Semiconductor devices are used in a variety of electronic applications, such as personal computers, cell phones, digital cameras, and other electronic equipment, as examples. Semiconductor devices are typically fabricated by sequentially depositing insulating or dielectric layers, conductive layers, and semiconductive layers of material over a semiconductor substrate, and patterning the various material layers using lithography to form circuit components and elements thereon.
A transistor is an element that is used often in semiconductor devices. There may be a large number of transistors (e.g. hundreds of, thousands of, or millions of transistors) on a single integrated circuit (IC), for example. A common type of transistor used in semiconductor device fabrication is a metal oxide semiconductor field effect transistor (MOSFET), as an example. A planar transistor (e.g. planar MOSFET) typically includes a gate dielectric disposed over a channel region in a substrate, and a gate electrode formed over the gate dielectric. A source region and a drain region of the transistor are formed on either side of the channel region.
Multiple gate field-effect transistors (MuGFETs) are a recent development in semiconductor technology. One type of MuGFET is referred to as a FinFET, which is a transistor structure that includes a fin-shaped semiconductor material that is raised vertically out of the semiconductor surface of an integrated circuit.
Aspects of the present disclosure are best understood from the following detailed description when read with the accompanying figures. It is noted that, in accordance with the standard practice in the industry, various features are not drawn to scale. In fact, the dimensions of the various features may be arbitrarily increased or reduced for clarity of discussion.
The following disclosure provides many different embodiments, or examples, for implementing different features of the invention. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, merely examples and are not intended to be limiting. For example, the formation of a first feature over or on a second feature in the description that follows may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features may be formed between the first and second features, such that the first and second features may not be in direct contact. In addition, the present disclosure may repeat reference numerals and/or letters in the various examples. This repetition is for the purpose of simplicity and clarity and does not in itself dictate a relationship between the various embodiments and/or configurations discussed.
Further, spatially relative terms, such as “beneath,” “below,” “lower,” “above,” “upper” and the like, may be used herein for ease of description to describe one element or feature's relationship to another element(s) or feature(s) as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The apparatus may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein may likewise be interpreted accordingly.
Methods of, and structures formed by, depositing a layer using Atomic Layer Deposition (ALD) are provided in accordance with various embodiments. Some example methods to form Fin Field-Effect Transistors (finFETs), and the structures formed thereby, by using ALD are provided in accordance with various embodiments. Intermediate stages of forming generic structures and, further, example finFETs are illustrated. Some embodiments discussed herein are discussed in the context of finFETs formed using a gate-last process. Some variations of the embodiments are discussed. One of ordinary skill in the art will readily understand other modifications that may be made that are contemplated within the scope of other embodiments. Although method embodiments are discussed in a particular order, various other method embodiments may be performed in any logical order and may include fewer or more steps described herein.
The surface 32 of the substrate 30 is terminated with a terminating species TS. In some examples, the terminating species TS is hydroxide (—OH), oxygen (—O), or the like. Termination by hydroxide (—OH) and/or oxygen (—O) can occur, for example, as a result of a cleaning or photoresist stripping process performed on the surface 32 of the substrate 30 and/or by exposing the surface 32 of the substrate 30 to a natural environment that contains oxygen. Termination by hydroxide (—OH) and/or oxygen (—O) can form an oxide layer, such as a native oxide, on the surface 32 of the substrate 30. The terminating species TS can be other species, such as hydrogen (—H), nitrogen (—N), ammonia (—NH3), or the like, such as depending on a cleaning and/or stripping process that is performed on the surface 32.
In
In
The inventors have observed a loading effect when depositing a layer across different underlying materials using ALD. This loading effect can be the result of longer incubation times on one material than on a different material on which the layer is deposited. This can further result in the deposited layer having a non-uniform thickness—the layer can have a greater thickness where the layer is deposited on one material than where the layer is deposited on another material. This can complicate deposition of such a layer in high aspect ratio openings, such as in a metal gate-last process, as illustrated below.
