et al. | Oct 2017 | A1 |
| 20170294318 | Yoshida et al. | Oct 2017 | A1 |
| 20170306478 | Raisanen et al. | Oct 2017 | A1 |
| 20170306479 | Raisanen et al. | Oct 2017 | A1 |
| 20170306480 | Zhu et al. | Oct 2017 | A1 |
| 20170316933 | Xie et al. | Nov 2017 | A1 |
| 20170316940 | Ishikawa et al. | Nov 2017 | A1 |
| 20170317194 | Tang et al. | Nov 2017 | A1 |
| 20170338192 | Lee et al. | Nov 2017 | A1 |
| 20170342559 | Fukazawa et al. | Nov 2017 | A1 |
| 20170343896 | Darling et al. | Nov 2017 | A1 |
| 20170358670 | Kub et al. | Dec 2017 | A1 |
| 20170372884 | Margetis et al. | Dec 2017 | A1 |
| 20180010247 | Niskanen | Jan 2018 | A1 |
| 20180025890 | Choi | Jan 2018 | A1 |
| 20180025939 | Kovalgin et al. | Jan 2018 | A1 |
| 20180033616 | Masaru | Feb 2018 | A1 |
| 20180033625 | Yoo | Feb 2018 | A1 |
| 20180033645 | Saido et al. | Feb 2018 | A1 |
| 20180033674 | Jeong | Feb 2018 | A1 |
| 20180033679 | Pore | Feb 2018 | A1 |
| 20180040746 | Johnson et al. | Feb 2018 | A1 |
| 20180047749 | Kim | Feb 2018 | A1 |
| 20180057937 | Lee et al. | Mar 2018 | A1 |
| 20180061628 | Ou et al. | Mar 2018 | A1 |
| 20180061851 | Ootsuka | Mar 2018 | A1 |
| 20180069019 | Kim et al. | Mar 2018 | A1 |
| 20180076021 | Fukushima et al. | Mar 2018 | A1 |
| 20180083435 | Redler | Mar 2018 | A1 |
| 20180087152 | Yoshida | Mar 2018 | A1 |
| 20180087154 | Pore et al. | Mar 2018 | A1 |
| 20180087156 | Kohei et al. | Mar 2018 | A1 |
| 20180102276 | Zhu et al. | Apr 2018 | A1 |
| 20180105930 | Kang et al. | Apr 2018 | A1 |
| 20180108587 | Jiang | Apr 2018 | A1 |
| 20180114680 | Kim et al. | Apr 2018 | A1 |
| 20180119283 | Fukazawa | May 2018 | A1 |
| 20180122642 | Raisanen | May 2018 | A1 |
| 20180122709 | Xie | May 2018 | A1 |
| 20180122959 | Calka et al. | May 2018 | A1 |
| 20180127876 | Tolle | May 2018 | A1 |
| 20180130652 | Pettinger et al. | May 2018 | A1 |
| 20180130701 | Chun | May 2018 | A1 |
| 20180135173 | Kim et al. | May 2018 | A1 |
| 20180135179 | Toshiyuki et al. | May 2018 | A1 |
| 20180142353 | Tetsuya et al. | May 2018 | A1 |
| 20180142357 | Yoshikazu | May 2018 | A1 |
| 20180151346 | Blanquart | May 2018 | A1 |
| 20180151358 | Margetis et al. | May 2018 | A1 |
| 20180158688 | Chen | Jun 2018 | A1 |
| 20180166258 | Kim et al. | Jun 2018 | A1 |
| 20180166315 | Coomer | Jun 2018 | A1 |
| 20180171475 | Maes et al. | Jun 2018 | A1 |
| 20180171477 | Kim et al. | Jun 2018 | A1 |
| 20180174826 | Raaijmakers et al. | Jun 2018 | A1 |
| 20180182613 | Blanquart et al. | Jun 2018 | A1 |
| 20180182618 | Blanquart et al. | Jun 2018 | A1 |
| 20180189923 | Zhong et al. | Jul 2018 | A1 |
| 20180195174 | Kim et al. | Jul 2018 | A1 |
| 20180223429 | Fukazawa et al. | Aug 2018 | A1 |
| 20180233372 | Vayrynen et al. | Aug 2018 | A1 |
| 20180286663 | Kobayashi et al. | Oct 2018 | A1 |
| 20180286675 | Blomberg et al. | Oct 2018 | A1 |
| 20180286711 | Oosterlaken et al. | Oct 2018 | A1 |
| Number | Date | Country |
|---|---|---|
| 2588350 | Nov 2003 | CN |
| 1563483 | Jan 2005 | CN |
| 1664987 | Sep 2005 | CN |
| 1825535 | Aug 2006 | CN |
| 101330015 | Dec 2008 | CN |
| 101522943 | Sep 2009 | CN |
| 101681873 | Mar 2010 | CN |
| 101423937 | Sep 2011 | CN |
| 102383106 | Mar 2012 | CN |
| 102008052750 | Jun 2009 | DE |
| 0887632 | Dec 1998 | EP |
| 1889817 | Feb 2008 | EP |
| 2036600 | Mar 2009 | EP |
| 2426233 | Jul 2012 | EP |
| 1408266 | Aug 1965 | FR |
| 2233614 | Jan 1975 | FR |
| 752-277 | Jul 1956 | GB |
| 58-19462 | Apr 1983 | JP |
| 59-211779 | Nov 1984 | JP |
| 61038863 | Feb 1986 | JP |
| H01296613 | Nov 1989 | JP |
| H0293071 | Apr 1990 | JP |
| H02-185038 | Jul 1990 | JP |
| 03-044472 | Feb 1991 | JP |
| H03-044472 | Feb 1991 | JP |
| H03-155625 | Jul 1991 | JP |
| H03-248427 | Nov 1991 | JP |
| H04029313 | Jan 1992 | JP |
| H04-115531 | Apr 1992 | JP |
| H04115531 | Apr 1992 | JP |
| H05-23079 | Mar 1993 | JP |
| H05-118928 | May 1993 | JP |
| H05-171446 | Jul 1993 | JP |
| H06-053210 | Feb 1994 | JP |
| H0684888 | Mar 1994 | JP |
| H06-338497 | Dec 1994 | JP |
| H0729836 | Jan 1995 | JP |
| H07297271 | Jan 1995 | JP |
| H07-109576 | Apr 1995 | JP |
| 07-034936 | Aug 1995 | JP |
| H07-034936 | Aug 1995 | JP |
| 7-272694 | Oct 1995 | JP |
| H07-283149 | Oct 1995 | JP |
| H07283149 | Oct 1995 | JP |
| H07-209093 | Nov 1995 | JP |
| 08-181135 | Jul 1996 | JP |
| H08181135 | Jul 1996 | JP |
| H08-335558 | Dec 1996 | JP |
| H08335558 | Dec 1996 | JP |
| 9-89676 | Apr 1997 | JP |
| H09148322 | Jun 1997 | JP |
| H10041096 | Feb 1998 | JP |
| 10-064696 | Mar 1998 | JP |
| H10-064696 | Mar 1998 | JP |
| H10-153494 | Jun 1998 | JP |
| H10-227703 | Aug 1998 | JP |
| 10-0261620 | Sep 1998 | JP |
| H10-0261620 | Sep 1998 | JP |
| 2845163 | Jan 1999 | JP |
| H11-097163 | Apr 1999 | JP |
| H11-118615 | Apr 1999 | JP |
| H11-183264 | Jul 1999 | JP |
| H11-183265 | Jul 1999 | JP |
| H11-195688 | Jul 1999 | JP |
| H11-287715 | Oct 1999 | JP |
| 2001-15698 | Jan 2001 | JP |
| 2001015698 | Jan 2001 | JP |
| 2001023872 | Jan 2001 | JP |
| 2001207265 | Jul 2001 | JP |
| 2001207268 | Jul 2001 | JP |
| 2001210602 | Aug 2001 | JP |
| 2001220677 | Aug 2001 | JP |
| 2001342570 | Dec 2001 | JP |
| 2002164342 | Jun 2002 | JP |
| 2002170781 | Jun 2002 | JP |
| 2003035574 | Feb 2003 | JP |
| 2003133300 | May 2003 | JP |
| 2003153706 | May 2003 | JP |
| 2003303814 | Oct 2003 | JP |
| 2004014952 | Jan 2004 | JP |
| 2004023043 | Jan 2004 | JP |
| 2004091848 | Mar 2004 | JP |
| 2004113270 | Apr 2004 | JP |
| 2004128019 | Apr 2004 | JP |
| 2004134553 | Apr 2004 | JP |
| 2004294638 | Oct 2004 | JP |
| 2004310019 | Nov 2004 | JP |
| 2004538374 | Dec 2004 | JP |
| 2005033221 | Feb 2005 | JP |
| 2005079254 | Mar 2005 | JP |
| 2005507030 | Mar 2005 | JP |
| 2005172489 | Jun 2005 | JP |
| 2006059931 | Mar 2006 | JP |
| 2006090762 | Apr 2006 | JP |
| 2006153706 | Jun 2006 | JP |
| 2006186271 | Jul 2006 | JP |
| 2006188729 | Jul 2006 | JP |
| 2006278058 | Oct 2006 | JP |
| 2006319261 | Nov 2006 | JP |
| 2007027777 | Feb 2007 | JP |
| 3140111 | Mar 2008 | JP |
| 2008060304 | Mar 2008 | JP |
| 2008066159 | Mar 2008 | JP |
| 2008172083 | Jul 2008 | JP |
| 2008527748 | Jul 2008 | JP |
| 2008202107 | Sep 2008 | JP |
| 2009016815 | Jan 2009 | JP |
| 2009088421 | Apr 2009 | JP |
| 2009239082 | Apr 2009 | JP |
| 2009099938 | May 2009 | JP |
| 2009194248 | Aug 2009 | JP |
| 2009251216 | Oct 2009 | JP |
| 2010067940 | Mar 2010 | JP |
| 2010097834 | Apr 2010 | JP |
| 2010205967 | Sep 2010 | JP |
| 2010251444 | Oct 2010 | JP |
| 2011049592 | Mar 2011 | JP |
| 2011162830 | Aug 2011 | JP |
| 2011181681 | Sep 2011 | JP |
| 2012089837 | May 2012 | JP |
| 2012146939 | Aug 2012 | JP |
| 2013026479 | Feb 2013 | JP |
| 2013235912 | Nov 2013 | JP |
| 2014522104 | Aug 2014 | JP |
| 2016174158 | Sep 2016 | JP |
| 10-2000-0031098 | Jun 2000 | KR |
| 10-2000-0045257 | Jul 2000 | KR |
| 10-0295043 | Apr 2001 | KR |
| 10-2002-0064028 | Aug 2002 | KR |
| 2002-0086763 | Nov 2002 | KR |
| 10-0377095 | Mar 2003 | KR |
| 2003-0092305 | Dec 2003 | KR |
| 10-2005-0054122 | Jun 2005 | KR |
| 10-0547248 | Jan 2006 | KR |
| 10-0593960 | Jun 2006 | KR |
| 10-0688484 | Feb 2007 | KR |
| 10-2007-0084683 | Aug 2007 | KR |
| 10-2009-0055443 | Jun 2009 | KR |
| 10-2010-0020834 | Feb 2010 | KR |
| 20100020834 | Feb 2010 | KR |
| 10-2010-0032812 | Mar 2010 | KR |
| 20100032812 | Mar 2010 | KR |
| 10-1114219 | Mar 2012 | KR |
| 10-1535573 | Jul 2015 | KR |
| 538327 | Jun 2003 | TW |
| I226380 | Jan 2005 | TW |
| M292692 | Jun 2006 | TW |
| 200701301 | Jan 2007 | TW |
| 200731357 | Aug 2007 | TW |
| 201247690 | Dec 2012 | TW |
| 201330086 | Jul 2013 | TW |
| 1996017107 | Jun 1996 | WO |
| 1997003223 | Jan 1997 | WO |
| 1998032893 | Jul 1998 | WO |
| 1999023690 | May 1999 | WO |
| DM048579 | Jul 1999 | WO |
| 2004008491 | Jul 2002 | WO |
| 2004008827 | Jan 2004 | WO |
| 2004010467 | Jan 2004 | WO |
| 2004106584 | Dec 2004 | WO |
| 2005112082 | Nov 2005 | WO |
| 2006054854 | May 2006 | WO |
| 2006056091 | Jun 2006 | WO |
| 2006078666 | Jul 2006 | WO |
| 2006080782 | Aug 2006 | WO |
| 2006101857 | Sep 2006 | WO |
| 2006114781 | Nov 2006 | WO |
| 2007024720 | Mar 2007 | WO |
| 2007027165 | Mar 2007 | WO |
| 2007117718 | Oct 2007 | WO |
| 2007140376 | Dec 2007 | WO |
| 2008045972 | Apr 2008 | WO |
| 2008091900 | Jul 2008 | WO |
| 2008121463 | Oct 2008 | WO |
| 2008147731 | Dec 2008 | WO |
| 2009028619 | Mar 2009 | WO |
| 2009029532 | Mar 2009 | WO |
| 2009039251 | Mar 2009 | WO |
| 2009099776 | Aug 2009 | WO |
| 2009154889 | Dec 2009 | WO |
| 2009154896 | Dec 2009 | WO |
| 2010039363 | Apr 2010 | WO |
| 2010077533 | Jul 2010 | WO |
| 2010100702 | Sep 2010 | WO |
| 2010118051 | Oct 2010 | WO |
| 2010129428 | Nov 2010 | WO |
| 2010129430 | Nov 2010 | WO |
| 2010129431 | Nov 2010 | WO |
| 2010118051 | Jan 2011 | WO |
| 2011019950 | Feb 2011 | WO |
| 2011149640 | Dec 2011 | WO |
| 2012077590 | Jun 2012 | WO |
| 2013078065 | May 2013 | WO |
| 2013078066 | May 2013 | WO |
| 2014107290 | Jul 2014 | WO |
| 2015026230 | Feb 2015 | WO |
| 2015107009 | Jul 2015 | WO |
| 2018109553 | Jun 2016 | WO |
| 2018109554 | Jun 2016 | WO |
| 2017108713 | Jun 2017 | WO |
| 2017108714 | Jun 2017 | WO |
| 2017212546 | Dec 2017 | WO |
| 2018003072 | Jan 2018 | WO |
| 2018008088 | Jan 2018 | WO |
| 2018020316 | Feb 2018 | WO |
| 2018020318 | Feb 2018 | WO |
| 2018020320 | Feb 2018 | WO |
| 2018020327 | Feb 2018 | WO |
| 2008045972 | Apr 2018 | WO |
| 20181095 | Jun 2018 | WO |
| 2018109552 | Jun 2018 | WO |
| Entry |
|---|
| Kannan Selvaraj, Sathees et al. Selective atomic layer deposition of zirconia on copper patterned silicon substrates using ehtnaol as oxygen source as well as copper reductant. J. Vac. Sci. Technol. A 32(1), Jan./Feb. 2014. |
| S. K. Selvaraj et al. Surface Selective Atomic Layer Deposition of Hafnium Oxide for Copper Diffusion Barrier Application Using Tetrakis(diethylamino)Hafnium and Ethanol. 225th ECS Meeting, May 12, 2014, Meeting Abstract. |
| USPTO; Office Action dated Jan. 10, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Restriction Requirement dated Oct. 29, 2013 in U.S. Appl. No. 13/439,528. |
| USPTO; Final Office Action dated Feb. 11, 2016 U.S. Appl. No. 14/090,750. |
| Jones et al., “Growth of Aluminium Films by Low Pressure Chemical Vapour Deposition Using Tritertiarybutylaluminium,” Journal of Crystal Growth 135, pp. 285-289, Elsevier Science B.V. (1994). |
| Kim et al., “Characteristics of Low Temperaure High Quality Silicon Oxide by Plasma Enhanced Atomic Layer Deposition with In-Situ Plasma Densification Process,” The Electrochemical Society, ECS Transactions, College of Information and Communication Engineerign, Sungkyunkwan University, 53(1), 321-329 (2013). |
| Knoops et al., “Atomic Layer Deposition of Silicon Nitride from Bis(tert-butyloamino) silane and N2 Plama,” Applied Materials & Interfaces, American Chemical Society, A-E (2015). |
| Liu et al., “Research, Design, and Experimen of End Effector for Wafer Transfer Robot,” Industrial Robot: An International Journal, 79-91 (2012). |
| Marsik et al., “Effect of Ultraviolet Curing Wavelength on Low-k Dielectric Material Proerties and Plasma Damage Resistance,” Sciencedirect.com, 519, 11, 3619-3626 (2011). |
| Mason et al., “Hydrolysis of Tri-tert-butylaluminum: The First Structural Characterization of Alkylalumoxanes [(R2A1)2O]n and (RAIO)n,” J. American Chemical Society, vol. 115, No. 12, pp. 4971-4984 (1993). |
| Provine et al., “Correlation of Film Density and Wet Etch Rate in Hydrofluoric Acid of Plama Enhanced Atomic Layer Deposited Silicon Nitride,” AIP Advances, 6 (2016). |
| Sathees et al., “Selective Atomic Layer Deposition of Zirconia on Copper Patterened Silicon Substrates Using Ethanol as Oxygen Source as Well as Copper Reductant,” J. Vac. Sci. Technol. A32(1), (2014). |
| Yun et al., “Behavior of Various Organosilicon Molecules in PECVD Processes for Hydrocathon-Doped Silicon Oxide Films,” Solid State Phenomena, vol. 124-126, 347-350 (2007). |
| USPTO; Notice of Allowance dated Jun. 28, 2017 in U.S. Appl. No. 13/166,367. |
| USPTO; Non-Final Office Action dated Sep. 20, 2018 in U.S. Appl. No. 13/651,144. |
| USPTO; Notice of Allowance dated Aug. 13, 2018 in U.S. Appl. No. 13/941,226. |
| USPTO; Notice of Allowance dated Oct. 3, 2018 in U.S. Appl. No. 13/941,226. |
| USPTO; Notice of Allowance dated Aug. 29, 2018 in U.S. Appl. No. 14/090,750. |
| USPTO; Notice of Allowance dated Sep. 24, 2018 in U.S. Appl. No. 14/218,690. |
| USPTO; Final Office Action dated Sep. 5, 2018 in U.S. Appl. No. 14/752,712. |
| USPTO; Advisory Action dated Aug. 10, 2018 in U.S. Appl. No. 14/829,565. |
| USPTO; Non-Final Office Action dated Sep. 6, 2018 in U.S. Appl. No. 14/829,565. |
| USPTO; Notice of Allowance dated Oct. 20, 2017 in U.S. Appl. No. 14/884,695. |
| USPTO; Notice of Allowance dated Oct. 4, 2018 in U.S. Appl. No. 14/919,536. |
| USPTO; Non-Final Office Action dated Aug. 27, 2018 in U.S. Appl. No. 15/067,028. |
| USPTO; Notice of Allowance dated Oct. 14, 2018 in U.S. Appl. No. 15/135,333. |
| USPTO; Notice of Allowance dated May 22, 2017 in U.S. Appl. No. 15/222,738. |
| USPTO; Notice of Allowance dated Sep. 10, 2018 in U.S. Appl. No. 15/222,749. |
| USPTO; Non-Final Office Action dated Oct. 1, 2018 in U.S. Appl. No. 15/222,780. |
| USPTO; Non-Final Office Action dated Sep. 13, 2018 in U.S. Appl. No. 15/262,990. |
| USPTO; Non-Final Office Action dated Oct. 3, 2017 in U.S. Appl. No. 15/388,410. |
| USPTO; Non-Final Office Action dated Sep. 20, 2018 in U.S. Appl. No. 15/410,503. |
| USPTO; Final Office Action dated Aug. 29, 2018 in U.S. Appl. No. 15/434,051. |
| USPTO; Non-Final Office Action dated Sep. 10, 2018 in U.S. Appl. No. 15/489,453. |
| USPTO; Notice of Allowance dated Jul. 18, 2018 in U.S. Appl. No. 15/640,239. |
| USPTO; Notice of Allowance dated Aug. 30, 2018 in U.S. Appl. No. 15/640,239. |
| USPTO; Non-Final Office Action dated Sep. 21, 2017 in U.S. Appl. No. 15/659,631. |
| USPTO; Non-Final Office Action dated Aug. 27, 2018 in U.S. Appl. No. 15/662,107. |
| USPTO; Requirement for Restriction dated Sep. 11, 2018 in U.S. Appl. No. 15/672,063. |
| USPTO; Requirement for Restriction dated Aug. 14, 2018 in U.S. Appl. No. 15/705,955. |
| USPTO; Non-Final Office Action dated Oct. 4, 2018 in U.S. Appl. No. 15/726,222. |
| USPTO; Restriction Requirement dated Aug. 31, 2018 in U.S. Appl. No. 15/795,056. |
| USPTO; Non-Final Office Action dated Jun. 26, 2018 in U.S. Appl. No. 15/796,693. |
| USPTO; Non-Final Office Action dated Sep. 10, 2018 in U.S. Appl. No. 15/836,547. |
| European Patent Office; Office Action dated Aug. 10, 2018 in Application No. 09767208.3. |
| Korean Patent Office; Office Action dated Apr. 2, 2018 in Application No. 10-2011-0036449. |
| Korean Patent Office; Office Action dated Sep. 18, 2018 in Application No. 10-2012-0064526. |
| Korean Patent Office; Office Action dated Sep. 27, 2018 in Application No. 10-2012-0076564. |
| Korean Patent Office; Office Action dated Sep. 28, 2017 in Application No. 10-2017-7023740. |
| Taiwanese Patent Office; Office Action dated Sep. 26, 2018 in Application No. 103132230. |
| Taiwanese Patent Office; Office Action dated May 21, 2018 Application No. 103139014. |
| Taiwanese Patent Office; Office Action dated Jul. 9, 2018 in Application No. 104107876. |
| Taiwanese Patent Office; Office Action dates Aug. 7, 2018 Application No. 104107888. |
| Taiwanese Patent Office; Office Action dated Jul. 9, 2018 in Application No. 104110326. |
| Taiwanese Patent Office; Office Action dated Jul. 11, 2018 in Application No. 104124377. |
| Taiwanese Patent Office; Office Action dated Jun. 25, 2018 in Application No. 106138800. |
| Taiwanese Patent Office; Office Action dated Aug. 31, 2018 in Application No. 10720809210. |
| WIPO; International Search Report and Written Opinion dated Jul. 9, 2018 in Application No. PCT/IB2018/000419. |
| WIPO; International Search Report and Written Opinion dated Sep. 14, 2018 in Application No. PCT/IB2017/001640. |
| Crystal IS “Application Note: Using UV Reflective Materials to Maximize Disinfection”; AN011; Jun. 16, 2016. |
| Kukli et al., “Properties of hafnium oxide films grown by atomic layer deposition from hafnium tetraiodide and oxygen”. Journal of Applied Physics, vol. 92, No. 10, Nov. 15, 2002, pp. 5698-5703. |
| Liang et al. “Conversion of Metal Carbides to Carbide Derived Carbon by Reactive Ion Etching in Halogen Gas” Micro (MEMS) and Nanotechnologies for Space Applications, Thomas George et al. vol. 6223, 2006 p. 62230J-I to 62230J-11 lines 3-14 in the “Abstract” section and lines 7-9 in the “Introduction” section of p. 1, lines 3-4 in the “Introduction” section and lines 3-4 in the “Experimental Procedure” section of p. 2. |
| Sellers, Making Your Own Timber Dogs, Paul Sellers blog, Published on Nov. 18, 2014, [online], [site visited Jun. 10, 2017]. Available from Internet, <URL: https://paulsellers.com/2014/11/making-your-own-timber-dogs/>. |
| “Polyurethane HF”; webpage; no date. Cited in Notice of References dated May 18, 2017 in U.S. Appl. No. 14/884,695. |
| Xu et al., “14NM Metal Gate Film Stack Development and Challenges,” SMIC et al. (2016). |
| USPTO; Notice of Allowance dated Jul. 26, 2005 in U.S. Appl. No. 10/033,058. |
| USPTO; Non-Final Office Action dated Aug. 25, 2005 in U.S. Appl. No. 10/191,635. |
| USPTO; Final Office Action dated Apr. 25, 2006 in U.S. Appl. No. 10/191,635. |
| USPTO; Non-Final Office Action dated Nov. 20, 2006 in U.S. Appl. No. 10/191,635. |
| USPTO; Notice of Allowance dated May 21, 2007 in U.S. Appl. No. 10/191,635. |
| USPTO; Notice of Allowance dated Feb. 20, 2008 in U.S. Appl. No. 10/191,635. |
| USPTO; Non-Final Office Action dated May 13, 2003 in U.S. Appl. No. 10/222,229. |
| USPTO; Non-Final Office Action dated Oct. 22, 2003 in U.S. Appl. No. 10/222,229. |
| USPTO; Final Office Action dated Mar. 22, 2004 in U.S. Appl. No. 10/222,229. |
| USPTO; Advisory Action dated Oct. 7, 2004 in U.S. Appl. No. 10/222,229. |
| USPTO; Non-Final Office Action dated Dec. 22, 2004 in U.S. Appl. No. 10/222,229. |
| USPTO; Final Office Action dated Jun. 20, 2005 in U.S. Appl. No. 10/222,229. |
| USPTO; Advisory Action dated Nov. 16, 2005 in U.S. Appl. No. 10/222,229. |
| USPTO; Notice of Allowance dated Mar. 8, 2006 in U.S. Appl. No. 10/222,229. |
| USPTO; Non-Final Office Action dated Jan. 26, 2005 in U.S. Appl. No. 10/838,510. |
| USPTO; Notice of Allowance dated Jul. 12, 2005 in U.S. Appl. No. 10/838,510. |
| USPTO; Office Action dated Aug. 27, 2010 in U.S. Appl. No. 12/118,596. |
| USPTO; Office Action dated Feb. 15, 2011 in U.S. Appl. No. 12/118,596. |
| USPTO; Notice of Allowance dated Aug. 4, 2011 in U.S. Appl. No. 12/118,596. |
| USPTO; Non-Final Office Action dated Mar. 28, 2010 in U.S. Appl. No. 12/121,085. |
| USPTO; Notice of Allowance dated Jul. 26, 2010 in U.S. Appl. No. 12/121,085. |
| USPTO; Notice of Allowance dated Oct. 4, 2010 in U.S. Appl. No. 12/121,085. |
| USPTO; Non-Final Office Action dated Sep. 13, 2010 in U.S. Appl. No. 12/140,809. |
| USPTO; Final Office Action dated Dec. 28, 2010 in U.S. Appl. No. 12/140,809. |
| USPTO; Notice of Allowance dated Mar. 17, 2011 in U.S. Appl. No. 12/140,809. |
| USPTO; Non-Final Office Action dated Mar. 15, 2011 in U.S. Appl. No. 12/193,924. |
| USPTO; Foma; Office Action dated Sep. 30, 2011 in U.S. Appl. No. 12/193,924. |
| USPTO; Non-Final Office Action dated Oct. 24, 2012 in U.S. Appl. No. 12/193,924. |
| USPTO; Final Office Action dated Apr. 17, 2013 in U.S. Appl. No. 12/193,924. |
| USPTO; Advisory Action dated Jul. 9, 2013 in U.S. Appl. No. 12/193,924. |
| USPTO; Non-Final Office Action dated Jul. 28, 2011 in U.S. Appl. No. 12/330,096. |
| USPTO; Final Office Action dated Jan. 13, 2012 in U.S. Appl. No. 12/330,096. |
| USPTO; Notice of Allowance dated Mar. 6, 2012 in U.S. Appl. No. 12/330,096. |
| USPTO; Non-Final Office Action dated Mar. 20, 2012 in U.S. Appl. No. 12/330,096. |
| USPTO; Notice of Allowance dated Jun. 7, 2012 in U.S. Appl. No. 12/330,096. |
| USPTO; Non-Final Office Action dated Apr. 1, 2010 in U.S. Appl. No. 12/357,174. |
| USPTO; Final Office Action dated Sep. 1, 2010 in U.S. Appl. No. 12/357,174. |
| USPTO; Notice of Allowance dated Dec. 13, 2010 in U.S. Appl. No. 12/357,174. |
| USPTO; Non-Final Office Action dated Dec. 29, 2010 in U.S. Appl. No. 12/362,023. |
| USPTO; Non-Final Office Action dated Jul. 26, 2011 in U.S. Appl. No. 12/416,809. |
| USPTO; Final Office Action dated Dec. 6, 2011 in U.S. Appl. No. 12/416,809. |
| USPTO; Notice of Allowance dated Apr. 2, 2012 in U.S. Appl. No. 12/416,809. |
| USPTO; Advisory Action dated Feb. 3, 2012 in U.S. Appl. No. 12/416,809. |
| USPTO; Notice of Allowance dated Jun. 16, 2011 in U.S. Appl. No. 12/430,751. |
| USPTO; Notice of Allowance dated Jul. 27, 2011 in U.S. Appl. No. 12/430,751. |
| USPTO; Non-Final Office Action dated Aug. 3, 2011 in U.S. Appl. No. 12/436,300. |
| USPTO; Final Office Action dated Jan. 23, 2012 in U.S. Appl. No. 12/436,300. |
| USPTO; Advisory Action dated Mar. 6, 2012 in U.S. Appl. No. 12/436,300. |
| USPTO; Non-Final Office Action dated May 22, 2012 in U.S. Appl. No. 12/436,300. |
| USPTO; Notice of Allowance dated Nov. 28, 2012 in U.S. Appl. No. 12/436,300. |
| USPTO; Restriction Requirement dated Dec. 20, 2011 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated Apr. 11, 2012 in U.S. Appl. No. 12/436,306. |
| USPTO; Final Office Action dated Sep. 26, 2012 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated May 31, 2013 in U.S. Appl. No. 12/436,306. |
| USPTO; Final Office Action dated Oct. 17, 2013 in U.S. Appl. No. 12/436,306. |
| USPTO; Advisory Action dated Oct. 1, 2014 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated Feb. 4, 2014 in U.S. Appl. No. 12/436,306. |
| USPTO; Final Office Action dated Jun. 23, 2014 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated Feb. 3, 2015 in U.S. Appl. No. 12/436,306. |
| USPTO; Final Office Action dated May 13, 2015 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated Oct. 14, 2015 in U.S. Appl. No. 12/436,306. |
| USPTO; Final Office Action dated Dec. 31, 2015 in U.S. Appl. No. 12/436,306. |
| USPTO; Notice of Allowance dated Feb. 3, 2016 in U.S. Appl. No. 12/436,306. |
| USPTO; Non-Final Office Action dated Aug. 3, 2011 in U.S. Appl. No. 12/436,315. |
| USPTO; Notice of Allowance dated Nov. 17, 2011 in U.S. Appl. No. 12/436,315. |
| USPTO; Notice of Allowance dated Oct. 1, 2010 in U.S. Appl. No. 12/467,017. |
| USPTO; Non-Final Office Action dated Mar. 18, 2010 in U.S. Appl. No. 12/489,252. |
| USPTO; Notice of Allowance dated Sep. 2, 2010 in U.S. Appl. No. 12/489,252. |
| USPTO; Non-Final Office Action dated Dec. 15, 2010 in U.S. Appl. No. 12/553,759. |
| USPTO; Final Office Action dated May 4, 2011 in U.S. Appl. No. 12/553,759. |
| USPTO; Advisory Action dated Jul. 13, 2011 in U.S. Appl. No. 12/553,759. |
| USPTO; Non-Final Office Action dated Sep. 6, 2011 in U.S. Appl. No. 12/553,759. |
| USPTO; Notice of Allowance dated Jan. 24, 2012 in U.S. Appl. No. 12/553,759. |
| USPTO; Non-Final Office Action dated Oct. 19, 2012 in U.S. Appl. No. 12/618,355. |
| USPTO; Final Office Action dated May 8, 2013 in U.S. Appl. No. 12/618,355. |
| USPTO; Advisory Action dated Jul. 23, 2013 in U.S. Appl. No. 12/618,355. |
| USPTO; Non-Final Office Action dated Apr. 8, 2015 in U.S. Appl. No. 12/618,355. |
| USPTO; Final Office Action dated Oct. 22, 2015 in U.S. Appl. No. 12/618,355. |
| USPTO; Advisory Action dated Mar. 4, 2016 in U.S. Appl. No. 12/618,355. |
| USPTO; Non-Final Office Action dated Jun. 30, 2016 in U.S. Appl. No. 12/618,355. |
| USPTO; Final Office Action dated Feb. 10, 2017 in U.S. Appl. No. 12/618,355. |
| USPTO; Advisory Action dated May 16, 2017 in U.S. Appl. No. 12/618,355. |
| USPTO; Non-Final Office Action dated Nov. 29, 2017 in U.S. Appl. No. 12/618,355. |
| USPTO; Final Office Action dated Aug. 10, 2018 in U.S. Appl. No. 12/618,355. |
| USPTO; Non-Final Office Action dated Feb. 16, 2012 in U.S. Appl. No. 12/618,419. |
| USPTO; Final Office Action dated Jun. 22, 2012 in U.S. Appl. No. 12/618,419. |
| USPTO; Non-Final Office Action dated Nov. 27, 2012 in U.S. Appl. No. 12/618,419. |
| USPTO; Advisory Action dated Aug. 9, 2012 in U.S. Appl. No. 12/618,419. |
| USPTO; Notice of Allowance dated Apr. 12, 2013 in U.S. Appl. No. 12/618,419. |
| USPTO; Notice of Allowance dated Oct. 9, 2013 in U.S. Appl. No. 12/618,419. |
| USPTO; Requirement for Restriction dated Sep. 12, 2011 in U.S. Appl. No. 12/718,731. |
| USPTO; Non-Final Office Action dated Dec. 6, 2011 in U.S. Appl. No. 12/718,731. |
| USPTO; Notice of Allowance dated Mar. 16, 2012 in U.S. Appl. No. 12/718,731. |
| USPTO; Restriction Requirement dated Jan. 15, 2013 in U.S. Appl. No. 12/754,223. |
| USPTO; Office Action dated Feb. 26, 2013 in U.S. Appl. No. 12/754,223. |
| USPTO; Final Office Action dated Jun. 28, 2013 in U.S. Appl. No. 12/754,223. |
| USPTO; Office Action dated Feb. 25, 2014 in U.S. Appl. No. 12/754,223. |
| USPTO; Final Office Action dated Jul. 14, 2014 in U.S. Appl. No. 12/754,223. |
| USPTO; Non-Final Office Action dated Mar. 25, 2015 in U.S. Appl. No. 12/754,223. |
| USPTO; Final Office Action dated Aug. 12, 2015 in U.S. Appl. No. 12/754,223. |
| USPTO; Notice of Allowance dated May 23, 2016 in U.S. Appl. No. 12/754,223. |
| USPTO; Office Action dated Apr. 23, 2013 in U.S. Appl. No. 12/763,037. |
| USPTO; Final Office Action dated Oct. 21, 2013 in U.S. Appl. No. 12/763,037. |
| USPTO; Office Action dated Oct. 8, 2014 in U.S. Appl. No. 12/763,037. |
| USPTO; Notice of Allowance dated Jan. 27, 2015 in U.S. Appl. No. 12/763,037. |
| USPTO; Non-Final Office Action dated Jan. 24, 2011 in U.S. Appl. No. 12/778,808. |
| USPTO; Notice of Allowance dated May 9, 2011 in U.S. Appl. No. 12/778,808. |
| USPTO; Notice of Allowance dated Oct. 12, 2012 in U.S. Appl. No. 12/832,739. |
| USPTO; Non-Final Office Action dated Oct. 16, 2012 in U.S. Appl. No. 12/847,848. |
| USPTO; Final Office Action dated Apr. 22, 2013 in U.S. Appl. No. 12/847,848. |
| USPTO; Advisory Action dated Jul. 1, 2013 in U.S. Appl. No. 12/847,848. |
| USPTO; Notice of Allowance dated Jan. 16, 2014 in U.S. Appl. No. 12/847,848. |
| USPTO; Restriction Requirement dated Sep. 25, 2012 in U.S. Appl. No. 12/854,818. |
| USPTO; Office Action dated Dec. 6, 2012 in U.S. Appl. No. 12/854,818. |
| USPTO; Final Office Action dated Mar. 13, 2013 in U.S. Appl. No. 12/854,818. |
| USPTO; Office Action dated Aug. 30, 2013 in U.S. Appl. No. 12/854,818. |
| USPTO; Final Office Action dated Mar. 26, 2014 in U.S. Appl. No. 12/854,818. |
| USPTO; Office Action dated Jun. 3, 2014 in U.S. Appl. No. 12/854,818. |
| USPTO; Non-Final Office Action dated Jul. 11, 2012 in U.S. Appl. No. 12/875,889. |
| USPTO; Notice of Allowance dated Jan. 4, 2013 in U.S. Appl. No. 12/875,889. |
| USPTO; Notice of Allowance dated Jan. 9, 2012 in U.S. Appl. No. 12/901,323. |
| USPTO; Requirement for Restriction dated Jul. 22, 2013 in U.S. Appl. No. 12/910,607. |
| USPTO; Non-Final Office Action dated Nov. 20, 2013 in U.S. Appl. No. 12/910,607. |
| USPTO; Final Office Action dated Apr. 28, 2014 in U.S. Appl. No. 12/910,607. |
| USPTO; Advisory Action dated Jul. 9, 2014 in U.S. Appl. No. 12/910,607. |
| USPTO; Notice of Allowance dated Aug. 15, 2014 in U.S. Appl. No. 12/910,607. |
| USPTO; Non-Final Office Action dated Oct. 24, 2012 in U.S. Appl. No. 12/940,906. |
| USPTO; Final Office Action dated Feb. 13, 2013 in U.S. Appl. No. 12/940,906. |
| USPTO; Notice of Allowance dated Apr. 23, 2013 in U.S. Appl. No. 12/940,906. |
| USPTO; Non-Final Office Action dated Dec. 7, 2012 in U.S. Appl. No. 12/953,870. |
| USPTO; Final Office Action dated Apr. 22, 2013 in U.S. Appl. No. 12/953,870. |
| USPTO; Advisory Action dated Jul. 8, 2013 in U.S. Appl. No. 12/953,870. |
| USPTO; Non-Final Office Action dated Aug. 28, 2013 in U.S. Appl. No. 12/953,870. |
| USPTO; Final Office Action dated Apr. 17, 2014 in U.S. Appl. No. 12/953,870. |
| USPTO; Requirement for Restriction dated Sep. 10, 2010 in U.S. Appl. No. 12/148,956. |
| USPTO; Non-Final Office Action dated Sep. 19, 2012 in U.S. Appl. No. 13/016,735. |
| USPTO; Final Office Action dated Feb. 11, 2013 in U.S. Appl. No. 13/016,735. |
| USPTO; Notice of Allowance dated Apr. 24, 2013 in U.S. Appl. No. 13/016,735. |
| USPTO; Non-Final Office Action dated Apr. 4, 2012 in U.S. Appl. No. 13/030,438. |
| USPTO; Final Office Action dated Aug. 22, 2012 in U.S. Appl. No. 13/030,438. |
| USPTO; Notice of Allowance dated Oct. 24, 2012 in U.S. Appl. No. 13/030,438. |
| USPTO; Non-Final Office Action dated Dec. 3, 2012 in U.S. Appl. No. 13/040,013. |
| USPTO; Notice of Allowance dated May 3, 2013 in U.S. Appl. No. 13/040,013. |
| USPTO; Notice of Allowance dated Sep. 13, 2012 in U.S. Appl. No. 13/085,698. |
| USPTO; Non-Final Office Action dated Mar. 29, 2013 in U.S. Appl. No. 13/094,402. |
| USPTO; Final Office Action dated Jul. 17, 2013 in U.S. Appl. No. 13/094,402. |
| USPTO; Notice of Allowance dated Sep. 30, 2013 in U.S. Appl. No. 13/094,402. |
| USPTO; Restriction Requirement dated May 8, 2013 in U.S. Appl. No. 13/102,980. |
| USPTO; Office Action dated Oct. 7, 2013 in U.S. Appl. No. 13/102,980. |
| USPTO; Final Office Action dated Mar. 25, 2014 in U.S. Appl. No. 13/102,980. |
| USPTO; Advisory Action dated Jun. 12, 2014 in U.S. Appl. No. 13/102,980. |
| USPTO; Notice of Allowance dated Jul. 3, 2014 in U.S. Appl. No. 13/102,980. |
| USPTO; Notice of Allowance dated Sep. 17, 2014 in U.S. Appl. No. 13/102,980. |
| USPTO; Requirement for Restriction dated Jun. 5, 2014 in U.S. Appl. No. 13/154,271. |
| USPTO; Non-Final Office Action dated Jul. 17, 2014 in U.S. Appl. No. 13/154,271. |
| USPTO; Final Office Action dated Jan. 2, 2015 in U.S. Appl. No. 13/154,271. |
| USPTO; Non-Final Office Action dated May 27, 2015 in U.S. Appl. No. 13/154,271. |
| USPTO; Final Office Action dated Nov. 23, 2015 in U.S. Appl. No. 13/154,271. |
| USPTO; Notice of Allowance dated Feb. 10, 2016 in U.S. Appl. No. 13/154,271. |
| USPTO; Requirement for Restriction dated Apr. 6, 2016 in U.S. Appl. No. 13/166,367. |
| USPTO; Non-Final Office Action dated Jun. 27, 2016 in U.S. Appl. No. 13/166,367. |
| USPTO; Final Office Action dated Dec. 30, 2016 in U.S. Appl. No. 13/166,367. |
| USPTO; Advisory Action dated Apr. 21, 2017 in U.S. Appl. No. 13/166,367. |
| USPTO; Requirement for Restriction dated Jun. 18, 2014 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Oct. 27, 2014 in U.S. Appl. No. 13/169,951. |
| USPTO; Final Office Action dated May 26, 2015 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Sep. 1, 2015 in U.S. Appl. No. 13/169,951. |
| USPTO; Final Office Action dated Mar. 3, 2016 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Jun. 9, 2016 in U.S. Appl. No. 13/169,951. |
| USPTO; Final Office Action dated Dec. 9, 2016 in U.S. Appl. No. 13/169,951. |