The inventors have discovered that using a chlorine-based treatment before depositing a layer, such as a metal-containing or metal layer, using ALD can alleviate or remove the material dependency of ALD such that the thickness of the deposited layer can be more uniform as deposited across different materials. For example, in
Further, interface(s) between a layer deposited by ALD and underlying material(s) can be free from an oxide as a result of the chlorine-based treatment and ALD. For example, the first surface 39 may be free from an oxide between the layer 34 and the first layer 38, and the second surface 41 may be free from an oxide between the layer 34 and the second layer 40.
The following discussion illustrates an example context in which the manufacturing process discussed with respect to
Further in
Although not specifically illustrated, appropriate wells may be formed in the fins 72 and/or substrate 70. For example, an n-well may be formed in a first region 200 and a fourth region 500 (illustrated in
For example, to form an n-well in the first region 200 and the fourth region 500, a photoresist can formed over the fins 72 and the isolation regions 74 in the second region 300 and the third region 400 of the substrate 70. The photoresist can be patterned to expose the first region 200 and the fourth region 500 of the substrate 70. The photoresist can be formed by using a spin-on technique and can be patterned using acceptable photolithography techniques. Once the photoresist is patterned, an n-type impurity implant can be performed in the first region 200 and the fourth region 500, and the photoresist may act as a mask to substantially prevent p-type impurities from being implanted into the second region 300 and the third region 400. The n-type impurities may be phosphorus, arsenic, or the like implanted in the first region 200 and the fourth region 500 to a concentration of equal to or less than 1018 cm−3, such as between about 1017 cm−3 and about 1018 cm−3. After the implant, the photoresist can be removed, such as by an acceptable ashing process.
Further, to form a p-well in the second region 300 and the third region 400, a photoresist can be formed over the fins 72 and the isolation regions 74 in the first region 200 and the fourth region 500 of the substrate. The photoresist can be patterned to expose the second region 300 and the third region 400 of the substrate 70. The photoresist can be formed by using a spin-on technique and can be patterned using acceptable photolithography techniques. Once the photoresist is patterned, a p-type impurity implant may be performed in the second region 300 and the third region 400, and the photoresist may act as a mask to substantially prevent p-type impurities from being implanted into the first region 200 and the fourth region 500. The p-type impurities may be boron, BF2, or the like implanted in the second region 300 and the third region 400 to a concentration of equal to or less than 1018 cm−3, such as between about 1017 cm−3 and about 1018 cm−3. After the implant, the photoresist can be removed, such as by an acceptable ashing process. After the implants, an anneal may be performed to activate the p-type and n-type impurities that were implanted. The implantations may form an n-well in the first region 200 and the fourth region 400 and a p-well in the second region 300 and the third region 400.
In
A person having ordinary skill in the art will readily understand that the process described with respect to
In
Further in
Although not specifically illustrated, implants for lightly doped source/drain (LDD) regions may be performed. Similar to the implants discussed above, a mask, such as a photoresist, may be formed over the second region 300 and the third region 400, e.g., for n-type devices, while exposing the first region 200 and the fourth region 500, e.g., for p-type devices, and p-type impurities may be implanted into the exposed fins 72 in the first region 200 and the fourth region 500. The mask may then be removed. Subsequently, a mask, such as a photoresist, may be formed over the first region 200 and the fourth region 400 while exposing the second region 300 and the third region 400, and n-type impurities may be implanted into the exposed fins 72 in the second region 300 and the third region 400. The mask may then be removed. The n-type impurities may be the any of the n-type impurities previously discussed, and the p-type impurities may be the any of the p-type impurities previously discussed. The lightly doped source/drain regions may have a concentration of impurities from about 1015 cm−3 to about 1016 cm−3. An anneal may be used to activate the implanted impurities.
Further in
In
The epitaxial source/drain regions 84 in the first region 200 and the fourth region 500, e.g., for p-type devices, may be formed by masking, such as with a hard mask, the second region 300 and the third region 400, e.g., for n-type devices. Then, source/drain regions of the fins 72 in the first region 200 and the fourth region 500 are etched to form recesses. The etch may be any appropriate etch selective to the fins 72 and may be anisotropic. The epitaxial source/drain regions 84 in the first region 200 and the fourth region 500 are then epitaxially grown in the recesses. The epitaxial growth may be by using Metal-Organic CVD (MOCVD), Molecular Beam Epitaxy (MBE), Liquid Phase Epitaxy (LPE), Vapor Phase Epitaxy (VPE), the like, or a combination thereof. The epitaxial source/drain regions 84 may comprise any acceptable material, such as appropriate for p-type finFETs. For example, the epitaxial source/drain regions 84 may comprise SiGe, SiGeB, Ge, GeSn, or the like. The epitaxial source/drain regions 84 may have surfaces raised from respective outer surfaces of the fins 72 and may have facets. The mask may then be removed, such as by using an etch selective to the material of the mask.
The epitaxial source/drain regions 86 in the second region 300 and the third region 400 may be formed by masking, such as with a hard mask, the first region 200 and the fourth region 500. Then, source/drain regions of the fins 72 in the second region 300 and the third region 400 are etched to form recesses. The etch may be any appropriate etch selective to the fins 72 and may be anisotropic. The epitaxial source/drain regions 86 in the second region 300 and the third region 400 are then epitaxially grown in the recesses. The epitaxial growth may be by using MOCVD, MBE, LPE, VPE, the like, or a combination thereof. The epitaxial source/drain regions 86 may comprise any acceptable material, such as appropriate for n-type finFETs. For example, the epitaxial source/drain regions 86 may comprise silicon, SiC, SiCP, SiP, or the like. The epitaxial source/drain regions 86 may have surfaces raised from respective outer surfaces of the fins 72 and may have facets. The mask may then be removed, such as by using an etch selective to the material of the mask.
The epitaxial source/drain regions 84 and 86 and/or source/drain regions of the fins 72 may be implanted with dopants, similar to the process previously discussed for forming lightly doped source/drain regions, followed by an anneal. The source/drain regions may have an impurity concentration of between about 1019 cm−3 and about 1021 cm−3. The p-type impurities for source/drain regions in the first region 200 and the fourth region 500, e.g., for p-type devices, may be any of the p-type impurities previously discussed, and the n-type impurities for source/drain regions in the second region 300 and the third region 400, e.g., for n-type devices, may be any of the n-type impurities previously discussed. In other embodiments, the epitaxial source/drain regions 84 and 86 may be in situ doped during growth.
Further in
In
An interfacial dielectric 92 is formed in each opening and on the fins 72. The interfacial dielectric 92 may be, for example, an oxide or the like formed by thermal oxidation, chemical oxidation, ALD, or the like. A thickness of the interfacial dielectric 92 may be in a range from about 5 Å to about 30 Å, such as about 9 Å. A gate dielectric layer 94 is then formed conformally on the top surface of the ILD090 and in the openings along sidewalls of the gate spacers 82 and on the interfacial dielectric 92. In some embodiments, the gate dielectric layer 94 comprises a high-k dielectric material, and in these embodiments, the gate dielectric layer 94 may have a k value greater than about 7.0, and may include a metal oxide or a silicate of Hf, Al, Zr, La, Mg, Ba, Ti, Pb, and combinations thereof. The formation methods of gate dielectric layer 94 may include ALD, CVD, Molecular-Beam Deposition (MBD), the like, or a combination thereof. A thickness of the gate dielectric layer 94 may be in a range from about 5 Å to about 30 Å, such as about 15 Å.
A capping layer is then formed conformally on the gate dielectric layer 94. In the illustrated embodiment, the capping layer comprises a first sub-layer 96 and a second sub-layer 98. In some embodiments, the capping layer may be a single layer or may comprise additional sub-layers. The capping layer may function as a barrier layer to prevent a subsequently deposited metal-containing material from diffusing into the gate dielectric layer 94. Further, the second sub-layer 98, as illustrated, can function as an etch stop during the formation of work function tuning layers in various regions 200, 300, 400 and 500 if the first sub-layer 96 is formed from a same material as the work function tuning layers, as will become clearer subsequently. The first sub-layer 96 can comprise titanium nitride (TiN) or the like deposited conformally on the gate dielectric layer 94 by ALD, CVD, or the like. The second sub-layer 98 can comprise tantalum nitride (TaN) or the like deposited conformally on the first sub-layer 96 by ALD, CVD, or the like. A thickness of the capping layer may be in a range from about 5 Å to about 60 Å, such as about 25 Å. In the illustrated embodiment, a thickness of the first sub-layer 96 may be in a range from about 5 Å to about 30 Å, such as about 10 Å, and a thickness of the second sub-layer 98 may be in a range from about 5 Å to about 30 Å, such as about 15 Å.