| USPTO; Advisory Action dated May 13, 2016 in U.S. Appl. No. 13/169,951. |
| USPTO; Advisory Action dated Feb. 15, 2017 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Apr. 26, 2017 in U.S. Appl. No. 13/169,951. |
| USPTO; Final Office Action dated Nov. 2, 2017 in U.S. Appl. No. 13/169,951. |
| USPTO; Advisory Action dated Feb. 8, 2018 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Apr. 6, 2018 in U.S. Appl. No. 13/169,951. |
| USPTO; Non-Final Office Action dated Jun. 24, 2014 in U.S. Appl. No. 13/181,407. |
| USPTO; Final Office Action dated Sep. 24, 2014 in U.S. Appl. No. 13/181,407. |
| USPTO; Advisory Action dated Dec. 17, 2014 in U.S. Appl. No. 13/181,407. |
| USPTO; Non-Final Office Action dated Jan. 2, 2015 in U.S. Appl. No. 13/181,407. |
| USPTO; Final Office Action dated Apr. 8, 2015 in U.S. Appl. No. 13/181,407. |
| USPTO; Requirement for Restriction dated Sep. 25, 2012 in U.S. Appl. No. 13/184,351. |
| USPTO; Non-Final Office Action dated Jan. 23, 2013 in U.S. Appl. No. 13/184,351. |
| USPTO; Final Office Action dated Jul. 29, 2013 in U.S. Appl. No. 13/184,351. |
| USPTO; Advisory Action dated Nov. 7, 2013 in U.S. Appl. No. 13/184,351. |
| USPTO; Non-Final Office Action dated Jul. 16, 2014 in U.S. Appl. No. 13/184,351. |
| USPTO; Final Office Action dated Feb. 17, 2015 in U.S. Appl. No. 13/184,351. |
| USPTO; Advisory Action dated May 18, 2015 in U.S. Appl. No. 13/184,351. |
| USPTO; Non-Final Office Action dated Aug. 10, 2015 in U.S. Appl. No. 13/184,351. |
| USPTO; Final Office Action dated Feb. 12, 2016 in U.S. Appl. No. 13/184,351. |
| USPTO; Non-Final Office Action dated Dec. 15, 2016 in U.S. Appl. No. 13/184,351. |
| USPTO; Final Office Action dated Jun. 15, 2017 in U.S. Appl. No. 13/184,351. |
| USPTO; Advisory Action dated Oct. 4, 2017 in U.S. Appl. No. 13/184,351. |
| USPTO; Non-Final Office Action dated Jul. 26, 2018 in U.S. Appl. No. 13/184,351. |
| USPTO; Restriction Requirement dated Aug. 21, 2014 in U.S. Appl. No. 13/187,300. |
| USPTO; Non-Final Office Action dated Sep. 17, 2014 in U.S. Appl. No. 13/187,300. |
| USPTO; Final Office Action dated Apr. 15, 2015 in U.S. Appl. No. 13/187,300. |
| USPTO; Non-Final Office Action dated Apr. 7, 2016 in U.S. Appl. No. 13/187,300. |
| USPTO; Final Office Acton dated Sep. 23, 2016 in U.S. Appl. No. 13/187,300. |
| USPTO; Non-Final Office Action dated Jan. 30, 2017 in U.S. Appl. No. 13/187,300. |
| USPTO; Final Office Action dated Aug. 9, 2017 in U.S. Appl. No. 13/187,300. |
| USPTO; Non-Final Office Action dated Oct. 1, 2012 in U.S. Appl. No. 13/191,762. |
| USPTO; Final Office Action dated Apr. 10, 2013 in U.S. Appl. No. 13/191,762. |
| USPTO; Notice of Allowance dated Aug. 15, 2013 in U.S. Appl. No. 13/191,762. |
| USPTO; Non-Final Office Action dated Oct. 22, 2012 in U.S. Appl. No. 13/238,960. |
| USPTO; Final Office Action dated May 3, 2013 in U.S. Appl. No. 13/238,960. |
| USPTO; Non-Final Office Action dated Apr. 26, 2013 in U.S. Appl. No. 13/250,721. |
| USPTO; Notice of Allowance dated Sep. 11, 2013 in U.S. Appl. No. 13/250,721. |
| USPTO; Non-Final Office Action dated Jul. 2, 2014 in U.S. Appl. No. 13/283,408. |
| USPTO; Final Office Action dated Jan. 29, 2015 in U.S. Appl. No. 13/283,408. |
| USPTO; Non-Final Office Action dated Jun. 17, 2015 in U.S. Appl. No. 13/283,408. |
| USPTO; Final Office Action dated Dec. 18, 2015 in U.S. Appl. No. 13/283,408. |
| USPTO; Advisory Action dated Mar. 28, 2016 in U.S. Appl. No. 13/283,408. |
| USPTO; Notice of Allowance dated Mar. 28, 2016 in U.S. Appl. No. 13/283,408. |
| USPTO; Restriction Requirement dated Dec. 16, 2013 in U.S. Appl. No. 13/284,642. |
| USPTO; Restriction Requirement dated Apr. 21, 2014 in U.S. Appl. No. 13/284,642. |
| USPTO; Office Action dated Jul. 30, 2014 in U.S. Appl. No. 13/284,642. |
| USPTO; Notice of Allowance dated Feb. 11, 2015 in U.S. Appl. No. 13/284,642. |
| USPTO; Restriction Requirement dated Oct. 2, 2013 in U.S. Appl. No. 13/312,591. |
| USPTO; Office Action dated Jan. 28, 2014 in U.S. Appl. No. 13/312,591. |
| USPTO; Final Office Action dated May 14, 2014 in U.S. Appl. No. 13/312,591. |
| USPTO; Advisory Action dated Aug. 26, 2014 in U.S. Appl. No. 13/312,591. |
| USPTO; Non-Final Office Action dated Nov. 26, 2014 in U.S. Appl. No. 13/312,591. |
| USPTO; Final Office Action dated Mar. 20, 2015 in U.S. Appl. No. 13/312,591. |
| USPTO; Notice of Allowance dated May 14, 2015 in U.S. Appl. No. 13/312,591. |
| USPTO; Notice of Allowance dated Jun. 11, 2015 in U.S. Appl. No. 13/312,591. |
| USPTO; Requirement for Restriction dated Nov. 26, 2013 in U.S. Appl. No. 13/333,420. |
| USPTO; Non-Final Office Action dated Apr. 9, 2014 in U.S. Appl. No. 13/333,420. |
| USPTO; Notice of Allowance dated Sep. 15, 2014 in U.S. Appl. No. 13/333,420. |
| USPTO; Requirement for Restriction dated Jan. 10, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Office Action dated Feb. 11, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Final Office Action dated May 17, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Office Action dated Aug. 29, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Final Office Action dated Dec. 18, 2013 in U.S. Appl. No. 13/339,609. |
| USPTO; Notice of Allowance dated Apr. 7, 2014 in U.S. Appl. No. 13/339,609. |
| USPTO; Non-Final Office Action dated Oct. 10, 2012 in U.S. Appl. No. 13/406,791. |
| USPTO; Final Office Action dated Jan. 31, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Advisory Action dated Mar. 27, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Non-Final Office Action dated Apr. 25, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Final Office Action dated Aug. 23, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Advisory Action dated Oct. 29, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Non-Final Office Action dated Dec. 4, 2013 in U.S. Appl. No. 13/406,791. |
| USPTO; Final Office Action dated Apr. 21, 2014 in U.S. Appl. No. 13/406,791. |
| USPTO; Non-Final Office Action dated Jan. 14, 2013 in U.S. Appl. No. 13/410,970. |
| USPTO; Notice of Allowance dated Feb. 14, 2013 in U.S. Appl. No. 13/410,970. |
| USPTO; Non-Final Office Action dated Feb. 13, 2014 in U.S. Appl. No. 13/411,271. |
| USPTO; Non-Final Office Action dated Jul. 31, 2014 in U.S. Appl. No. 13/411,271. |
| USPTO; Advisory Action dated Apr. 22, 2015 in U.S. Appl. No. 13/411,271. |
| USPTO; Final Office Action dated Jan. 16, 2015 in U.S. Appl. No. 13/411,271. |
| USPTO; Notice of Allowance dated Oct. 6, 2015 in U.S. Appl. No. 13/411,271. |
| USPTO; Office Action dated Feb. 4, 2014 in U.S. Appl. No. 13/439,528. |
| USPTO; Final Office Action dated Jul. 8, 2014 in U.S. Appl. No. 13/439,528. |
| UPPTO; Notice of Allowance dated Oct. 21, 2014 in U.S. Appl. No. 13/439,528. |
| USPTO; Non-Final Office Action dated Apr. 11, 2013 in U.S. Appl. No. 13/450,368. |
| USPTO; Notice of Allowance dated Jul. 17, 2013 in U.S. Appl. No. 13/450,368. |
| USPTO; Office Action dated May 23, 2013 in U.S. Appl. No. 13/465,340. |
| USPTO; Final Office Action dated Oct. 30, 2013 in U.S. Appl. No. 13/465,340. |
| USPTO; Notice of Allowance dated Feb. 12, 2014 in U.S. Appl. No. 13/465,340. |
| USPTO; Non-Final Office Action dated Oct. 17, 2013 in U.S. Appl. No. 13/493,897. |
| USPTO; Notice of Allowance dated Mar. 20, 2014 in U.S. Appl. No. 13/493,897. |
| USPTO; Office Action dated Dec. 20, 2013 in U.S. Appl. No. 13/535,214. |
| USPTO; Final Office Action dated Jun. 18, 2014 in U.S. Appl. No. 13/535,214. |
| USPTO; Notice of Allowance dated Oct. 23, 2014 in U.S. Appl. No. 13/535,214. |
| USPTO; Non-Final Office Action dated Sep. 11, 2013 in U.S. Appl. No. 13/550,419. |
| USPTO; Final Office Action dated Jan. 27, 2014 in U.S. Appl. No. 13/550,419. |
| USPTO; Advisory Action dated Mar. 31, 2014 in U.S. Appl. No. 13/550,419. |
| USPTO; Notice of Allowance dated May 29, 2014 in U.S. Appl. No. 13/550,419. |
| USPTO; Non-Final Office Action dated Aug. 8, 2014 in U.S. Appl. No. 13/563,066. |
| USPTO; Final Office Action dated Feb. 12, 2015 in U.S. Appl. No. 13/563,066. |
| USPTO; Advisory Action dated Apr. 16, 2015 in U.S. Appl. No. 13/563,066. |
| USPTO; Notice of Allowance dated Jun. 12, 2015 in U.S. Appl. No. 13/563,066. |
| USPTO; Notice of Allowance dated Jul. 16, 2015 in U.S. Appl. No. 13/563,066. |
| USPTO; Non-Final Office Action dated May 28, 2013in U.S. Appl. No. 13/563,274. |
| USPTO; Notice of Allowance dated Sep. 27, 2013 in U.S. Appl. No. 13/563,274. |
| USPTO; Non-Final Office Action dated Nov. 7, 2013 in U.S. Appl. No. 13/565,564. |
| USPTO; Final Office Action dated Feb. 28, 2014 in U.S. Appl. No. 13/565,564. |
| USPTO; Advisory Action dated May 5, 2014 in U.S. Appl. No. 13/565,564. |
| USPTO; Non-Final Office Action dated Jul. 2, 2014 in U.S. Appl. No. 13/565,564. |
| USPTO; Notice of Allowance dated Nov. 3, 2014 in U.S. Appl. No. 13/565,564. |
| USPTO; Notice of Allowance dated Sep. 13, 2013 in U.S. Appl. No. 13/566,069. |
| USPTO; Non-Final Office Action dated Aug. 30, 2013 in U.S. Appl. No. 13/570,067. |
| USPTO; Notice of Allowance dated Jan. 6, 2014 in U.S. Appl. No. 13/570,067. |
| USPTO; Non-Final Office Action dated Oct. 15, 2014 in U.S. Appl. No. 13/597,043. |
| USPTO; Final Office Action dated Mar. 13, 2015 in U.S. Appl. No. 13/597,043. |
| USPTO;; Notice of Allowance dated Aug. 28, 2015 in U.S. Appl. No. 13/597,043. |
| USPTO; Non-Final Office Action dated Feb. 12, 2015 in U.S. Appl. No. 13/597,108. |
| USPTO; Final Office Action dated Jun. 1, 2015 in U.S. Appl. No. 13/597,108. |
| USPTO; Advisory Action dated Sep. 2, 2015 in U.S. Appl. No. 13/597,108. |
| USPTO; Non-Final Office Action dated Dec. 8, 2015 in U.S. Appl. No. 13/597,108. |
| USPTO; Final Office Action dated Jun. 2, 2016 in U.S. Appl. No. 13/597,108. |
| USPTO; Non-Final Office Action dated Sep. 15, 2016 in U.S. Appl. No. 13/597,108. |
| USPTO; Notice of Allowance dated Mar. 7, 2017 in U.S. Appl. No. 13/597,108. |
| USPTO; Notice of Allowance dated Mar. 27, 2014 in U.S. Appl. No. 13/604,498. |
| USPTO; Restriction Requirement dated Jul. 9, 2013 in U.S. Appl. No. 13/612,538. |
| USPTO; Office Action dated Nov. 15, 2013 in U.S. Appl. No. 13/612,538. |
| USPTO; Office Action dated Jul. 10, 2014 in U.S. Appl. No. 13/612,538. |
| USPTO; Notice of Allowance dated Feb. 25, 2015 in U.S. Appl. No. 13/612,538. |
| USPTO; Requirement for Restriction dated Feb. 4, 2015 in U.S. Appl. No. 13/646,403. |
| USPTO; Non-Final Office Action dated Apr. 15, 2015 in U.S. Appl. No. 13/646,403. |
| USPTO; Final Office Action dated Oct. 15, 2015 in U.S. Appl. No. 13/646,403. |
| USPTO; Notice of Allowance dated Feb. 2, 2016 in U.S. Appl. No. 13/646,403. |
| USPTO; Requirement for Restriction dated Apr. 11, 2014 in U.S. Appl. No. 13/646,471. |
| USPTO; Non-Final Office Action dated May 15, 2014 in U.S. Appl. No. 13/646,471. |
| USPTO; Final Office Action dated Aug. 18, 2014 in U.S. Appl. No. 13/646,471. |
| USPTO; Advisory Action dated Nov. 14, 2014 in U.S. Appl. No. 13/646,471. |
| USPTO; Non-Final Office Action dated Dec. 16, 2014 in U.S. Appl. No. 13/646,471. |
| USPTO; Final Office Action dated Apr. 21, 2015 in U.S. Appl. No. 13/646,471. |
| USPTO; Non-Final Office Action dated Aug. 19, 2015 in U.S. Appl. No. 13/646,471. |
| USPTO; Final Office Action dated Jan. 22, 2016 in U.S. Appl. No. 13/646,471. |
| USPTO; Advisory Action dated Apr. 15, 2016 in U.S. Appl. No. 13/646,471. |
| USPTO; Non-Final Office Action dated Jun. 2, 2016 in U.S. Appl. No. 13/646,471. |
| USPTO; Final Office Action dated Oct. 20, 2016 in U.S. Appl. No. 13/646,471. |
| USPTO; Restriction Requirement dated Mar. 4, 2015 in U.S. Appl. No. 13/651,144. |
| USPTO; Non-Final Office Action dated May 28, 2015 in U.S. Appl. No. 13/651,144. |
| USPTO; Final Office Action dated Dec. 14, 2017 in U.S. Appl. No. 13/651,144. |
| USPTO; Final Office Action dated Nov. 19, 2015 in U.S. Appl. No. 13/651,144. |
| USPTO; Non-Final Office Action dated May 10, 2016 in U.S. Appl. No. 13/651,144. |
| USPTO; Final Office Action dated Sep. 20, 2016 in U.S. Appl. No. 13/651,144. |
| USPTO; Non-Final Office Action dated May 17, 2017 in U.S. Appl. No. 13/651,144. |
| USPTO; Non-Final Office Action dated Dec. 14, 2017 in U.S. Appl. No. 13/651,144. |
| USPTO; Advisory Action dated Apr. 19, 2018 in U.S. Appl. No. 13/651,144. |
| USPTO; Non-Final Office Action dated Nov. 19, 2015 in U.S. Appl. No. 14/659,437. |
| USPTO; Final Office Action dated Mar. 17, 2016 in U.S. Appl. No. 14/659,437. |
| USPTO; Notice of Allowance dated May 31, 2016 in U.S. Appl. No. 14/659,437. |
| USPTO; Requirement for Restriction dated Dec. 24, 2014 in U.S. Appl. No. 13/665,366. |
| USPTO; Non-Final Office Action dated Jun. 18, 2015 in U.S. Appl. No. 13/665,366. |
| USPTO; Final Office Action dated Mar. 1, 2016 in U.S. Appl. No. 13/665,366. |
| USPTO; Advisory Action dated May 13, 2016 in U.S. Appl. No. 13/665,366. |
| USPTO; Non-Final Office Action dated Jun. 17, 2016 in U.S. Appl. No. 13/665,366. |
| USPTO; Final Office Action dated May 3, 2017 in U.S. Appl. No. 13/665,366. |
| USPTO; Non-Final Office Action dated Apr. 3, 2015 in U.S. Appl. No. 13/677,133. |
| USPTO; Notice of Allowance dated Aug. 4, 2015 in U.S. Appl. No. 13/677,133. |
| USPTO; Notice of Allowance dated Aug. 24, 2015 in U.S. Appl. No. 13/677,133. |
| USPTO; Office Action dated Jun. 2, 2014 in U.S. Appl. No. 13/677,151. |
| USPTO; Final Office Action dated Nov. 14, 2014 in U.S. Appl. No. 13/677,151. |
| USPTO; Notice of Allowance dated Feb. 26, 2015 in U.S. Appl. No. 13/677,151. |
| USPTO; Notice of Allowance dated Mar. 17, 2015 in U.S. Appl. No. 13/677,151. |
| USPTO; Non-Final Office Action dated Aug. 20, 2013 in U.S. Appl. No. 13/679,502. |
| USPTO; Final Office Action dated Feb. 25, 2014 in U.S. Appl. No. 13/679,502. |
| USPTO; Notice of Allowance dated May 2, 2014 in U.S. Appl. No. 13/679,502. |
| USPTO; Non-Final Office Action dated Jul. 21, 2015 in U.S. Appl. No. 13/727,324. |
| USPTO; Final Office Action dated Jan. 22, 2016 in U.S. Appl. No. 13/727,324. |
| USPTO; Advisory Action dated Apr. 6, 2016 in U.S. Appl. No. 13/727,324. |
| USPTO; Non-Final Office Action dated May 25, 206 in U.S. Appl. No. 13/727,324. |
| USPTO; Final Office Action dated Dec. 1, 2016 in U.S. Appl. No. 13/727,324. |
| USPTO; Notice of Allowance dated Mar. 1, 2017 in U.S. Appl. No. 13/727,324. |
| USPTO; Non-Final Office Action dated Oct. 24, 2013 in U.S. Appl. No. 13/749,878. |
| USPTO; Non-Final Office Action dated Jun. 18, 2014 in U.S. Appl. No. 13/749,878. |
| USPTO; Final Office Action dated Dec. 10, 2014 in U.S. Appl. No. 13/749,878. |
| USPTO; Notice of Allowance dated Mar. 13, 2015 dated in U.S. Appl. No. 13/749,878. |
| USPTO; Non-Final Office Action dated Sep. 16, 2013 in U.S. Appl. No. 13/760,160. |
| USPTO; Final Office Action dated Dec. 27, 2013 in U.S. Appl. No. 13/760,160. |
| USPTO; Non-Final Office Action dated Jun. 4, 2014 in U.S. Appl. No. 13/760,160. |
| USPTO; Final Office Action dated Sep. 25, 2014 in U.S. Appl. No. 13/760,160. |
| USPTO; Final Office Action dated Jan. 28, 2015 in U.S. Appl. No. 13/760,160. |
| USPTO; Final Office Action dated May 12, 2015 in U.S. Appl. No. 13/760,160. |
| USPTO; Notice of Allowance dated Oct. 21, 2015 in U.S. Appl. No. 13/760,160. |
| USPTO; Notice of Allowance dated Jan. 20, 2016 in U.S. Appl. No. 13/760,160. |
| USPTO; Office Action dated Apr. 23, 2014 in U.S. Appl. No. 13/784,362. |
| USPTO; Notice of Allowance dated Aug. 13, 2014 in U.S. Appl. No. 13/784,362. |
| USPTO; Non-Final Office Action dated Dec. 19, 2013 in U.S. Appl. No. 13/784,388. |
| USPTO; Notice of Allowance dated Jun. 4, 2014 in U.S. Appl. No. 13/784,388. |
| USPTO; Restriction Requirement dated May 8, 2014 in U.S. Appl. No. 13/791,246. |
| USPTO; Non-Final Office Action dated Sep. 19, 2014 in U.S. Appl. No. 13/791,246. |
| USPTO; Final Office Action dated Mar. 25, 2015 in U.S. Appl. No. 13/791,246. |
| USPTO; Non-Final Office Action dated Oct. 26, 2015 in U.S. Appl. No. 13/791,246. |
| USPTO; Final Office Action dated Apr. 20, 2016 in U.S. Appl. No. 13/791,246. |
| USPTO; Advisory Action dated Jul. 13, 2016 in U.S. Appl. No. 13/791,246. |
| USPTO; Non-Final Office Action dated Aug. 11, 2016 in U.S. Appl. No. 13/791,246. |
| USPTO; Notice of Allowance dated Oct. 19, 2016 in U.S. Appl. No. 13/791,246. |
| USPTO; Notice of Allowance dated Nov. 25, 2016 in U.S. Appl. No. 13/791,246. |
| USPTO; Non-Final Office Action dated Nov. 6, 2015 in U.S. Appl. No. 13/791,339. |
| USPTO; Final Office Action dated Apr. 12, 2016 in U.S. Appl. No. 13/791,339. |
| USPTO; Advisory Action dated Jul. 14, 2016 in U.S. Appl. No. 13/791,339. |
| USPTO; Notice of Allowance dated Aug. 24, 2016 in U.S. Appl. No. 13/791,339. |
| USPTO; Non-Final Office Action dated Mar. 21, 2014 in U.S. Appl. No. 13/799,708. |
| USPTO; Notice of Allowance dated Oct. 31, 2014 in U.S. Appl. No. 13/799,708. |
| USPTO; Non-Final Office Action dated Sep. 1, 2016 in U.S. Appl. No. 14/827,177. |
| USPTO; Restriction Requirement dated Jun. 26, 2014 in U.S. Appl. No. 13/874,708. |
| USPTO; Non-Final Office Action dated Oct. 9, 2014 in U.S. Appl. No. 13/874,708. |
| USPTO; Notice of Allowance dated Mar. 10, 2015 in U.S. Appl. No. 13/874,708. |
| USPTO; Notice of Allowance dated Apr. 10, 2014 in U.S. Appl. No. 13/901,341. |
| USPTO; Notice of Allowance dated Jun. 6, 2014 in U.S. Appl. No. 13/901,341. |
| USPTO; Non-Final Office Action dated Jan. 2, 2015 in U.S. Appl. No. 13/901,372. |
| USPTO; Final Office Action dated Apr. 16, 2015 in U.S. Appl. No. 13/901,372. |
| USPTO; Notice of Allowance dated Aug. 5, 2015 in U.S. Appl. No. 13/901,372. |
| USPTO; Advisory Action dated Jun. 29, 2015 in U.S. Appl. No. 13/901,372. |
| USPTO; Non-Final Office Action dated Jul. 8, 2015 in U.S. Appl. No. 13/901,400. |
| USPTO; Final Office Action dated Jan. 14, 2016 in U.S. Appl. No. 13/901,400. |
| USPTO; Notice of Allowance dated Apr. 12, 2016 in U.S. Appl. No. 13/901,400. |
| USPTO; Non-Final Office Action dated Apr. 24, 2014 in U.S. Appl. No. 13/912,666. |
| USPTO; Final Office Action dated Sep. 25, 2014 in U.S. Appl. No. 13/912,666. |
| USPTO; Advisory Action dated Dec. 11, 2014 in U.S. Appl. No. 13/912,666. |
| USPTO; Non-Final Office Action dated Jan. 26, 2015 in U.S. Appl. No. 13/912,666. |
| USPTO; Notice of Allowance dated Jun. 25, 2015 in U.S. Appl. No. 13/912,666. |
| USPTO; Requirement for Restriction dated Sep. 4, 2014 in U.S. Appl. No. 13/915,732. |
| USPTO; Non-Final Office Action dated Dec. 16, 2014 in U.S. Appl. No. 13/915,732. |
| USPTO; Final Office Action dated Apr. 10, 2015 in U.S. Appl. No. 13/915,732. |
| USPTO; Notice of Allowance dated Jun. 19, 2015 in U.S. Appl. No. 13/915,732. |
| USPTO; Notice of Allowance dated Mar. 17, 2015 in U.S. Appl. No. 13/923,197. |
| USPTO; Non-Final Office Action dated Sep. 12, 2014 in U.S. Appl. No. 13/941,134. |
| USPTO; Notice of Allowance dated Jan. 20, 2015 in U.S. Appl. No. 13/941,134. |
| USPTO; Restriction Requirement dated Apr. 30, 2015 in U.S. Appl. No. 13/941,216. |
| USPTO; Non-Final Office Action dated Jul. 30, 2015 in U.S. Appl. No. 13/941,216. |
| USPTO; Final Office Action dated Mar. 1, 2016 in U.S. Appl. No. 13/941,216. |
| USPTO; Non-Final Office Action dated Jun. 15, 2016 in U.S. Appl. No. 13/941,216. |
| USPTO; Notice of Allowance dated Sep. 13, 2016 in U.S. Appl. No. 13/941,216. |
| USPTO; Notice of Allowance dated Nov. 14, 2016 in U.S. Appl. No. 13/941,216. |
| USPTO; Non-Final Office Action dated Jan. 14, 2014 in U.S. Appl. No. 13/941,226. |
| USPTO; Non-Final Office Action dated Jul. 8, 2014 in U.S. Appl. No. 13/941,226. |
| USPTO; Non-Final Office Action dated Feb. 3, 2015 in U.S. Appl. No. 13/941,226. |
| USPTO; Final Office Action dated Feb. 12, 2016 in U.S. Appl. No. 13/941,226. |
| USPTO; Advisory Action dated Jul. 29, 2016 in U.S. Appl. No. 13/941,226. |
| USPTO; Non-Final Office Action dated Aug. 8, 2017 in U.S. Appl. No. 13/941,226. |
| USPTO; Restriction Requirement dated Sep. 16, 2014 in U.S. Appl. No. 13/948,055. |
| USPTO; Non-Final Office Action dated Oct. 30, 2014 in U.S. Appl. No. 13/948,055. |
| USPTO; Notice of Allowance dated Feb. 27, 2015 in U.S. Appl. No. 13/948,055. |
| USPTO; Notice of Allowance dated Mar. 31, 2015 in U.S. Appl. No. 13/948,055. |
| USPTO; Non-Final Office Action dated Jun. 29, 2015 in U.S. Appl. No. 13/966,782. |
| USPTO; Final Office Action dated Jan. 4, 2016 in U.S. Appl. No. 13/966,782. |
| USPTO; Notice of Allowance dated Mar. 21, 2016 in U.S. Appl. No. 13/966,782. |
| USPTO; Notice of Allowance dated Oct. 7, 2015 in U.S. Appl. No. 13/973,777. |
| USPTO; Non-Final Office Action dated Feb. 20, 2015 in U.S. Appl. No. 14/018,231. |
| USPTO; Notice of Allowance dated Jul. 20, 2015 in U.S. Appl. No. 14/018,231. |
| USPTO; Restriction Requirement Action dated Jan. 28, 2015 in U.S. Appl. No. 14/018,345. |
| USPTO; Non-Final Office Action dated Apr. 7, 2015 in U.S. Appl. No. 14/018,345. |
| USPTO; Final Office Action dated Sep. 14, 2015 in U.S. Appl. No. 14/018,345. |
| USPTO; Notice of Allowance dated Jan. 14, 2016 in U.S. Appl. No. 14/018,345. |
| USPTO; Notice of Allowance dated Mar. 17, 2016 in U.S. Appl. No. 14/018,345. |
| USPTO; Non-Final Office Action dated Mar. 26, 2015 in U.S. Appl. No. 14/031,982. |
| USPTO; Final Office Action dated Aug. 28, 2015 in U.S. Appl. No. 14/031,982. |
| USPTO; Notice of Allowance dated Nov. 17, 2015 in U.S. Appl. No. 14/031,982. |
| USPTO; Non-Final Office Action Restriction dated Jan. 2, 2015 in U.S. Appl. No. 14/040,196. |
| USPTO; Non-Final Office Action dated Apr. 28, 2015 in U.S. Appl. No. 14/040,196. |
| USPTO; Notice of Allowance dated Sep. 11, 2015 in U.S. Appl. No. 14/040,196. |
| USPTO; Non-Final Action dated Dec. 3, 2015 in U.S. Appl. No. 14/050,150. |
| USPTO; Final Office Action dated Jun. 15, 2016 in U.S. Appl. No. 14/050,150. |
| USPTO; Final Office Action dated Jul. 8, 2016 in U.S. Appl. No. 14/050,150. |
| USPTO; Notice of Allowance dated Oct. 20, 2016 in U.S. Appl. No. 14/050,150. |
| USPTO; Non-Final Office Action dated Dec. 15, 2014 in U.S. Appl. No. 14/065,114. |
| USPTO; Final Office Action dated Jun. 19, 2015 in U.S. Appl. No. 14/065,114. |
| USPTO; Advisory Action dated Aug. 24, 2015 in U.S. Appl. No. 14/065,114. |
| USPTO; Non-Final Office Action dated Oct. 7, 2015 in U.S. Appl. No. 14/065,114. |
| USPTO; Notice of Allowance dated Feb. 22, 2016 in U.S. Appl. No. 14/065,114. |
| USPTO; Non-Final Office Action dated Nov. 14, 2014 in U.S. Appl. No. 14/069,244. |
| USPTO; Notice of Allowance dated Mar. 25, 2015 in U.S. Appl. No. 14/069,244. |
| USPTO; Non-Final Office Action dated Mar. 19, 2015 in U.S. Appl. No. 14/079,302. |
| USPTO; Final Office Action dated Sep. 1, 2015 in U.S. Appl. No. 14/079,302. |
| USPTO; Non-Final Office Action dated Dec. 23, 2015 in U.S. Appl. No. 14/079,302. |
| USPTO; Non-Final Office Action dated Apr. 27, 2016 in U.S. Appl. No. 14/079,302. |
| USPTO; Final Office Action dated Aug. 22, 2016 in U.S. Appl. No. 14/079,302. |
| USPTO; Notice of Allowance dated Dec. 14, 2016 in U.S. Appl. No. 14/079,302. |
| USPTO; Requirement for Restriction dated Aug. 11, 2015 in U.S. Appl. No. 14/090,750. |
| USPTO; Non-Final Office Action dated Sep. 9, 2015 in U.S. Appl. No. 14/090,750. |
| USPTO; Final Office Action dated Feb. 11, 2016 in U.S. Appl. No. 14/090,750. |
| USPTO; Advisory Action dated May 5, 2016 in U.S. Appl. No. 14/090,750. |
| USPTO; Non-Final Office Action dated Jun. 14, 2016 in U.S. Appl. No. 14/090,750. |
| USPTO; Advisory Action dated Dec. 21, 2016 in U.S. Appl. No. 14/090,750. |
| USPTO; Advisory Action dated Jan. 30, 2018 in U.S. Appl. No. 14/090,750. |
| USPTO; Final Office Action dated Sep. 28, 2016 in U.S. Appl. No. 14/090,750. |
| USPTO; Non Final Office Action dated Jun. 23, 2017 in U.S. Appl. No. 14/090,750. |
| USPTO; Final Office Action dated Nov. 17, 2017 in U.S. Appl. No. 14/090,750. |
| USPTO; Non-Final Office Action dated Mar. 12, 2018 in U.S. Appl. No. 14/090,750. |
| USPTO; Non-Final Office Action dated Mar. 19, 2015 in U.S. Appl. No. 14/166,462. |
| USPTO; Notice of Allowance dated Sep. 3, 2015 in U.S. Appl. No. 14/166,462. |
| USPTO; Non-Final Office Action dated Nov. 17, 2015 in U.S. Appl. No. 14/172,220. |
| USPTO; Office Action dated May 29, 2014 in U.S. Appl. No. 14/183,187. |
| USPTO; Final Office Action dated Nov. 7, 2014 in U.S. Appl. No. 14/183,187. |
| USPTO; Advisory Action dated Feb. 20, 2015 in U.S. Appl. No. 14/183,187. |
| USPTO; Non-Final Office Action dated Mar. 16, 2015 in U.S. Appl. No. 14/183,187. |
| USPTO; Final Office Action dated Jul. 10, 2015 in U.S. Appl. No. 14/183,187. |
| USPTO; Notice of Allowance dated Aug. 31, 2015 in U.S. Appl. No. 14/183,187. |
| USPTO; Requirement for Restriction dated Sep. 24, 2015 in U.S. Appl. No. 14/188,760. |
| USPTO; Non-Final Office Action dated Jan. 11, 2016 in U.S. Appl. No. 14/188,760. |
| USPTO; Final Office Action dated Aug. 25, 2016 in U.S. Appl. No. 14/188,760. |
| USPTO; Advisory Action dated Jan. 12, 2017 in U.S. Appl. No. 14/188,760. |
| USPTO; Non-Final Office Action dated Mar. 23, 2017 in U.S. Appl. No. 14/188,760. |
| USPTO; Final Office Action dated Oct. 5, 2017 in U.S. Appl. No. 14/188,760. |
| USPTO; Advisory Action dated Jan. 3, 2018 in U.S. Appl. No. 14/188,760. |
| USPTO; Non-Final Office Action dated Apr. 18, 2018 in U.S. Appl. No. 14/188,760. |
| USPTO; Non-Final Office Action dated Oct. 8, 2015 in U.S. Appl. No. 14/218,374. |
| USPTO; Final Office Action dated Feb. 23, 2016 in U.S. Appl. No. 14/218,374. |
| USPTO; Advisory Action dated Apr. 29, 2016 in U.S. Appl. No. 14/218,374. |
| USPTO; Notice of Allowance dated Aug. 5, 2016 in U.S. Appl. No. 14/218,374. |
| USPTO; Restriction Requirement dated May 20, 2016 in U.S. Appl. No. 14/218,690. |
| USPTO; Non-Final Office Action dated Jul. 15, 2016 in U.S. Appl. No. 14/218,690. |
| USPTO; Final Office Action dated Nov. 14, 2016 in U.S. Appl. No. 14/218,690. |
| USPTO; Non-Final Office Action dated Apr. 6, 2017 in U.S. Appl. No. 14/218,690. |
| USPTO; Final Office Action dated Jul. 20, 2017 in U.S. Appl. No. 14/218,690. |
| USPTO; Non-Final Office Action dated Jan. 11, 2018 in U.S. Appl. No. 14/218,690. |
| USPTO; Final Office Action dated May 24, 2018 in U.S. Appl. No. 14/218,690. |
| USPTO; Non-Final Office Action dated Sep. 22, 2015 in U.S. Appl. No. 14/219,839. |
| USPTO; Final Office Action dated Mar. 25, 2016 in U.S. Appl. No. 14/219,839. |
| USPTO; Non-Final Office Action dated Dec. 22, 2016 in U.S. Appl. No. 14/219,839. |
| USPTO; Advisory Action dated Jun. 30, 2016 in U.S. Appl. No. 14/219,839. |
| USPTO; Final Office Action dated Jul. 6, 2017 in U.S. Appl. No. 14/219,839. |
| USPTO; Non-Final Office Action dated Mar. 27, 2018 in U.S. Appl. No. 14/219,839. |
| USPTO; Non-Final Office Action dated Nov. 25, 2015 in U.S. Appl. No. 14/219,879. |
| USPTO; Final Office action dated May 19, 2016 in U.S. Appl. No. 14/219,879. |
| USPTO; Advisory Action dated Aug. 22, 2016 in U.S. Appl. No. 14/219,879. |
| USPTO; Non-Final Office Action dated Dec. 23, 2016 in U.S. Appl. No. 14/219,879. |
| USPTO; Final Office action dated Jul. 6, 2017 in U.S. Appl. No. 14/219,879. |
| USPTO; Advisory Action dated Oct. 5, 2017 in U.S. Appl. No. 14/219,879. |
| USPTO; Non-Final Office Action dated Apr. 6, 2018 in U.S. Appl. No. 14/219,879. |
| USPTO; Non-Final Office Action dated Sep. 18, 2015 in U.S. Appl. No. 14/244,689. |
| USPTO; Notice of Allowance dated Feb. 11, 2016 in U.S. Appl. No. 14/244,689. |
| USPTO; Non-Final Office Action dated Oct. 7, 2015 in U.S. Appl. No. 14/246,969. |
| USPTO; Final Office Action dated May 4, 2016 in U.S. Appl. No. 14/246,969. |
| USPTO; Advisory Action dated Aug. 2, 2016 in U.S. Appl. No. 14/246,969. |
| USPTO; Non Final Office Action dated Aug. 12, 2016 in U.S. Appl. No. 14/246,969. |
| USPTO; Notice of Allowance dated Feb. 27, 2017 in U.S. Appl. No. 14/246,969. |
| USPTO; Non-Final Office Action dated Nov. 20, 2015 in U.S. Appl. No. 14/260,701. |
| USPTO; Notice of Allowance dated Jun. 2, 2016 in U.S. Appl. No. 14/260,701. |
| USPTO; Notice of Allowance dated Feb. 23, 2016 in U.S. Appl. No. 14/327,134. |
| USPTO; Requirement for Restriction dated Jun. 15, 2015 in U.S. Appl. No. 14/268,348. |
| USPTO; Non-Final Office Action dated Aug. 19, 2015 in U.S. Appl. No. 14/268,348. |
| USPTO; Non-Final Office Action dated Jan. 6, 2016 in U.S. Appl. No. 14/268,348. |
| USPTO; Final Office Action dated Apr. 29, 2016 in U.S. Appl. No. 14/268,348. |
| USPTO; Notice of Allowance dated Aug. 30, 2016 in U.S. Appl. No. 14/268,348. |
| USPTO; Requirement for Restriction dated May 21, 2015 in U.S. Appl. No. 14/281,477. |
| USPTO; Non-Final Office Action dated Oct. 20, 2015 in U.S. Appl. No. 14/281,477. |
| USPTO; Advisory Action dated Mar. 28, 2016 in U.S. Appl. No. 14/281,477. |
| USPTO; Non-Final Office Action dated Jan. 13, 2017 in U.S. Appl. No. 14/444,744. |
| USPTO; Final Office Action dated Jul. 10, 2017 in U.S. Appl. No. 14/444,744. |
| USPTO; Non-Final Office Action dated Nov. 29, 2017 in U.S. Appl. No. 14/444,744. |
| USPTO; Final Office Action dated Mar. 28, 2018 in U.S. Appl. No. 14/444,744. |
| USPTO; Non-Final Office Action dated Jul. 27, 2018 in U.S. Appl. No. 14/444,744. |
| USPTO; Non-Final Office Action dated May 18, 2016 in U.S. Appl. No. 14/449,838. |
| USPTO; Notice of Allowance dated Nov. 28, 2016 in U.S. Appl. No. 14/449,838. |
| USPTO; Non-Final Office Action dated Feb. 12, 2015 in U.S. Appl. No. 14/457,058. |
| USPTO; Final Office Action dated Jul. 14, 2015 in U.S. Appl. No. 14/457,058. |
| USPTO; Non-Final Office Action dated Nov. 6, 2015 in U.S. Appl. No. 14/457,058. |
| USPTO; Final Office Acton dated Jun. 17, 2016 in U.S. Appl. No. 14/457,058. |
| USPTO; Advisory Action dated Sep. 21, 2016 in U.S. Appl. No. 14/457,058. |
| USPTO; Non-Final Office Action dated Oct. 6, 2016 in U.S. Appl. No. 14/457,058. |
| USPTO; Final Office Acton dated May 4, 2017 in U.S. Appl. No. 14/457,058. |
| USPTO; Non-Final Office Action dated Oct. 19, 2017 in U.S. Appl. No. 14/457,058. |
| USPTO; Final Office Action dated Jun. 14, 2018 in U.S. Appl. No. 14/457,058. |
| USPTO; Non-Final Office Action dated Sep. 16, 2016 in U.S. Appl. No. 14/465,252. |
| USPTO; Final Office Action dated Nov. 1, 2016 in U.S. Appl. No. 14/465,252. |
| USPTO; Non-Final Office Action dated Mar. 6, 2017 in U.S. Appl. No. 14/465,252. |
| USPTO; Final Office Action dated Jun. 9, 2017 in U.S. Appl. No. 14/465,252. |
| USPTO; Notice of Allowance dated Oct. 3, 2017 in U.S. Appl. No. 14/465,252. |
| USPTO; Non-Final Office Action dated May 31, 2018 in U.S. Appl. No. 15/491,726. |
| USPTO; Requirement for Restriction dated Sep. 3, 2015 in U.S. Appl. No. 14/498,036. |
| USPTO; Non-Final Office Action dated Nov. 24, 2015 in U.S. Appl. No. 14/498,036. |