A first work function tuning layer 100 is then formed conformally on the capping layer, e.g., on the second sub-layer 98. The first work function tuning layer 100 may be any acceptable material to tune a work function of a device to a desired amount given the application of the device to be formed, and may be deposited using any acceptable deposition process. In some embodiments, the first work function tuning layer 100 comprises titanium nitride (TiN) or the like deposited by ALD or the like. A thickness of the first work function tuning layer 100 may be in a range from about 5 Å to about 30 Å, such as about 10 Å.
A mask 102 is then patterned over the first work function tuning layer 100 in the fourth region 500, while the first work function tuning layer 100 in the first, second, and third regions 200, 300, and 400 is exposed. In some embodiments, the mask 102 is a photoresist, which can be formed over the fourth region 500. The photoresist can be patterned to expose the first, second, and third regions 200, 300, and 400. The photoresist can be formed by using a spin-on technique and can be patterned using acceptable photolithography techniques. Once the mask 102 is patterned, an etch selective to the first work function tuning layer 100 is performed to remove the first work function tuning layer 100 from the first, second, and third regions 200, 300, and 400, as illustrated in
A terminating species, such as hydroxide and/or oxygen, can terminate the surfaces of the second sub-layer 98 and the first work function tuning layer 100 as a result of the etching, mask 102 removal, and/or exposure to an oxygen-containing ambient, such as a natural environment. The species, such as when hydroxide and/or oxygen, can form an oxide, such as a native oxide, on these layers 98 and 100. In some embodiments, a chlorine-based treatment is performed on the surfaces of the second sub-layer 98 and the first work function tuning layer 100, as discussed with respect to
Then in
A mask 106 is then patterned over the second work function tuning layer 104 in the third and fourth regions 400 and 500, while the second work function tuning layer 104 in the first and second regions 200 and 300 is exposed. In some embodiments, the mask 106 is a photoresist, which can be formed over the third and fourth regions 400 and 500. The photoresist can be patterned to expose the first and second regions 200 and 300. The photoresist can be formed by using a spin-on technique and can be patterned using acceptable photolithography techniques. Once the mask 106 is patterned, an etch selective to the second work function tuning layer 104 is performed to remove the second work function tuning layer 104 from the first and second regions 200 and 300, as illustrated in
A terminating species, such as hydroxide and/or oxygen, can terminate the surfaces of the second sub-layer 98 and the second work function tuning layer 104 as a result of the etching, mask 106 removal, and/or exposure to an oxygen-containing ambient, such as a natural environment. The species, when hydroxide and/or oxygen, can form an oxide, such as a native oxide, on these layers 98 and 104. In some embodiments, a chlorine-based treatment is performed on the surfaces of the second sub-layer 98 and the second work function tuning layer 104, as discussed with respect to
Then in
A mask 112 is then patterned over the fourth work function tuning layer 110 in the second, third, and fourth regions 300, 400, and 500, while the fourth work function tuning layer 110 in the first region 200 is exposed. In some embodiments, the mask 112 is a photoresist, which can be formed over the second, third, and fourth regions 300, 400, and 500. The photoresist can be patterned to expose the first region 200. The photoresist can be formed by using a spin-on technique and can be patterned using acceptable photolithography techniques. Once the mask 112 is patterned, an etch selective to the fourth work function tuning layer 110 and third work function tuning layer 108 is performed to remove the fourth work function tuning layer 110 and third work function tuning layer 108 from the first region 200, as illustrated in
A terminating species, such as hydroxide and/or oxygen, can terminate the surfaces of the second sub-layer 98 and the fourth work function tuning layer 110 as a result of the etching, mask 112 removal, and/or exposure to an oxygen-containing ambient, such as a natural environment. The species, when hydroxide and/or oxygen, can form an oxide, such as a native oxide, on these layers 98 and 110. In some embodiments, a chlorine-based treatment is performed on the surfaces of the second sub-layer 98 and the fourth work function tuning layer 110, as discussed with respect to