| USPTO; Final Office Action dated Apr. 5, 2016 in U.S. Appl. No. 14/498,036. |
| USPTO; Advisory Action dated Jun. 16, 2016 in U.S. Appl. No. 14/498,036. |
| USPTO; Notice of Allowance dated Aug. 17, 2016 in U.S. Appl. No. 14/498,036. |
| USPTO; Requirement for Restriction dated Mar. 20, 2015 in U.S. Appl. No. 14/505,290. |
| USPTO; Non-Final Office Action dated Apr. 10, 2015 in U.S. Appl. No. 14/505,290. |
| USPTO; Notice of Allowance dated Aug. 21, 2015 in U.S. Appl. No. 14/505,290. |
| USPTO; Non-Final Office Action dated Dec. 17, 2015 in U.S. Appl. No. 14/508,296. |
| USPTO; Final Office Action dated May 26, 2016 in U.S. Appl. No. 14/508,296. |
| USPTO; Advisory Action dated Aug. 17, 2016 in U.S. Appl. No. 14/508,296. |
| USPTO; Non-Final Office Action dated Sep. 8, 2016 in U.S. Appl. No. 14/508,296. |
| USPTO; Final Office Action dated Dec. 7, 2016 in U.S. Appl. No. 14/508,296. |
| USPTO; Notice of Allowance dated Jan. 27, 2017 in U.S. Appl. No. 14/508,296. |
| USPTO; Restriction for Requirement dated Dec. 30, 2016 in U.S. Appl. No. 14/508,489. |
| USPTO; Non-Final Office Action dated Apr. 6, 2017 in U.S. Appl. No. 14/508,489. |
| USPTO; Final Office Action dated Oct. 4, 2017 in U.S. Appl. No. 14/508,489. |
| USPTO; Non-Final Office Action dated May 15, 2018 in U.S. Appl. No. 14/508,489. |
| USPTO; Non-Final Office Action dated Jan. 16, 2015 in U.S. Appl. No. 14/563,044. |
| USPTO; Final Office Action dated Jul. 16, 2015 in U.S. Appl. No. 14/563,044. |
| USPTO; Notice of Allowance dated Oct. 15, 2015 in U.S. Appl. No. 14/563,044. |
| USPTO; Notice of Allowance dated Dec. 2, 2015 in U.S. Appl. No. 14/563,044. |
| USPTO; Non-Final Office Action dated May 4, 2016 in U.S. Appl. No. 14/568,647. |
| USPTO; Final Office Action dated Sep. 29, 2016 in U.S. Appl. No. 14/568,647. |
| USPTO; Advisory Action dated Dec. 21, 2016 in U.S. Appl. No. 14/568,647. |
| USPTO; Non-Final Office Action dated Feb. 2, 2017 in U.S. Appl. No. 14/568,647. |
| USPTO; Final Office Action dated May 19, 2017 in U.S. Appl. No. 14/568,647. |
| USPTO; Non-Final Office Action dated Sep. 14, 2017 in U.S. Appl. No. 14/568,647. |
| USPTO; Final Office Action dated Jan. 23, 2018 in U.S. Appl. No. 14/568,647. |
| USPTO; Advisory Action dated Apr. 12, 2018 in U.S. Appl. No. 14/568,647. |
| USPTO; Non-Final Office Action dated May 25, 2018 in U.S. Appl. No. 14/568,647. |
| USPTO; Non-Final Office Action dated Oct. 1, 2015 in U.S. Appl. No. 14/571,126. |
| USPTO; Final Office Action dated Feb. 22, 2016 in U.S. Appl. No. 14/571,126. |
| USPTO; Notice of Allowance dated May 18, 2016 in U.S. Appl. No. 14/571,126. |
| USPTO; Notice of Allowance dated Jun. 2, 2016 in U.S. Appl. No. 14/571,126. |
| USPTO; Non-Final Office Action dated Nov. 25, 2015 in U.S. Appl. No. 14/598,532. |
| USPTO; Notice of Allowance dated May 16, 2016 in U.S. Appl. No. 14/598,532. |
| USPTO; Non-Final Office Action dated Jan. 15, 2016 in U.S. Appl. No. 14/606,364. |
| USPTO; Restriction Requirement dated Mar. 7, 2016 in U.S. Appl. No. 14/606,364. |
| USPTO; Final Office Action dated Jun. 14, 2016 in U.S. Appl. No. 14/606,364. |
| USPTO; Advisory Action dated Aug. 25, 2016 in U.S. Appl. No. 14/606,364. |
| USPTO; Non-Final Office Action dated Sep. 27, 2016 in U.S. Appl. No. 14/606,354. |
| USPTO; Final Office Action dated Jan. 12, 2017 in U.S. Appl. No. 14/606,364. |
| USPTO; Non-Final Office Action dated May 10, 2017 in U.S. Appl. No. 14/606,364. |
| USPTO; Non-Final Office Action dated Mar. 3, 2016 in U.S. Appl. No. 14/622,603. |
| USPTO; Notice of Allowance dated Aug. 2, 2016 in U.S. Appl. No. 14/622,603. |
| USPTO; Notice of Allowance dated Feb. 16, 2016 in U.S. Appl. No. 14/634,342. |
| USPTO; Non-Final Office Action dated Oct. 19, 2017 in U.S. Appl. No. 14/645,234. |
| USPTO; Non-Final Office Action dated May 16, 2018 in U.S. Appl. No. 14/645,234. |
| USPTO; Final Office Action dated Aug. 10, 2018 in U.S. Appl. No. 14/645,234. |
| USPTO; Non-Final Office Action dated Jun. 7, 2017 in U.S. Appl. No. 14/656,588. |
| USPTO; Final Office Action dated Dec. 26, 2017 in U.S. Appl. No. 14/656,588. |
| USPTO; Non-Final Office Action dated Apr. 6, 2018 in U.S. Appl. No. 14/656,588. |
| USPTO; Requirement for Restriction dated Oct. 26, 2015 in U.S. Appl. No. 14/659,152. |
| USPTO; Non-Final Office Action dated Mar. 21, 2016 in U.S. Appl. No. 14/659,152. |
| USPTO; Final Office Action dated Jul. 29, 2016 in U.S. Appl. No. 14/659,152. |
| USPTO; Notice of Allowance dated Nov. 22, 2016 in U.S. Appl. No. 14/659,152. |
| USPTO; Non-Final Office Action dated Sep. 7, 2017 in U.S. Appl. No. 14/660,755. |
| USPTO; Restriction Requirement dated Sep. 11, 2017 in U.S. Appl. No. 14/660,755. |
| USPTO; Notice of Allowance dated Oct. 2, 2017 in U.S. Appl. No. 14/660,755. |
| USPTO; Notice of Allowance dated Mar. 25, 2016 in U.S. Appl. No. 14/693,138. |
| USPTO; Requirement for Restriction dated Jul. 5, 2017 in U.S. Appl. No. 14/752,712. |
| USPTO; Non-Final Office Action dated Aug. 3, 2017 in U.S. Appl. No. 14/752,712. |
| USPTO; Final Office Action dated Nov. 29, 2017 in U.S. Appl. No. 14/752,712. |
| USPTO; Advisory Action dated Feb. 15, 2018 in U.S. Appl. No. 14/752,712. |
| USPTO; Non-Final Office Action dated Mar. 21, 2018 in U.S. Appl. No. 14/752,712. |
| USPTO; Non-Final Office Action dated Nov. 29, 2017 in U.S. Appl. No. 14/793,323. |
| USPTO; Final Office Action dated Mar. 29, 2018 in U.S. Appl. No. 14/793,323. |
| USPTO; Non-Final Office Action dated Aug. 10, 2018 in U.S. Appl. No. 14/793,323. |
| USPTO; Non-Final Office Action dated Jun. 16, 2017 in U.S. Appl. No. 14/798,136. |
| USPTO; Notice of Allowance dated Oct. 5, 2017 in U.S. Appl. No. 14/798,136. |
| USPTO; Non-Final Office Action dated Mar. 30, 2016 in U.S. Appl. No. 14/808,979. |
| USPTO; Final Office Acton dated Sep. 30, 2016 in U.S. Appl. No. 14/808,979. |
| USPTO; Non-Final Office Action dated Dec. 20, 2016 in U.S. Appl. No. 14/808,979. |
| USPTO; Final Office Action dated Jun. 8, 2017 in U.S. Appl. No. 14/808,979. |
| USPTO; Non-Final Office Action dated Sep. 21, 2017 in U.S. Appl. No. 14/808,979. |
| USPTO; Final Office Action dated Mar. 14, 2018 in U.S. Appl. No. 14/808,979. |
| USPTO; Notice of Allowance dated Jun. 27, 2018 in U.S. Appl. No. 14/808,979. |
| USPTO; Non-Final Office Action dated Feb. 23, 2018 in U.S. Appl. No. 14/817,953. |
| USPTO; Notice of Allowance dated Jul. 11, 2018 in U.S. Appl. No. 14/817,953. |
| USPTO; Requirement for Restriction dated Mar. 17, 2016 in U.S. Appl. No. 14/827,177. |
| USPTO; Notice of Allowance dated Jan. 27, 2017 in U.S. Appl. No. 14/827,177. |
| USPTO; Requirement for Restriction dated Aug. 8, 2016 in U.S. Appl. No. 14/829,565. |
| USPTO; Non-Final Office Action dated Sep. 9, 2016 in U.S. Appl. No. 14/829,565. |
| USPTO; Final Office Action dated Feb. 9, 2017 in U.S. Appl. No. 14/829,565. |
| USPTO; Advisory Action dated Apr. 20, 2017 in U.S. Appl. No. 14/829,565. |
| USPTO; Non-Final Office Action dated Sep. 19, 2017 in U.S. Appl. No. 14/829,565. |
| USPTO; Final Office Action dated Mar. 5, 2018 in U.S. Appl. No. 14/829,565. |
| USPTO; Non-Final Office Action dated Apr. 29, 2016 in U.S. Appl. No. 14/835,637. |
| USPTO; Final Office Action dated Nov. 25, 2016 in U.S. Appl. No. 14/835,637. |
| USPTO; Advisory Action dated Feb. 14, 2017 in U.S. Appl. No. 14/835,637. |
| USPTO; Notice of Allowance dated Apr. 25, 2017 in U.S. Appl. No. 14/835,637. |
| USPTO; Non-Final Office Action dated Jul. 29, 2016 in U.S. Appl. No. 14/884,695. |
| USPTO; Final Office Action dated Feb. 9, 2017 in U.S. Appl. No. 14/884,695. |
| USPTO; Advisory Action dated Apr. 20, 2017 in U.S. Appl. No. 14/884,695. |
| USPTO; Non-Final Office Action dated May 18, 2017 in U.S. Appl. No. 14/884,695. |
| USPTO; Requirement for Restriction dated Dec. 1, 2016 in U.S. Appl. No. 14/886,571. |
| USPTO; Non-Final Office Action dated May 18, 2017 in U.S. Appl. No. 14/886,571. |
| USPTO; Final Office Action dated Sep. 21, 2017 in U.S. Appl. No. 14/886,571. |
| USPTO; Notice of Allowance dated Dec. 6, 2017 in U.S. Appl. No. 14/886,571. |
| USPTO; Requirement for Restriction dated Sep. 20, 2016 in U.S. Appl. No. 14/919,536. |
| USPTO; Non-Final Office Action dated Dec. 1, 2016 in U.S. Appl. No. 14/919,536. |
| USPTO; Final Office Action dated Mar. 28, 2017 in U.S. Appl. No. 14/919,536. |
| USPTO; Non-Final Office Action dated Aug. 29, 2017 in U.S. Appl. No. 14/919,536. |
| USPTO; Final Office Action dated May 11, 2018 in U.S. Appl. No. 14/919,536. |
| USPTO; Non-Final Office Action dated May 3, 2016 in U.S. Appl. No. 14/937,053. |
| USPTO; Notice of Allowance dated Jul. 26, 2016 in U.S. Appl. No. 14/937,053. |
| USPTO; Requirement for Restriction dated Sep. 15, 2016 in U.S. Appl. No. 14/938,180. |
| USPTO; Non-Final Office Action dated Dec. 15, 2016 in U.S. Appl. No. 14/938,180. |
| USPTO; Notice of Allowance dated Nov. 9, 2017 in U.S. Appl. No. 14/938,180. |
| USPTO; Non-Final Office Action dated Apr. 14, 2017 in U.S. Appl. No. 14/956,115. |
| USPTO; Final Office Action dated Jul. 21, 2017 in U.S. Appl. No. 14/956,115. |
| USPTO; Notice of Allowance dated Dec. 14, 2017 in U.S. Appl. No. 14/956,115. |
| USPTO; Notice of Allowance dated Feb. 3, 2017 in U.S. Appl. No. 14/977,291. |
| USPTO; Non-Final Office Action dated Aug. 12, 2016 in U.S. Appl. No. 14/981,434. |
| USPTO; Notice of Allowance dated Nov. 21, 2016 in U.S. Appl. No. 14/981,434. |
| USPTO; Non-Final Office Action dated Jan. 12, 2017 in U.S. Appl. No. 14/981,468. |
| USPTO; Notice of Allowance dated Jun. 7, 2017 in U.S. Appl. No. 14/981,468. |
| USPTO; Non-Final Office Action dated Mar. 22, 2016 in U.S. Appl. No. 14/987,420. |
| USPTO; Non-Final Office Action dated Dec. 14, 2016 in U.S. Appl. No. 14/997,683. |
| USPTO; Final Office Action dated Apr. 14, 2017 in U.S. Appl. No. 14/997,683. |
| USPTO; Non-Final Office Action dated Sep. 1, 2017 in U.S. Appl. No. 14/997,683. |
| USPTO; Final Office Action dated Feb. 6, 2018 in U.S. Appl. No. 14/997,683. |
| USPTO; Advisory Action dated May 2, 2018 in U.S. Appl. No. 14/997,683. |
| USPTO; Non-Final Office Action dated Jun. 20, 2018 in U.S. Appl. No. 14/997,683. |
| USPTO; Non-Final Office Action dated Sep. 23, 2016 in U.S. Appl. No. 15/048,422. |
| USPTO; Notice of Allowance dated May 4, 2017 in U.S. Appl. No. 15/048,422. |
| USPTO; Requirement for Restriction dated Apr. 19, 2017 in U.S. Appl. No. 15/050,159. |
| USPTO; Non-Final Office Action dated Aug. 4, 2017 in U.S. Appl. No. 15/050,159. |
| USPTO; Notice of Allowance dated Feb. 7, 2018 in U.S. Appl. No. 15/050,159. |
| USPTO; Non-Final Office Action dated Apr. 22, 2016 in U.S. Appl. No. 15/055,122. |
| USPTO; Notice of Allowance dated Sep. 15, 2016 in U.S. Appl. No. 15/055,122. |
| USPTO; Non-Final Office Action dated Feb. 20, 2018 in U.S. Appl. No. 15/060,412. |
| USPTO; Requirement for Restriction dated Jun. 4, 2018 in U.S. Appl. No. 15/067,028. |
| USPTO; Requirement for Restriction dated Jun. 28, 2018 in U.S. Appl. No. 15/074,813. |
| USPTO; Non-Final Office Action dated Jan. 9, 2018 in U.S. Appl. No. 15/135,224. |
| USPTO; Notice of Allowance dated Jun. 29, 2018 in U.S. Appl. No. 15/135,224. |
| USPTO; Non-Final Office Action dated Jan. 9, 2018 in U.S. Appl. No. 15/135,258. |
| USPTO; Final Office Action dated Jul. 6, 2018 in U.S. Appl. No. 15/135,258. |
| USPTO; Non-Final Office Action dated Jan. 9, 2018 in U.S. Appl. No. 15/135,333. |
| USPTO; Non Final Office Action dated Nov. 21, 2016 in U.S. Appl. No. 15/144,481. |
| USPTO; Final Office Action dated May 26, 2017 in U.S. Appl. No. 15/144,481. |
| USPTO; Non-Final Office Action dated Sep. 21, 2017 in U.S. Appl. No. 15/144,481. |
| USPTO; Notice of Allowance dated Apr. 11, 2018 in U.S. Appl. No. 15/144,481. |
| USPTO; Non-Final Office Action dated Apr. 13, 2017 in U.S. Appl. No. 15/144,506. |
| USPTO; Final Office Action dated Oct. 10, 2017 in U.S. Appl. No. 15/144,506. |
| USPTO; Final Office Action dated Jul. 26, 2018 in U.S. Appl. No. 15/144,506. |
| USPTO; Requirement for Restriction dated Jun. 22, 2018 in U.S. Appl. No. 15/182,504. |
| USPTO; Non-Final Office Action dated Nov. 28, 2016 in U.S. Appl. No. 15/203,632. |
| USPTO; Final Office Action dated Jun. 7, 2017 in U.S. Appl. No. 15/203,632. |
| USPTO; Advisory Action dated Aug. 23, 2017 in U.S. Appl. No. 15/203,632. |
| USPTO; Notice of Allowance dated Sep. 20, 2017 in U.S. Appl. No. 15/203,632. |
| USPTO; Non-Final Office Action dated Nov. 29, 2016 in U.S. Appl. No. 15/203,642. |
| USPTO; Final Office Action dated Apr. 13, 2017 in U.S. Appl. No. 15/203,642. |
| USPTO; Advisory Action dated Jun. 22, 2017 in U.S. Appl. No. 15/203,642. |
| USPTO; Notice of Allowance dated Aug. 7, 2017 in U.S. Appl. No. 15/203,642. |
| USPTO; Non-Final Office Action dated Jun. 1, 2017 in U.S. Appl. No. 15/205,827. |
| USPTO; Final Office Action dated Oct. 16, 2017 in U.S. Appl. No. 15/205,827. |
| USPTO; Non-Final Office Action dated May 14, 2018 in U.S. Appl. No. 15/205,827. |
| USPTO; Requirement for Restriction dated Jan. 26, 2017 in U.S. Appl. No. 15/205,890. |
| USPTO; Non-Final Office Action dated Mar. 31, 2017 in U.S. Appl. No. 15/205,890. |
| USPTO; Notice of Allowance dated Oct. 16, 2017 in U.S. Appl. No. 15/205,890. |
| USPTO; Non-Final Office Action dated Jan. 20, 2017 in U.S. Appl. No. 15/210,256. |
| USPTO; Notice of Allowance dated May 18, 2017 in U.S. Appl. No. 15/210,256. |
| USPTO; Notice of Allowance dated Jul. 24, 2017 in U.S. Appl. No. 15/210,256. |
| USPTO; Requirement for Restriction dated Apr. 3, 2017 in U.S. Appl. No. 15/222,715. |
| USPTO; Non Final Office Action dated Apr. 21, 2017 in U.S. Appl. No. 15/222,715. |
| USPTO; Notice of Allowance dated Jul. 14, 2017 in U.S. Appl. No. 15/222,715. |
| USPTO; Notice of Allowance dated Sep. 27, 2017 in U.S. Appl. No. 15/222,715. |
| USPTO; Non-Final Office Action dated Feb. 3, 2017 in U.S. Appl. No. 15/222,738. |
| USPTO; Notice of Allowance dated Feb. 3, 2017 in U.S. Appl. No. 15/222,738. |
| USPTO; Notice of Allowance dated Aug. 23, 2017 in U.S. Appl. No. 15/222,738. |
| USPTO; Non-Final Office Action dated Jan. 17, 2017 in U.S. Appl. No. 15/222,749. |
| USPTO; Final Office Action dated May 5, 2017 in U.S. Appl. No. 15/222,749. |
| USPTO; Non-Final Office Action dated Sep. 7, 2017 in U.S. Appl. No. 15/222,749. |
| USPTO: Final Office Action dated Jun. 4, 2018 in U.S. Appl. No. 15/222,749. |
| USPTO; Non-Final Office Action dated Jan. 3, 2017 in U.S. Appl. No. 15/222,780. |
| USPTO; Final Office Action dated May 5, 2017 in U.S. Appl. No. 15/222,780. |
| USPTO; Non-Final Office Action dated Sep. 7, 2017 in U.S. Appl. No. 15/222,780. |
| USPTO; Final Office Action dated May 17, 2018 in U.S. Appl. No. 15/222,780. |
| USPTO; Requirement for Restriction dated Dec. 5, 2017 in U.S. Appl. No. 15/254,605. |
| USPTO; Notice of Allowance dated Jul. 12, 2018 in U.S. Appl. No. 15/254,605. |
| USPTO; Non-Final Office Action dated Aug. 28, 2017 in U.S. Appl. No. 15/254,724. |
| USPTO; Notice of Allowance dated Jan. 17, 2018 in U.S. Appl. No. 15/254,724. |
| USPTO; Notice of Allowance dated Apr. 2, 2018 in U.S. Appl. No. 15/254,724. |
| USPTO; Non-Final Office Action dated May 22, 2018 in U.S. Appl. No. 15/262,990. |
| USPTO; Non-Final Office Action dated Aug. 3, 2018 in U.S. Appl. No. 15/273,488. |
| USTPO; Non-Final Office Action dated Jul. 2, 2018 in U.S. Appl. No. 15/286,503. |
| USPTO; Requirement for Restriction dated Sep. 12, 2017 in U.S. Appl. No. 15/377,439. |
| USPTO; Non-Final Office Action dated Oct. 23, 2017 in U.S. Appl. No. 15/377,439. |
| USPTO; Final Office Action dated Apr. 16, 2018 in U.S. Appl. No. 15/377,439. |
| USPTO; Advisory Action dated Aug. 8, 2018 in U.S. Appl. No. 15/377,439. |
| USPTO; Notice of Allowance dated Aug. 8, 2017 in U.S. Appl. No. 15/380,895. |
| USPTO; Notice of Allowance dated Oct. 11, 2017 in U.S. Appl. No. 15/380,895. |
| USPTO; Non-Final Office Action dated Jan. 4, 2018 in U.S. Appl. No. 15/380,921. |
| USPTO; Requirement for Restriction dated Sep. 21, 2017 in U.S. Appl. No. 15/380,921. |
| USPTO; Final Office Action dated Jun. 28, 2018 in U.S. Appl. No. 15/380,921. |
| USPTO; Final Office Action dated May 15, 2018 in U.S. Appl. No. 15/388,410. |
| USPTO; Non-Final Office Action dated Aug. 11, 2017 in U.S. Appl. No. 15/397,237. |
| USPTO; Notice of Allowance dated Dec. 22, 2017 in U.S. Appl. No. 15/397,237. |
| USPTO; Non-Final Office Action dated Apr. 12, 2017 in U.S. Appl. No. 15/397,319. |
| USPTO; Final Office Action dated Jul. 12, 2017 in U.S. Appl. No. 15/397,319. |
| USPTO; Notice of Allowance dated Dec. 15, 2017 in U.S. Appl. No. 15/397,319. |
| USPTO; Non-Final Office Action dated Aug. 7, 2018 in U.S. Appl. No. 15/428,808. |
| USPTO; Non-Final Office Action dated Apr. 6, 2018 in U.S. Appl. No. 15/434,051. |
| USPTO; Notice of Allowance dated Oct. 6, 2017 in U.S. Appl. No. 15/450,199. |
| USPTO; Non-Final Office Action dated Dec. 15, 2017 in U.S. Appl. No. 15/466,149. |
| USPTO; Notice of Allowance dated Apr. 20, 2018 in U.S. Appl. No. 15/466,149. |
| USPTO; Non-Final Office Action dated Oct. 4, 2017 in U.S. Appl. No. 15/489,453. |
| USPTO; Final Office Action dated Apr. 19, 2018 in U.S. Appl. No. 15/489,453. |
| USPTO; Notice of Allowance dated Dec. 19, 2017 in U.S. Appl. No. 15/489,660. |
| USPTO; Non-Final Office Action dated Apr. 6, 2018 in U.S. Appl. No. 15/472,750. |
| USPTO; Non-Final Office Action dated Dec. 6, 2017 in U.S. Appl. No. 15/476,035. |
| USPTO; Notice of Allowance dated Mar. 21, 2018 in U.S. Appl. No. 15/476,035. |
| USPTO; Notice of Allowance dated Aug. 14, 2018 in U.S. Appl. No. 15/476,035. |
| USPTO; Non-Final Office Action dated Jan. 16, 2018 in U.S. Appl. No. 15/499,647. |
| USPTO; Notice of Allowance dated May 23, 2018 in U.S. Appl. No. 15/499,647. |
| USPTO; Non-Final Office Action dated Jun. 21, 2018 in U.S. Appl. No. 15/499,647. |
| USPTO; Office Action dated May 3, 2018 in U.S. Appl. No. 15/589,861. |
| USPTO; Requirement of Restriction dated Mar. 30, 2018 in U.S. Appl. No. 15/589,849. |
| USPTO; Office Action dated Aug. 30, 2018 in U.S. Appl. No. 15/589,849. |
| USPTO; Non-Final Office Action dated Apr. 4, 2018 in U.S. Appl. No. 15/592,730. |
| USPTO; Requirement for Restriction dated Aug. 1, 2018 in U.S. Appl. No. 15/627,189. |
| USPTO; Non-Final Office Action dated Jun. 5, 2018 in U.S. Appl. No. 15/650,686. |
| USPTO; Requirement for Restriction dated Apr. 6, 2018 in U.S. Appl. No. 15/659,631. |
| USPTO; Non-Final Office Action dated Aug. 9, 2018 in U.S. Appl. No. 15/660,805. |
| USPTO; Non-Final Office Action dated Jul. 27, 2018 in U.S. Appl. No. 15/673,110. |
| USPTO; Non-Final Office Action dated Apr. 25, 2018 in U.S. Appl. No. 15/673,278. |
| USPTO; Non-Final Office Action dated Jan. 18, 2018 in U.S. Appl. No. 15/683,701. |
| USPTO; Final Office Action dated Aug. 24, 2018 in U.S. Appl. No. 15/683,701. |
| USPTO; Non-Final Office Action dated Aug. 9, 2018 in U.S. Appl. No. 15/691,241. |
| USPTO; Requirement for Restriction dated Jul. 11, 2018 in U.S. Appl. No. 15/707,786. |
| USPTO; Requirement for Restriction dated May 11, 2018 in U.S. Appl. No. 15/711,989. |
| USPTO; Non-Final Office Action dated Jun. 14, 2018 in U.S. Appl. No. 15/711,989. |
| USPTO; Non-Final Office Action dated May 29, 2018 in U.S. Appl. No. 15/719,208. |
| USPTO; Non-Final Office Action dated Apr. 19, 2018 in U.S. Appl. No. 15/726,959. |
| USPTO; Non-Final Office Action dated May 17, 2018 in U.S. Appl. No. 15/729,485. |
| USPTO; Non-Final Office Action dated Jun. 26, 2018 in U.S. Appl. No. 15/796,593. |
| USPTO; Non-Final Office Action dated Dec. 26, 2017 in U.S. Appl. No. 15/798,120. |
| USPTO; Notice of Allowance dated Jun. 13, 2018 in U.S. Appl. No. 15/798,120. |
| USPTO; Requirement for Restriction dated Apr. 6, 2018 in U.S. Appl. No. 15/798,201. |
| USPTO; Non-Final Office Action dated Aug. 9, 2018 in U.S. Appl. No. 15/798,201. |
| USPTO; Non-Final Office Action dated Jul. 2, 2018 in U.S. Appl. No. 15/815,483. |
| USPTO; Requirement for Restriction dated Mar. 21, 2018 in U.S. Appl. No. 15/863,340. |
| USPTO; Non-Final Office Action dated Jul. 23, 2018 in U.S. Appl. No. 15/863,340. |
| USPTO; Notice of Allowance dated May 14, 2012 in U.S. Appl. No. 29/411,637. |
| USPTO; Notice of Allowance dated Oct. 2, 2013 in U.S. Appl. No. 29/412,887. |
| USPTO; Non-Final Office Action dated Mar. 16, 2015 in U.S. Appl. No. 29/447,298. |
| USPTO; Notice of Allowance dated Jul. 6, 2015 in U.S. Appl. No. 29/447,298. |
| USPTO; Notice of Allowance dated Dec. 19, 2013 in U.S. Appl. No. 29/448,094. |
| USPTO; Notice of Allowance dated Nov. 26, 2014 in U.S. Appl. No. 29/481,301. |
| USPTO; Notice of Allowance dated Feb. 17, 2015 in U.S. Appl. No. 29/481,308. |
| USPTO; Requirement for Restriction dated Dec. 1, 2014 in U.S. Appl. No. 29/481,312. |
| USPTO; Notice of Allowance dated Jan. 12, 2015 in U.S. Appl. No. 29/481,312. |
| USPTO; Requirement for Restriction dated Dec. 4, 2014 in U.S. Appl. No. 29/481,315. |
| USPTO; Notice of Allowance dated Apr. 30, 2015 in U.S. Appl. No. 29/481,315. |
| USPTO; Notice of Allowance dated May 11, 2015 in U.S. Appl. No. 29/511,011. |
| USPTO; Notice of Allowance dated May 11, 2015 in U.S. Appl. No. 29/514,153. |
| USPTO; Notice of Allowance dated Dec. 14, 2015 in U.S. Appl. No. 29/514,264. |
| USPTO; Notice of Allowance dated Jun. 16, 2017 in U.S. Appl. No. 29/570,711. |
| USPTO; Notice of Allowance dated Jun. 26, 2018 in U.S. Appl. No. 29/604,288. |
| PCT; International Preliminary Report on Patentability dated Nov. 24, 2009 and International Search Report dated Jul. 31, 2008 in Application No. PCT/US2008/063919. |
| PCT; International Preliminary Report on Patentability dated Feb. 24, 2010 in Application No. PCT/US2008/074063. |
| PCT; International Preliminary Report on Patentability dated Nov. 26, 2009 in Application No. PCT/US2009/043454. |
| PCT; International Preliminary Report on Patentability dated Jun. 14, 2011 in Application No. PCT/US2009/066377. |
| PCT; International Search report and Written Opinion dated Nov. 12, 2010 in Application No. PCT/US2010/030126. |
| PCT; International Preliminary Report on Patentability dated Oct. 11, 2011 Application No. PCT/US2010/030126. |
| PCT; International Preliminary Report on Patentability dated Nov. 9, 2011 in Application No. PCT/US2010/033244. |
| PCT; International Preliminary Report on Patentability dated Nov. 9, 2011 in Application No. PCT/US2010/033248. |
| PCT; International Preliminary Report on Patentability dated Nov. 9, 2011 in Application No. PCT/US2010/033252. |
| PCT; International Search report and Written Opinion dated Jan. 20, 2011 in Application No. PCT/US2010/045368. |
| PCT; International Search report and Written Opinion dated Feb. 6, 2013 in Application No. PCT/US2012/065343. |
| PCT; International Search report and Written Opinion dated Feb. 13, 2013 in Application No. PCT/US2012/065347. |
| PCT; International Search Report and Written Opinion dated Nov. 16, 2017 in Application No. PCT/IB2017/001015. |
| PCT; International Search Report and Written Opinion dated Nov. 13, 2017 in Application No. PCT/IB2017/001050. |
| PCT; International Search Report and Written Opinion dated Nov. 30, 2017 in Application No. PCT/IB2017/001070. |
| PCT; International Search Report and Written Opinion dated Jan. 25, 2018 in Application No. PCT/IB2017/001262. |
| PCT: International Search Report and Written Opinion dated Jun. 1, 2018 in Application No. PCT/IB2017/001644. |
| PCT: International Search Report and Written Opinion dated Jun. 1, 2018 in Application No. PCT/IB2017/001656. |
| Chinese Patent Office; Office Action dated Jan. 10, 2013 in Application No. 201080015699.9. |
| Chinese Patent Office; Office Action dated Aug. 1, 2013 in Application No. 201080015699.9. |
| Chinese Patent Office; Office Action dated Jan. 21, 2014 in Application No. 201080015699.9. |
| Chinese Patent Office; Office Action dated Jul. 24, 2014 in Application No. 201080015699.9. |
| Chinese Patent Office; Office Action dated Jan. 12, 2015 in Application No. 201080015699.9. |
| Chinese Patent Office; Office Action dated Dec. 10, 2013 in Application No. 201080020267.7. |
| Chinese Patent Office; Office Action dated Jan. 21, 2013 in Application No. 201080020268.1. |
| Chinese Patent Office; Office Action dated Sep. 26, 2013 in Application No. 201080020268.1. |
| Chinese Patent Office; Office Action dated Apr. 3, 2014 in Application No. 201080020268.1. |
| Chinese Patent Office; Office Action dated Sep. 23, 2014 in Application No. 201080020268.1. |
| Chinese Patent Office; Office Action dated Apr. 7, 2015 in Application No. 201080020268.1. |
| Chinese Patent Office; Office Action dated May 24, 2013 in Application No. 201080036764.6. |
| Chinese Patent Office; Office Action dated Jan. 2, 2014 in Application No. 201080036764.6. |
| Chinese Patent Office; Office Action dated Jul. 1, 2014 in Application No. 201080036764.6. |
| Chinese Patent Office; Office Action dated Feb. 8, 2014 in Application No. 201110155056. |
| Chinese Patent Office; Office Action dated Sep. 16, 2014 in Application No. 201110155056. |
| Chinese Patent Office; Office Action dated Feb. 9, 2015 in Application No. 201110155056. |
| Chinese Patent Office; Office Action dated Dec. 4, 2015 in Application No. 201210201995.9. |
| Chinese Patent Office; Office Action dated Jul. 14, 2016 in Application No. 201210201995.9. |
| Chinese Patent Office; Office Action dated Jan. 20, 2017 in Application No. 201210201995.9. |
| Chinese Patent Office; Office Action dated Dec. 24, 2015 in Application No. 201280057466.4. |
| Chinese Patent Office; Office Action dated Dec. 4, 2015 in Application No. 201280057542.1. |
| Chinese Patent Office; Office Action dated May 16, 2016 in Application No. 201280057542.1. |
| Chinese Patent Office; Office Action dated Sep. 9, 2016 in Application No. 201280057542.1. |
| Chinese Patent Office; Office Action dated Dec. 5, 2016 in Application No. 201310412808.6. |
| Chinese Patent Office; Office Action dated Feb. 5, 2018 in Application No. 201410331047.6. |
| European Patent Office; Supplementary European Search Report and Opinion dated Nov. 9, 2012 in Application No. 08798519.8. |
| European Patent Office; Office Action dated Jul. 18, 2016 in Application No. 08798519.8. |
| European Patent Office; Extended European Search Report dated Dec. 9, 2016 in Application No. 9767208.3. |
| European Patent Office; Supplementary European Search Report and Opinion dated Jan. 5, 2017 in Application No. 09836647.9. |
| European Patent Office; Office Action dated Feb. 28, 2018 in Application No. 09836647.9. |
| Japanese Patent Office; Office Action dated Dec. 20, 2011 in Application No. 2010-522075. |
| Japanese Patent Office; Office Action dated Apr. 11, 2012 in Application No. 2010-522075. |
| Japanese Patent Office; Office Action dated May 31, 2012 in Application No. 2011-514650. |
| Japanese Patent Office; Office Action dated Sep. 11, 2012 in Application No. 2011-514650. |
| Japanese Patent Office; Office Action dated Dec. 25, 2013 in Application No. 2012-504786. |
| Japanese Patent Office; Office Action dated Jan. 25, 2014 in Application No. 2012-504786. |
| Japanese Patent Office; Office Action dated Dec. 1, 2014 in Application No. 2012-504786. |
| Japanese Patent Office; Office Action dated Mar. 11, 2013 in Application No. 2012-509857. |
| Korean Patent Office; Office Action dated Dec. 10, 2015 in Application No. 10-2010-0028336. |
| Korean Patent Office; Final Office Action dated Jun. 29, 2016 in Application No. 10-2010-0028336. |
| Korean Patent Office; Office Action dated Mar. 3, 2016 in Application No. 10-2010-0067768. |
| Korean Patent Office; Office Action dated Aug. 1, 2016 in Application No. 10-2010-0067768. |
| Korean Patent Office; Office Action dated May 2, 2016 in Application No. 10-2010-0082446. |
| Korean Patent Office; Office Action dated Sep. 19, 2016 in Application No. 10-2010-0082446. |
| Korean Patent Office; Office Action dated Nov. 24, 2017 in Application No. 10-20110036449. |
| Korean Patent Office; Office Action dated May 23, 2017 in Application No. 10-20110036449. |
| Korean Patent Office; Office Action dated Sep. 4, 2017 in Application No. 10-2011-0087600. |
| Korean Patent Office; Office Action dated Oct. 23, 2017 in Application No. 10-2011-0142924. |
| Korean Patent Office; Office Action dated Dec. 11, 2015 in Application No. 10-20117023416. |
| Korean Patent Office; Office Action dated Mar. 13, 2016 in Application No. 10-20117023416. |
| Korean Patent Office; Office Action dated Oct. 30, 2017 in Application No. 10-2012-0041878. |
| Korean Patent Office; Office Action dated Mar. 21, 2018 in Application No. 20120042518. |
| Korean Patent Office; Office Action dated Mar. 21, 2018 in Application No. 10-2012-0064526. |
| Korean Patent Office; Office Action dated Mar. 30, 2018 in Application No. 10-2012-0076564. |
| Korean Patent Office; Office Action dated Apr. 30, 2018 in Application No. 10-2012-0103114. |
| Korean Patent Office; Office Action dated Oct. 24, 2016 in Application No. 10-20127004062. |
| Korean Patent Office; Office Action dated Jul. 24, 2017 in Application No. 10-20127004062. |
| Korean Patent Office; Office Action dated Sep. 28, 2017 in Application No. 10-20147017112. |
| Korean Patent Office; Office Action dated Nov. 9, 2016 in Application No. 10-20167023913. |
| Korean Patent Office; Office Action dated Sep. 15, 2017 in Application No. 30-2017-0001320. |
| Korean Patent Office; Office Action dated Jul. 11, 2018 in Application No. 30-2018-006016. |
| Taiwanese Patent Office; Office Action dated Aug. 30, 2013 in Application No. 97132391. |
| Taiwanese Patent Office; Office Action dated Dec. 20, 2013 in Application No. 98117513. |
| Taiwan Patent Office; Office Action dated Jul. 4, 2014 in Application No. 099110511. |
| Taiwanese Patent Office; Office Action dated Aug. 27, 2014 in Application No. 99114329. |
| Taiwanese Patent Office; Office Action dated Dec. 26, 2014 in Application No. 99114330. |
| Taiwanese Patent Office; Office Action dated Aug. 14, 2014 in Application No. 99114331. |
| Taiwan Patent Office; Office Action dated Dec. 19, 2014 in Taiwan Application No. 099127063. |
| Taiwanese Patent Office; Office Action received in Application No. 100113130. |
| Taiwan Patent Office; Office Action dated May 13, 2016 in Taiwan Application No. 101142582. |
| Taiwanese Patent Office; Office Action dated Aug. 1, 2016 in Application No. 101124745. |
| Taiwanese Patent Office; Office Action received in Application No. 102113028. |
| Taiwanese Patent Office; Office Action received in Application No. 102115605. |
| Taiwanese Patent Office; Office Action dated Feb. 24, 2017 in Application No. 102115605. |
| Taiwanese Patent Office; Office Action received in Application No. 102125191. |
| Taiwanese Patent Office; Office Action dated Dec. 6, 2016 in Application No. 102126071. |