Then in
Then in
As illustrated, the layered structure 120a in the first region 200 includes the gate dielectric layer 94, the capping layer (which includes the first sub-layer 96 and the second sub-layer 98), and the barrier layer 114. As illustrated, the layered structure 120b in the second region 300 includes the gate dielectric layer 94, the capping layer (which includes the first sub-layer 96 and the second sub-layer 98), the third work function tuning layer 108, the fourth work function tuning layer 110, and the barrier layer 114. As illustrated, the layered structure 120c in the third region 400 includes the gate dielectric layer 94, the capping layer (which includes the first sub-layer 96 and the second sub-layer 98), the second work function tuning layer 104, the third work function tuning layer 108, the fourth work function tuning layer 110, and the barrier layer 114. As illustrated, the layered structure 120d in the fourth region 500 includes the gate dielectric layer 94, the capping layer (which includes the first sub-layer 96 and the second sub-layer 98), the first work function tuning layer 100, the second work function tuning layer 104, the third work function tuning layer 108, the fourth work function tuning layer 110, and the barrier layer 114.
In
Next, a planarization process, such as a CMP, may be performed to remove the excess portions of conductive material 122, which excess portions are over the top surface of ILD090. Then, a controlled etch-back selective to the conductive material 122, and possibly selective to the layered structures 120a, 120b, 120c, and 120d, is performed to recess the conductive material 122, which results in the gate structures illustrated in
In
An upper ILD (ILD1) 126 is deposited over the ILD090 and the dielectric caps 124, and contacts 128 are formed through the ILD1126, ILD090, and ESL 88 to the epitaxial source/drain regions 84 and 86. ILD1126 is formed of a dielectric material such as PSG, BSG, BPSG, USG, or the like, and may be deposited by any suitable method, such as CVD and PECVD. Openings for contacts 128 are formed through the ILD1126, ILD090, and ESL 88. The openings may be formed using acceptable photolithography and etching techniques. A liner, such as a diffusion barrier layer, an adhesion layer, or the like, and a conductive material are formed in the openings. The liner may include titanium, titanium nitride, tantalum, tantalum nitride, or the like. The conductive material may be copper, a copper alloy, silver, gold, tungsten, aluminum, nickel, or the like. A planarization process, such as a CMP, may be performed to remove excess material from a surface of the ILD1126. The remaining liner and conductive material form contacts 128 in the openings. An anneal process may be performed to form a silicide at the interface between the epitaxial source/drain regions 84 and 86 and the contacts 128, respectively.
Although not explicitly shown, a person having ordinary skill in the art will readily understand that further processing steps may be performed on the structure in
Additional details of some specific examples are discussed below. As a point of reference, a titanium nitride (TiN) layer is deposited by ALD on a tantalum nitride (TaN) layer without using a chlorine-based treatment. The point of reference may follow, for example, the process outlined above from the deposition of the second sub-layer 98 to the deposition of the second work function tuning layer 104 without using a chlorine-based treatment. In this point of reference, the TaN layer had a thickness of 16.49 Å, and the TiN layer had a thickness of 15.62 Å.
This point of reference was then modified to include a gaseous WCl5 treatment before depositing the TiN layer by ALD. Using a 1 second treatment, the TaN layer had a thickness of 16.52 Å, and the TiN layer had a thickness of 15.21 Å. Using a 2 second treatment, the TaN layer had a thickness of 16.27 Å, and the TiN layer had a thickness of 15.36 Å. Using a 4 second treatment, the TaN layer had a thickness of 15.58 Å, and the TiN layer had a thickness of 17.01 Å. Using a 30 second treatment, the TaN layer had a thickness of 9.76 Å, and the TiN layer had a thickness of 21.43 Å. Using a 60 second treatment, the TaN layer had a thickness of 11.57 Å, and the TiN layer had a thickness of 18.57 Å. Using the treatments for 30 seconds and 60 seconds resulted in thicknesses comparable to depositing a TiN layer in situ on the TaN layer, where the TaN layer had a thickness of 9.59 Å, and the TiN layer had a thickness of 22.30 Å.
In these examples, a tantalum oxide (e.g., Ta2O5) layer was observed on the TaN layer before the WCl5 treatment. The following reaction was observed:
WCl5(g)+Ta2O5(s)→WOCly(g)+TaClx(s)
This reaction results in Cl passivating the TaN layer and the oxide being removed as a gaseous byproduct of the reaction. The Cl is believed to increase the reactivity on the TaN layer during the ALD process compared to when a Ta2O5 layer is present on the TaN layer. This can result in a shorter incubation cycle for the ALD process, which can result in faster deposition rates in the ALD process.
In other examples, a gaseous TiCl4 treatment or a gaseous TaCl5 treatment is used. Using these treatments and the gaseous WCl5 treatment in different examples, it was observed that a higher treatment temperature can increase the efficiency of an oxide removal. For example, a gaseous TaCl5 treatment at 525° C. had a higher oxide removal rate than a gaseous TaCl5 treatment at 500° C., and the gaseous TaCl5 treatment at 500° C. had a higher oxide removal rate than gaseous TaCl5 treatment at 375° C. An increased temperature can decrease a barrier for desorption of the oxide byproduct of the reaction between the oxide layer on the TaN layer and the Cl-based treatment, and thus, the removal rate of the oxide layer can be increased with increased temperature.
Some embodiments can achieve advantages. As discussed, using a chlorine-based treatment on layers of different materials before using ALD to deposit another layer on those layers can increase the deposition rate of the ALD process, thereby reducing the loading effect. Further, the deposition rate can be substantially the same when using ALD to deposit a layer on differing materials, thereby reducing substrate dependence. With these advantages, gap fill problems can be overcome in processes, such as the gate-last process discussed above.
An embodiment is a method. In accordance with the method, a first metal-containing layer is formed on a substrate. A second metal-containing layer is formed on the substrate. A material of the first metal-containing layer is different from a material of the second metal-containing layer. A chlorine-based treatment is performed on the first metal-containing layer and the second metal-containing layer. A third metal-containing layer is deposited on the first metal-containing layer and the second metal-containing layer using Atomic Layer Deposition (ALD).
Another embodiment is a method. In accordance with the method, a dielectric is formed on a substrate, and the dielectric has a first opening and a second opening. A first metal-containing layer is formed on the dielectric and in the first opening and the second opening. A second metal-containing layer is formed on the first metal-containing layer. The second metal-containing layer is removed from the first opening. The first metal-containing layer in the first opening and the second metal-containing layer in the second opening are exposed to a chlorine-based fluid. A third metal-containing layer is formed on the first metal-containing layer in the first opening and the second metal-containing layer in the second opening using Atomic Layer Deposition (ALD).
A further embodiment is a method. In accordance with the method, a first metal-containing layer and a second metal-containing layer is formed, and a material of the first metal-containing layer is different from a material of the second metal-containing layer. The first metal-containing layer has a surface terminated with an oxygen-containing species. The oxygen-containing species is removed from the surface of the first metal-containing layer, and the surface of the first metal-containing layer is passivated with a chlorine-based species. A third metal-containing layer is deposited by Atomic Layer Deposition (ALD) on the surface of the first metal-containing layer passivated with the chlorine-based species and on a surface of the second metal-containing layer.
The foregoing outlines features of several embodiments so that those skilled in the art may better understand the aspects of the present disclosure. Those skilled in the art should appreciate that they may readily use the present disclosure as a basis for designing or modifying other processes and structures for carrying out the same purposes and/or achieving the same advantages of the embodiments introduced herein. Those skilled in the art should also realize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and that they may make various changes, substitutions, and alterations herein without departing from the spirit and scope of the present disclosure.
This application is a continuation of U.S. application Ser. No. 14/815,286, filed on Jul. 31, 2015, which application is hereby incorporated herein by reference.
Number | Date | Country | |
---|---|---|---|
Parent | 14815286 | Jul 2015 | US |
Child | 15935655 | US |