| Taiwanese Patent Office; Office Action dated May 17, 2018 in Application No. 102126071. |
| Taiwanese Patent Office; Office Action dated Feb. 10, 2017 in Application No. 102127065. |
| Taiwanese Patent Office; Office Action dated Mar. 11, 2016 in Application No. 102129262. |
| Taiwanese Patent Office; Office Action dated Dec. 29, 2016 in Application No. 102129397. |
| Taiwanese Patent Office; Office Action dated Nov. 4, 2016 in Application No. 102131839. |
| Taiwanese Patent Office; Office Action dated Dec. 2, 2016 in Application No. 102136496. |
| Taiwanese Patent Office; Office Action dated Jan. 10, 2018 in Application No. 102136496. |
| Taiwanese Patent Office; Office Action dated Nov. 11, 2016 in Application No. 102132952. |
| Taiwanese Patent Office; Office Action dated Jul. 17, 2017 in Application No. 103101400. |
| Taiwanese Patent Office; Office Action dated Feb. 23, 2017 in Application No. 103102563. |
| Taiwanese Patent Office; Office Action dated Mar. 3, 2017 in Application No. 103105251. |
| Taiwanese Patent Office; Office Action received in Application No. 103106021. |
| Taiwanese Patent Office; Office Action dated Oct. 31, 2017 in Application No. 103106022. |
| Taiwanese Patent Office; Office Action dated Jul. 5, 2017 in Application No. 103117477. |
| Taiwanese Patent Office; Office Action dated Nov. 22, 2017 in Application No. 103117478. |
| Taiwanese Patent Office; Office Action dated May 19, 2017 in Application No. 103120478. |
| Taiwanese Patent Office; Office Action dated Nov. 8, 2017 in Application No. 103124509. |
| Taiwanese Patent Office; Office Action dated Nov. 20, 2017 in Application No. 103127588. |
| Taiwanese Patent Office; Office Action dated Sep. 19, 2017 in Application No. 103127734. |
| Taiwanese Patent Office; Office Action dated Nov. 22, 2017 in Application No. 103134537. |
| Taiwanese Patent Office; Office Action dated Aug. 24, 2017 in Application No. 103136251. |
| Taiwanese Patent Office; Office Action dated Feb. 26, 2018 in Application No. 103138510. |
| Taiwanese Patent Office; Office Action dated May 21, 2018 in Application No. 103139014. |
| Taiwanese Patent Office; Office Action dated Jun. 22, 2018 in Application No. 104105533. |
| Taiwanese Patent Office; Office Action dated Jun. 13, 2018 in Application No. 104111910. |
| Taiwanese Patent Office; Office Action received in Application No. 106117181. |
| Bearzotti, et al., “Fast Humidity Response of a Metal Halide-Doped Novel Polymer,” Sensors and Actuators B, 7, pp. 451-454, (1992). |
| Becker et al., “Atomic Layer Deposition of Insulating Hafnium and Zirconium Nitrides,” Chem. Mater., 16, 3497-3501 (2004). |
| Bhatnagar et al., “Copper Interconnect Advances to Meet Moore's Law Milestones,” Solid State Technology, 52, 10 (2009). |
| Buriak, “Organometallic Chemistry on Silicon and Germanium Surfaces,” Chemical Reviews, 102, 5 (2002). |
| Cant et al., “Chemisorption Sites on Porous Silica Glass and on Mixed-Oxide Catalysis,” Can. J. Chem. 46, 1373 (1968). |
| Chang et al. “Small-Subthreshold-Swing and Low-Voltage Flexible Organic Thin-Film Transistors Which Use HfLaO as the Gate Dielectric,” IEEE Electron Device Letters, Feb. 2009, pp. 133-135; vol. 30, No. 2; IEEE Electron Device Society. |
| Chatterjee et al., “Sub-100nm Gate Length Metal Gate NMOS Transistors Fabricated by a Replacement by a Replacement Gate Process,” IEEE Semiconductor Process and Device Center, 821-824 (1997). |
| Chen et al., “A Self-Aligned Airgap Interconnect Scheme,” IEEE International Interconnect Technology Conference, vol. 1-3, 146-148 (2009). |
| Choi et al., “Improvement of Silicon Direct Bonding using Surfaces Activated by Hydrogen Plasma Treatment,” Journal of the Korean Physical Society, 37, 6, 878-881 (2000). |
| Choi et al., “Low Temperature Formation of Silicon Oxide Thin Films by Atomic Layer Deposition Using NH3/O2 Plasma,” ECS Solid State Letters, 2(12) p. 114-p. 116 (2013). |
| Coates, “Process Analytical Technology: Spectroscopic Tools and Implementation Strategies for the Chemical and Pharmaceutical Industries.” Blackwell Publishing Ltd, 91-132, (2005). |
| Crowell, “Chemical methods of thin film deposition: Chemical vapor deposition, atomic layer deposition, and related technologies,” Journal of Vacuum Science & Technology A 21.5, (2003): S88-S95. |
| Cui et al., “Impact of Reductive N2/H2 Plasma on Porous Low-Dielectric Constant SiCOH Thin Films,” Journal of Applied Physics 97, 113302, 1-8 (2005). |
| Dingemans et al., “Comparison Between Aluminum Oxide Surface Passivation Films Deposited with Thermal Aid,” Plasma Aid and Pecvd, 35th IEEE PVCS, Jun. 2010. |
| Drummond et al., “Hydrophobic Radiofrequency Plasma-Deposited Polymer Films: Dielectric Properties and Surface Forces,” Colloids and Surfaces A, 129-130, 117-129 (2006). |
| Easley et al., “Thermal Isolation of Microchip Reaction Chambers for Rapid Non-Contact DNA Amplification,” J. Micromech. Microeng. 17, 1758-1766 (2007). |
| Elam et al., “New Insights into Sequential Infiltration Synthesis”, ECS Transactions, vol. 69, pp. 147-157 (2015). |
| Ge et al., “Carbon Nanotube-Based Synthetic Gecko Tapes,” Department of Polymer Science, PNAS, 10792-10795 (2007). |
| George et al., “Atomic Layer Deposition: An Overview,” Chem. Rev. 110, 111-131 (2010). |
| Grill et al., “The Effect of Plasma Chemistry on the Damage Induced Porous SiCOH Dielectrics,” IBM Research Division, RC23683 (W0508-008), Materials Science, 1-19 (2005). |
| Guan et al., “Voltage gated ion and molecule transport in engineered nanochannels: theory, fabrication and applications,” Nanotechnology 25 (2014) 122001. |
| Gupta et al., “Conversion of Metal Carbides to Carbide Derived Carbon by Reactive Ion Etching in Halogen Gas,” Proceedings of SPIE—The International Society for Optical Engineering and Nanotechnologies for Space Applications, ISSN: 0277-786X (2006). |
| Harrison et al., “Poly-gate Replacement Through Contact Hole (PRETCH): A New Method for High-K/ Metal Gate and Multi-Oxide Implementation on Chip,” IEEE (2004). |
| Heo et al., “Structural Characterization of Nanoporous Low-Dielectric Constant SiCOH Films Using Organosilane Precursors,” NSTI-Nanotech, vol. 4, 122-123 (2007). |
| Henke et al.., “X-Ray Interactions: Photo absorption, Scattering, Transmission, and Reflection at E=50-30,000 eV, Z=1-92,” Atomic Data and Nuclear Data Tables, 54, 181-342 (1993). |
| H.J. Yun et al., “Comparison of Atomic Scale Etching of Poly-Si in Inductively Coupled Ar and He Plasmas”, Korean Journal of Chemical Engineering, vol. 24, 670-673 (2007). |
| Hubert et al., “A Stacked SONOS Technology, up to 4 Levels and 6nm Crystalline Nanowires, With Gate-All-Around or Independent Gates (-Flash), Suitable for Full 3D Integration,” Minatec, IEDM09-637-640 (2009). |
| Hudis, “Surface Crosslinking of Polyethylene Using a Hydrogen Glow Discharge,” J. Appl. Polym. Sci., 16 (1972) 2397. |
| Jones et al., “Growth of Aluminum Films by Low Pressure Chemical Vapour Deposition Using Tritertiarybutylaluminium,” Journal of Crystal Growth 135, pp. 285-289, Elsevier Science B.V. (1994). |
| Jones et al., “Recent Developments in Metalorganic Precursors for Metalorganic Chemical Vapour Deposition,” Journal of Crystal Growth 146, pp. 503-510, Elsevier Science B.V. (1995). |
| Jung et al., “Double Patterning of Contact Array with Carbon Polymer,” Proc. of SPIE, 6924, 69240C, 1-10 (2008). |
| Katamreddy et al., “ALD and Characterization of Aluminum Oxide Deposited on Si(100) using Tris(diethylamino) Aluminum and Water Vapor,” Journal of the Electrochemical Society, 153 (10) C701-C706 (2006). |
| Kim et al., “Passivation Effect on Low-k S/OC Dielectrics by H2 Plasma Treatment,” Journal of the Korean Physical Society, 40, 1, 94-98 (2002). |
| Kim et al., “Characteristics of Low Temperature High Quality Silicon Oxide by Plasma Enhanced Atomic Layer Deposition with In-Situ Plasma Densification Process,” The Electrochemical Society, ECS Transactions, College of Information and Communication Engineering, Sungkyunkwan University, 53(1), 321-329 (2013). |
| King, Plasma Enhanced Atomic Layer Deposition of SiNx: H and SiO2, J. Vac. Sci. Technol., A29(4) (2011). |
| Klug et al., “Atomic Layer Deposition of Amorphous Niobium Carbide-Based Thin Film Superconductors,” The Journal of Physical Chemistry C, vol. 115, pp. 25063-25071, (2011). |
| Kobayshi, et al., “Temperature Dependence of SiO2 Film Growth with Plasma-Enhanced Atomic Layer Deposition,” regarding Thin Solid Films, published by Elsevier in the International Journal on the Science and Technology of Condensed Matter, in vol. 520, No. 11, 3994-3998 (2012). |
| Koo et al., “Characteristics of Al2O3 Thin Films Deposited Using Dimethylaluminum Isopropoxide and Trimethylaluminum Precursors by the Plasma-Enhanced Atomic-Layer Deposition Method,” Journal of Physical Society, 48, 1, 131-136 (2006). |
| Koutsokeras et al. “Texture and Microstructure Evolution in Single-Phase TixTa1—xN Alloys of Rocksalt Structure,” Journal of Applied Physics, 110, pp. 043535-1-043535-6, (2011). |
| Knoops et al., “Atomic Layer Deposition of Silicon Nitride from Bis(tert-butyloamino) silane and N2 Plasma,” Applied Materials & Interfaces, American Chemical Society, A-E (2015). |
| Krenek et al. “IR Laser CVD of Nanodisperse Ge—Si—Sn Alloys Obtained by Dielectric Breakdown of GeH4/SiH4/SnH4 Mixtures”, NanoCon 2014, Nov. 5-7, Brno, Czech Republic, EU. |
| Kurosawa et al., “Synthesis and Characterization of Plasma-Polymerized Hexamethyldisiloxane Films,” Thin Solid Films, 506-507, 176-179 (2006). |
| Lanford et al., “The Hydrogen Content of Plasmadeposited Silicon Nitride,” J. Appl. Phys., 49, 2473 (1978). |
| Lee et al., Layer Selection by Multi-Level Permutation in 3-D Stacked NAND Flash Memory, IEEE Electron Device Letters, vol. 37, No. 7, 866-869 (2016). |
| Lieberman, et al., “Principles of Plasma Discharges and Materials Processing,” Second Edition, 368-381. |
| Lim et al., “Low-Temperature Growth of SiO2 Films by Plasma-Enhanced Atomic Layer Deposition,” ETRI Journal, 27 (1), 118-121 (2005). |
| Liu et al., “Research, Design, and Experiment of End Effector for Wafer Transfer Robot,” Industrial Robot: An International Journal, 79-91 (2012). |
| Longrie et al., “Plasma-Enhanced ALD of Platinum with O2, N2 and NH3 Plasmas”, ECS Journal of Solid State Science and Technology, vol. 1, pp. Q123-Q129 (2012). |
| Mackus et al., “Optical Emission Spectroscopy as a Tool for Studying Optimizing and Monitoring Plasma-Assisted Atomic Layer Deposition Processes,” Journal of Vacuum Science and Technology, 77-87 (2010). |
| Maeno, “Gecko Tape Using Carbon Nanotubes,” Nitto Denko Gihou, 47, 48-51. |
| Maeng et al. Electrical properties of atomic layer disposition Hf02 and Hf0xNy on Si substrates with various crystal orientations, Journal of the Electrochemical Society, Apr. 2008, p. H267-H271, vol. 155, No. 4, Department of Materials Science and Engineering, Pohang University of Science and Technology, Pohang, Korea. |
| Marsik et al., “Effect of Ultraviolet Curing Wavelength on Low-k Dielectric Material Properties and Plasma Damage Resistance,” Sciencedirect.com, 519, 11, 3619-3626 (2011). |
| Mason et al., “Hydrolysis of Tri-tert-butylaluminum: The First Structural Characterization of Alkylalumoxanes [(R2Al)2O]n and (RAIO)n,” J. American Chemical Society, vol. 115, No. 12, pp. 4971-4984 (1993). |
| Massachusetts Institute of Technology Lincoln Laboratory, “Solid State Research,” Quarterly Technical Report (1995). |
| Maydannik et al., “Spatial atomic layer deposition: Performance of low temperature H2O and 03oxidant chemistry for flexible electronics encapsulation”, Journal of Vacuum Science and Technology: Part A AVS/ AIP, vol. 33 (1901). |
| Meng et al., “Atomic Layer of Deposition of Silicon Nitride Thin Films: A Review of Recent Progress, Challenges, and Outlooks,” Materials, 9, 1007 (2016). |
| Mix et al., “Characterization of plasma-polymerized allyl alcohol polymers and copolymers with styrene,” Adhes. Sci. Technol., 21 (2007), S. 487-507. |
| Moeen, “Design, Modelling and Characterization of Si/SiGe Structures for IR Bolometer Applications,” KTH Royal Institute of Technology. Information and Communication Technology, Department of Integrated Devices and Circuits, Stockholm Sweden (2015). |
| Morishige et al., “Thermal Desorption and Infrared Studies of Ammonia Amines and Pyridines Chemisorbed on Chromic Oxide,” J. Chem. Soc., Faraday Trans. 1, 78, 2947-2957 (1982). |
| Mosleh et al., “Enhancement of Material Quality of (Si)GeSn Films Grown by SnC14 Precursor,” ECS Transactions, 69 (5), 279-285 (2015). |
| Mukai et al., “A Study of CD Budget in Spacer Patterning Technology,” Proc. of SPIE, 6924, 1-8 (2008). |
| Nigamananda et al., “Low-Temperature (<200oC) Plasma Enhanced Atomic Deposition of Dense Titanium Nitride Thin Films.” |
| Nogueira et al., “Production of Highly Hydrophobic Films Using Low Frequency and High Density Plasma,” Revista Brasileira de Aplicacoes de Vacuo, 25(1), 45-53 (2006). |
| Novaro et al. Theoretical Study on a Reaction Pathway of Ziegler-Natta-Type Catalysis, J. Chem. Phys. 68(5), Mar. 1, 1978 p. 2337-2351. |
| S. Okamoto et al., “Luminescent Properties of Pr3+-sensitized LaPO4: Gd3+ Ultraviolet-B Phosphor Under Vacuum-Ultraviolet Light Excitation,” J. App. Phys. 106, 013522 (2009). |
| Park “Substituted Aluminum Metal Gate on High-K Dielectric for Low Work-Function and Fermi-Level Pinning Free,” 4 pages, IEEE 0-7803-8684-1/04 (2004). |
| Portet et al., “Impact of Synthesis Conditions on Surface Chemistry and Structure of Carbide-Derived Carbons,” Thermochimica Acta, 497, 137-142 (2010). |
| Potts et al., “Low Temperature Plasma-Enhanced Atomic Layer Deposition of metal Oxide Thin Films,” Journal of the Electrochemical Society, 157, 66-74 (2010). |
| Potts et al., “Room-Temperature ALD of Metal Oxide Thin Films by Energy-Enhanced ALD”, Chemical Vapor Deposition, vol. 19, pp. 125-133 (2013). |
| Presser, et al., “Effect of Pore Size on Carbon Dioxide Sorption by Carbide Derived Carbon,” Energy & Environmental Science 4.8, 3059-3066 (2011). |
| Provine et al., “Correlation of Film Density and Wet Etch Rate in Hydrofluoric Acid of Plasma Enhanced Atomic Layer Deposited Silicon Nitride,” AIP Advances, 6 (2016). |
| Radamson et al. “Growth of Sn-alloyed Group IV Materials for Photonic and Electronic Applications”, Chapter 5 pp. 129-144, Manufacturing Nano Structures. |
| Sakuma et al., “Highly Scalable Horizontal Channel 3-D NAND Memory Excellent in Compatibility with Conventional Fabrication Technology,” IEEE Electron Device Letters, vol. 34, No. 9, 1142-1144 (2013). |
| Salim, “In-situ Fourier Transform Infrared Spectroscopy of Chemistry and Growth in Chemical Vapor Deposition,” Massachusetts Institute of Technology, 187 pages (1995). |
| Salim et al., “In Situ Concentration Monitoring in a Vertical OMVPE Reactor by Fiber-Optics-Based Fourier Transform Infrared Spectroscopy,” Journal of Crystal Growth 169, pp. 443-449, Elsevier Science B.V. (1996). |
| Schmatz et al., “Unusual Isomerization Reactions in 1.3-Diaza-2-Silcyclopentanes,” Organometallics, 23, 1180-1182 (2004). |
| Scientific and Technical Information Center EIC 2800 Search Report dated Feb. 16, 2012. |
| Selvaraj et al., “Selective Atomic Layer Deposition of Zirconia on Copper Patterned Silicon Substrates Using Ethanol as Oxygen Source as Well as Copper Reductant,” J. Vac. Sci. Technol. A32(1), (2014). |
| Selvaraj et al., “Surface Selective Atomic Layer Deposition of Hafnium Oxide for Copper Diffusion Barrier Application Using Tetrakis (diethylamino) Hafnium and Ethanol,” 225th ECS Meeting, Meeting Abstract, (May 12, 2014). |
| S.D. Athavale and D.J. Economou, “Realization of Atomic Layer Etching of Silicon”, Journal of Vacuum Science and Technology B, vol. 14, year 1996, pp. 3702-3705. |
| Sham Ma et al., “PDL Oxide Enabled Doubling,” Proc. of SPIE, 6924, 69240D, 1-10 (2008). |
| Tseng et al., “Etch Properties of Resists Modified by Sequential Infiltration Synthesis,” American Vacuum Society (2011). |
| Tseng et al., “Enhanced Block Copolymer Lithography Using Sequntial Infiltration Synthesis,” Journal of Physical Chemistry, vol. 5, 17725-17729 (2011). |
| Varma, et al., “Effect of Metal Halides on Thermal, Mechanical, and Electrical Properties of Polypyromelitimide Films,” Journal of Applied Polymer Science, vol. 32, pp. 3987-4000, (1986). |
| Voltaix, “Meterial Safety Data Sheet for: Trisilylamine”, pp. 1-8, (2014). |
| Wang et al., “Tritertiarybutylaluminum as an Organometallic Source for Epitaxial Growth of AlGaSb,” Appl. Phys. Lett. 67 (10), Sep. 4, pp. 1384-1386, American Institute of Physics (1995). |
| Wirths, et al, “SiGeSn Growth tudies Using Reduced Pressure Chemical Vapor Deposition Towards Optoeleconic Applications,” This Soid Films, 557, 183-187 (2014). |
| Yoshida, et al., Threshold Voltage Tuning for 10NM and Beyond CMOS Integration, Solid State Technology, 57(7): 23-25 (2014). |
| Yu et al., “Modulation of the Ni FUSI Workfunction by Yb Doping: from Midgap to N-Type Band-Edge,” 4 pages, IEEE 0-7803-9269-8/05 (2005). |
| Yun et al., “Behavior of Various Organosilicon Molecules in PECVD Processes for Hydrocarbon-Doped Silicon Oxide Films,” Solid State Phenomena, vol. 124-126, 347-350 (2007). |
| Yun et al., “Single-Crystalline Si Stacked Array (STAR) NAND Flash Memory,” IEEE Transactions on Electron Devices, vol. 58, No. 4, 1006-1014 (2011). |
| Yun et al., “Effect of Plasma on Characteristics of Zirconium Oxide Films Deposited by Plasma-Enhanced Atomic Layer Deposition,” Electrochemical and Solid State Letters, 8(11) F47-F50 (2005). |
| Yushin et al., “Carbon-Derived Carbon,” Department of Materials Science and Engineering, Taylor & Francis Group, LLC (2006). |
| Chemistry Stack Exchange, “Why is CF4 Non-Polar and CHF Polar,” https://chemistry.stackexchange.com/questions/31604/why-is-cf4-non-polar-and-chf3-polar, (2015). |
| EPO; Extended European Search Report dated Apr. 28, 2014 in Application No. 11162225.4. |
| EPO; Notice of Allowance dated Feb. 3, 2015 in Application No. 11162225.4. |
| IPOS; Notice of Allowance dated Aug. 14, 2017 in Application No. 10201401237. |
| JPO; Office Action dated Mar. 27, 2012 in Application No. 2009-532567. |
| JPO; Notice of Allowance dated Jul. 31, 2012 in Application No. 2009-532567. |
| JPO; Office Action dated May 9, 2013 in Application No. 2010058415. |
| JPO; Office Action dated Nov. 5, 2013 in Application No. 2010058415. |
| JPO; Office Action dated Aug. 29, 2014 in Application No. 2010058415. |
| JPO; Notice of Allowance dated Dec. 24, 2014 in Application No. 2010058415. |
| JPO; Office Action dated Aug. 26, 2013 in Application No. 2010-153754. |
| JPO; Office Action dated Nov. 5, 2013 in Application No. 2010-193285. |
| JPO; Notice of Allowance dated Apr. 2, 2013 in Application No. 2010-509478. |
| JPO; Office Action dated Aug. 31, 2015 in Application No. 2011-284831. |
| JPO; Notice of Allowance dated Mar. 9, 2016 in Application No. 2011-284831. |
| JPO; Notice of Allowance dated Dec. 21, 2012 in Application No. 2011-514650. |
| JPO; Office Action dated Dec. 15, 2014 in Application No. 2011090067. |
| JPO; Notice of Allowance dated May 1, 2015 in Application No. 2011090067. |
| JPO; Office Action dated Jul. 19, 2016 in Application No. 2012-153698. |
| JPO; Notice of Allowance dated Oct. 26, 2016 in Application No. 2012-153698. |
| JPO; Notice of Allowance dated Jun. 12, 2015 in Application No. 2012-504786. |
| JPO; Notice of Allowance dated Jul. 2, 2013 in Application No. 2012-509857. |
| JPO; Office Action dated May 31, 2017 in Application No. 2013-160173. |
| JPO; Notice of Allowance dated Aug. 25, 2017 in Application No. 2013-160173. |
| JPO; Office Action dated Jun. 15, 2017 in Application No. 2013-178344. |
| JPO; Office Action dated Jan. 29, 2018 in Application No. 2013-178344. |
| JPO; Notice of Allowance dated Aug. 21, 2018 in Application No. 2013-178344. |
| JPO; Office Action dated Apr. 10, 2018 in Application No. 2014-120675. |
| JPO; Notice of Allowance dated Jun. 12, 2018 in Application No. 2014-120675. |
| JPO; Office Action dated Apr. 3, 2018 in Application No. 2014-188835. |
| JPO; Notice of Allowance dated Jun. 12, 2018 in Application No. 2014-188835. |
| JPO; Office Action dated May 8, 2018 in Application No. 2014-205548. |
| JPO; Notice of Allowance dated May 22, 2018 in Application No. 2014-216540. |
| JPO; Office Action dated Jul. 31, 2018 in Application No. 2015-034774. |
| KIPO; Notice of Allowance dated Sep. 29, 2016 in Application No. 10-2010-0028336. |
| KIPO; Notice of Allowance dated Dec. 1, 2016 in Application No. 10-2010-0067768. |
| KIPO; Notice of Allowance dated Mar. 7, 2017 in Application No. 10-2010-0082446. |
| KIPO; Office Action dated Mar. 13, 2017 in Application No. 20110034612. |
| KIPO; Office Action dated Jul. 20, 2017 in Application No. 20110034612. |
| KIPO; Notice of Allowance dated Sep. 1, 2017 in Application No. 20110034612. |
| KIPO; Notice of Allowance dated Oct. 24, 2018 in Application No. 10-2011-0036449. |
| KIPO; Notice of Allowance dated Jan. 11, 2018 in Application No. 10-2011-0087600. |
| KIPO; Notice of Allowance dated Mar. 14, 2018 in Application No. 10-2011-0142924. |
| KIPO; Notice of Allowance dated Jun. 2, 0216 in Application No. 10-2011-7023416. |
| KIPO; Notice of Allowance dated Feb. 28, 2018 in Application No. 10-2012-0041878. |
| KIPO; Notice of Allowance dated May 30, 2018 in Application No. 10-2012-0042518. |
| KIPO; Office Action dated Dec. 13, 2018 in Application No. 10-2012-0064526. |
| KIPO; Notice of Allowance dated Nov. 22, 2018 in Application No. 10-2012-0103114. |
| KIPO; Notice of Allowance dated Feb. 23, 2018 in Application No. 10-2014-7017112. |
| KIPO; Notice of Allowance dated May 30, 2017 in Application No. 10-2016-7023913. |
| KIPO; Notice of Allowance dated Feb. 27, 2018 in Application No. 10-2017-0175442. |
| KIPO; Notice of Allowance dated Jul. 19, 2018 in Application No. 20187013945. |
| KIPO; Notice of Allowance dated Jan. 19, 2018 in Application No. 30-2017-0001320. |
| KIPO; Notice of Allowance dated Jul. 1, 2018 in Application No. 30-2017-0052872. |
| KIPO; Notice of Allowance dated Oct. 16, 2018 in Application No. 30-2018-0006016. |
| SIPO; Notice of Allowance dated May 8, 2015 in Application No. 201080015699.9. |
| SIPO; Notice of Allowance dated Aug. 22, 2014 in Application No. 201080020267.7. |
| SIPO; Notice of Allowance dated Oct. 16, 2015 in Application No. 201080020268.1. |
| SIPO; Notice of Allowance dated Oct. 24, 2014 in Application No. 201080036764.6. |
| SIPO; Notice of Allowance dated Aug. 26, 2015 in Application No. 201110155056. |
| SIPO; Notice of Allowance dated Apr. 13, 2017 in Application No. 201210201995.9. |
| SIPO; Notice of Allowance dated Jun. 16, 2016 in Application No. 201280057466.4. |
| SIPO; Notice of Allowance dated Jan. 3, 2017 in Application No. 201280057542.1. |
| SIPO; Notice of Allowance dated Jul. 20, 2017 in Application No. 201310412808.6. |
| SIPO; Notice of Allowance dated May 25, 2017 in Application No. 201730010308.9. |
| SIPO; Notice of Allowance dated Oct. 24, 2018 in Application No. 201830060972.9. |
| TIPO; Notice of Allowance dated Jun. 12, 2014 in Application No. 98117513. |
| TIPO; Notice of Allowance dated Feb. 24, 2016 in Application No. 99110511. |
| TIPO; Notice of Allowance dated Apr. 28, 2015 in Application No. 99114330. |
| TIPO; Notice of Allowance dated Oct. 16, 2015 in Application No. 99114331. |
| TIPO; Notice of Allowance dated Mar. 14, 2016 in Application No. 99127063. |
| TIPO; Notice of Allowance dated Jun. 29, 2016 in Applicaton No. 100113130. |
| TIPO; Notice of Allowance dated Oct. 14, 2015 in Application No. 100130472. |
| TIPO; Notice of Allowance dated Oct. 19, 2016 in Application No. 101124745. |
| TIPO; Notice of Allowance dated Nov. 2, 2016 in Application No. 101142581. |
| TIPO; Notice of Allowance dated Sep. 9, 2016 in Application No. 101142582. |
| TIPO; Notice of Allowance dated Feb. 13, 2017 in Application No. 102113028. |
| TIPO; Notice of Allowance dated Dec. 26, 2017 in Application No. 102115605. |
| TIPO; Notice of Allowance dated May 3, 2017 in Application No. 102129262. |
| TIPO; Notice of Allowance dated Aug. 24, 2018 in Application No. 102126071. |
| TIPO; Notice of Allowance dated Jul. 18, 2017 in Application No. 102127065. |
| TIPO; Notice of Allowance dated Aug. 29, 2017 in Application No. 102129397. |
| TIPO; Notice of Allowance dated Jan. 26, 2017 in Application No. 102131839. |
| TIPO; Notice of Allowance dated Apr. 19, 2017 in Application No. 102132952. |
| TIPO; Notice of Allowance dated Jan. 24, 2018 in Application No. 103101400. |
| TIPO; Notice of Allowance dated Nov. 30, 2017 in Application No. 103102563. |
| TIPO; Notice of Allowance dated Oct. 20, 2017 in Application No. 103105251. |
| TIPO; Notice of Allowance dated Apr. 10, 2018 in Application No. 103106021. |
| TIPO; Notice of Allowance dated Apr. 10, 2018 in Application No. 103106022. |
| TIPO; Notice of Allowance dated Jan. 22, 2018 in Application No. 103117477. |
| TIPO; Notice of Allowance dated Mar. 13, 2018 in Application No. 103117478. |
| TIPO; Notice of Allowance dated Sep. 25, 2017 in Application No. 103120478. |
| TIPO; Office Action dated Sep. 20, 2018 in Application No. 103123439. |
| TIPO; Office Action dated Apr. 25, 2018 in Application No. 103124509. |
| TIPO; Notice of Allowance dated Jun. 19, 2018 in Application No. 103127588. |
| TIPO; Notice of Allowance dated Dec. 11, 2017 in Application No. 103127734. |
| TIPO; Notice of Allowance dated Apr. 19, 2018 in Application No. 103134537. |
| TIPO; Notice of Allowance dated Oct. 17, 2017 in Application No. 103136251. |
| TIPO; Notice of Allowance dated Jun. 13, 2018 in Application No. 103138510. |
| TIPO; Notice of Allowance dated Sep. 11, 2018 in Application No. 103139014. |
| TIPO; Notice of Allowance dated Sep. 18, 2018 in Application No. 104111910. |
| TIPO; Notice of Allowance dated Dec. 5, 2017 in Application No. 105308015. |
| TIPO; Notice of Allowance dated Jun. 5, 2018 in Application No. 106117181. |
| TIPO; Office Action dated Sep. 28, 2018 in Application No. 106119537. |
| TIPO; Office Action dated Aug. 31, 2018 in Application No. 106138119. |
| TIPO; Office Action dated Oct. 3, 2018 in Application No. 106142731. |
| TIPO; Office Action dated Sep. 28, 2018 in Application No. 107112951. |
| TIPO; Notice of Allowance dated Aug. 29, 2018 in Application No. 107300633. |
| TIPO; Notice of Allowance dated Apr. 11, 2018 in Application No. 105308015D01. |
| USPTO; Non-Final Office Action dated Feb. 15, 2012 in U.S. Appl. No. 13/085,531. |
| USPTO; Notice of Allowance dated Jul. 12, 2012 in U.S. Appl. No. 13/085,531. |
| USPTO; Final Office Action dated Nov. 2, 2018 in U.S. Appl. No. 13/169,951. |
| USPTO; Final Office Action dated Nov. 1, 2018 in U.S. Appl. No. 14/219,839. |
| USPTO; Final Office Action dated Nov. 2, 2018 in U.S. Appl. No. 14/219,879. |
| USPTO; Final Office Action dated Nov. 28, 2018 in U.S. Appl. No. 14/508,489. |
| USPTO; Notice of Allowance dated Nov. 19, 2018 in U.S. Appl. No. 14/656,588. |
| USPTO; Notice of Allowance dated Nov. 19, 2018 in U.S. Appl. No. 14/919,536. |
| USPTO; Final Office Action dated Dec. 10, 2018 in U.S. Appl. No. 14/997,683. |
| USPTO; Final Office Action dated Oct. 19, 2018 in U.S. Appl. No. 15/060,412. |
| USPTO; Non-Final Office Action dated Sep. 26, 2018 in U.S. Appl. No. 15/074,813. |
| USPTO; Non-Final Office Action dated Nov. 23, 2018 in U.S. Appl. No. 15/135,258. |
| USPTO; Non-Final Office Action dated Oct. 9, 2018 in U.S. Appl. No. 15/182,504. |
| USPTO; Final Office Action dated Oct. 9, 2018 in U.S. Appl. No. 15/205,827. |
| USPTO; Non-Final Office Action dated Nov. 14, 2018 in U.S. Appl. No. 15/377,439. |
| USPTO; Notice of Allowance dated Nov. 14, 2018 in U.S. Appl. No. 15/388,410. |
| USPTO; Notice of Allowance dated Dec. 28, 2018 in U.S. Appl. No. 15/388,410. |
| USPTO; Restriction Requirement dated Dec. 5, 2018 in U.S. Appl. No. 15/402,993. |
| USPTO; Advisory Action dated Dec. 4, 2018 in U.S. Appl. No. 15/434,051. |
| USPTO; Notice of Allowance dated Nov. 30, 2018 in U.S. Appl. No. 15/472,750. |
| USPTO; Notice of Allowance dated Nov. 1, 2018 in U.S. Appl. No. 15/499,647. |
| USPTO; Notice of Allowance dated Nov. 15, 2018 in U.S. Appl. No. 15/499,647. |
| USPTO; Final Office Action dated Nov. 16, 2018 in U.S. Appl. No. 15/592,730. |
| USPTO; Restriction Requirement dated Oct. 10, 2018 in U.S. Appl. No. 15/615,489. |
| USPTO; Non-Final Office Action dated Nov. 9, 2018 in U.S. Appl. No. 15/636,307. |
| USPTO; Final Office Action dated Nov. 20, 2018 in U.S. Appl. No. 15/650,686. |
| USPTO; Non-Final Office Action dated Dec. 4, 2018 in U.S. Appl. No. 15/672,063. |
| USPTO; Restriction Requirement dated Oct. 15, 2018 in U.S. Appl. No. 15/672,119. |
| USPTO; Advisory Action dated Nov. 26, 2018 in U.S. Appl. No. 15/683,701. |
| USPTO; Non-Final Office Action dated Dec. 18, 2018 in U.S. Appl. No. 15/690,017. |
| USPTO; Non-Final Office Action dated Dec. 6, 2018 in U.S. Appl. No. 15/705,955. |
| USPTO; Notice of Allowance dated Dec. 6, 2018 in U.S. Appl. No. 15/711,989. |
| USPTO; Final Office Action dated Dec. 13, 2018 in U.S. Appl. No. 15/719,208. |
| USPTO; Final Office Action dated Nov. 14, 2018 in U.S. Appl. No. 15/726,959. |
| USPTO; Non-Final Office Action dated Nov. 28, 2018 in U.S. Appl. No. 15/795,056. |
| USPTO; Non-Final Office Action dated Sep. 26, 2018 in U.S. Appl. No. 15/832,188. |
| USPTO; Notice of Allowance dated Dec. 10, 2018 in U.S. Appl. No. 15/863,340. |
| USPTO; Restriction Requirement dated Dec. 13, 2018 in U.S. Appl. No. 15/886,225. |
| USPTO; Non-Final Office Action dated Nov. 15, 2018 in U.S. Appl. No. 15/890,037. |
| USPTO; Restriction Requirement dated Oct. 9, 2018 in U.S. Appl. No. 15/892,756. |
| USPTO; Restriction Requirement dated Nov. 26, 2018 in U.S. Appl. No. 15/917,262. |
| USPTO; Restriction Requirement dated Nov. 2, 2018 in U.S. Appl. No. 16/018,692. |
| WIPO; International Search Report and Written Opinion dated Nov. 6, 2018 in Application No. PCT/IB2017/001652. |
| Beynet et al. “Low temperature plasma-enhanced ALD enables cost-effective spacer defined double patterning,” Proceedings of SPIE, 7520, (2009). |
| Gupta et al., “Charge carrier transport and electroluminescence in atomic layer deposited poly-GaN/c-Si heterojunction diodes,” Journal of Applied Physics, 124, 084503 (2018). |
| Mackenzie et al. “Stress Control of Si-Based PEVCD Dielectrics,” Proc. Symp. Silicon Nitrode and Silicon Dioxide Thin Insulating Films & Other Emerging Dielectrics VIII, 148-159 (2005). |
| Number | Date | Country | |
|---|---|---|---|
| 20180010247 A1 | Jan 2018 | US |