Precursors for Atomic Layer Deposition

Abstract
Atomic layer deposition (ALD) and chemical vapor deposition (CVD) precursors that are useful for forming metal-containing films are provided. These compounds include triazapentadienyl, α-imino enolate compounds and α-imino ketone compounds having formulae 1, 2, and 3, respectively. An ALD method using the precursors is also provided.
Description
FIELD OF THE INVENTION

In at least one aspect, the present invention is related to the formation of metal films from “metalorganic” precursors.


BACKGROUND OF THE INVENTION

The growth of thin films is a central step in the fabrication of many functional materials. In recent years, atomic layer deposition (ALD) has been recognized as an important process for forming thin films for the electronics industry. Synthesizing suitable precursors for ALD growth of transition metal-containing thin films is an important and challenging aspect of this process. Transition metal complexes should possess the following features in order to serve as good precursors in ALD of transition metal-containing thin films: (1) the highest possible volatility to allow the lowest deposition temperatures, (2) high thermal stability throughout the range of desired deposition temperatures, (3) the ability to chemisorb or react with surface sites, and (4) high reactivity with the second precursor (co-reactant that reduces the metal precursor to its metal).


Accordingly, there is a need for the design of novel ALD precursors having the requisite chemical properties.


SUMMARY OF THE INVENTION

The present invention solves one or more problems of the prior art by providing a triazapentadienyl compound that is useful for forming a metal-containing film. The triazapentadienyl compound is described generally by formula (I):




embedded image


wherein:


M is a metal selected from groups 2 to 12 of the Periodic Table (e.g., Mg, Zn, Cr, Mn, Fe, Co, or Ni);


R1 is C1-8 alkyl, C5-12 aryl, or NR5R6;


R2 is C1-8 alkyl;


R3, R4 are each independently hydrogen or C1-8 alkyl; and


R5, R6 are each independently C1-8 alkyl with the proviso that when M is Zn, Mg, Cr, R5 is C2-8 alkyl.


In another embodiment, an α-imino enolate compound that is useful for forming a metal-containing film is provided. The α-imino enolate compound is described generally by formula (I):




embedded image


wherein:


M is a metal selected from groups 2 to 12 of the Periodic Table (e.g., Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu);


R7, R8, R9 are each independently hydrogen, C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl; and R10 is C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl.


In another embodiment, an α-imino ketonate compound that is useful for forming a metal-containing film is provided. The α-imino ketonate compound is described generally by formula (III):




embedded image


M is a metal selected from groups 2 to 12 of the Periodic Table (e.g., Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu);


R11 is C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl; and


R12, R13 are each independently hydrogen, C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl.


In another embodiment, a method of forming a metal-containing product is provided. The method includes a step of reacting a first compound having bidentate ligands with an reactive compound to form a first product. The first compound is selected from the group consisting of compounds having formula 1, 2 and 3 set forth above.





BRIEF DESCRIPTION OF THE DRAWINGS

Exemplary embodiments of the present invention will become more fully understood from the detailed description and the accompanying drawings, wherein:



FIG. 1 is a schematic illustration of an ALD deposition system used in an embodiment of the present invention;



FIG. 2 provides examples of acids that can be reacted with the compounds of having formula 1, 2, and 3;



FIG. 3 provides thermogravimetric analysis (TGA) for compounds 1-5;



FIG. 4 provides thermogravimetric analysis (TGA) for compounds 7-10;



FIG. 5 provides an X-ray Powder Diffraction Spectrum of nickel metal produced upon treatment of compound 10 with hydrazine;



FIG. 6 provides thermogravimetric analysis (TGA) for compounds 18-20, and 22;



FIG. 7 provides an X-ray powder diffraction spectrum of copper metal produced upon treatment of 17 with BH3(NHMe2); and



FIG. 8 provides an X-ray powder diffraction spectrum of nickel metal produced upon treatment of 16 with BH3(NHMe2).





DESCRIPTION OF THE INVENTION

Reference will now be made in detail to presently preferred compositions, embodiments and methods of the present invention which constitute the best modes of practicing the invention presently known to the inventors. The Figures are not necessarily to scale. However, it is to be understood that the disclosed embodiments are merely exemplary of the invention that may be embodied in various and alternative forms. Therefore, specific details disclosed herein are not to be interpreted as limiting, but merely as a representative basis for any aspect of the invention and/or as a representative basis for teaching one skilled in the art to variously employ the present invention.


Except in the examples, or where otherwise expressly indicated, all numerical quantities in this description indicating amounts of material or conditions of reaction and/or use are to be understood as modified by the word “about” in describing the broadest scope of the invention. Practice within the numerical limits stated is generally preferred. Also, unless expressly stated to the contrary:percent, “parts of,” and ratio values are by weight; the description of a group or class of materials as suitable or preferred for a given purpose in connection with the invention implies that mixtures of any two or more of the members of the group or class are equally suitable or preferred; description of constituents in chemical terms refers to the constituents at the time of addition to any combination specified in the description, and does not necessarily preclude chemical interactions among the constituents of a mixture once mixed; the first definition of an acronym or other abbreviation applies to all subsequent uses herein of the same abbreviation and applies mutatis mutandis to normal grammatical variations of the initially defined abbreviation; and, unless expressly stated to the contrary, measurement of a property is determined by the same technique as previously or later referenced for the same property.


It is also to be understood that this invention is not limited to the specific embodiments and methods described below, as specific components and/or conditions may, of course, vary. Furthermore, the terminology used herein is used only for the purpose of describing particular embodiments of the present invention and is not intended to be limiting in any way.


It must also be noted that, as used in the specification and the appended claims, the singular form “a,” “an,” and “the” comprise plural referents unless the context clearly indicates otherwise. For example, reference to a component in the singular is intended to comprise a plurality of components.


Throughout this application, where publications are referenced, the disclosures of these publications in their entireties are hereby incorporated by reference into this application to more fully describe the state of the art to which this invention pertains.


In an embodiment, a triazapentadienyl compound that is useful for forming a metal-containing film is provided. The triazapentadienyl compound is described generally by formula (1):




embedded image


wherein:


M is a metal selected from groups 2 to 12 of the Periodic Table. In particular, M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu;


R1 is C1-8 alkyl, C5-12 aryl, or NR5R6;


R2 is C1-8 alkyl;


R3, R4 are each independently hydrogen or C1-8 alkyl; and


R5, R6 are each independently C1-8 alkyl with the proviso that when M is Cr, R5 is C2-8 alkyl. In a refinement, when R1 is C1-8 alkyl, M is Zn, Mg, Cr, Mn, Fe, Co, or Ni, and when R1 is N R5R6; M is Zn, Mg, Mn, Fe, Co, or Ni. In a refinement, R1, R2, R3, R4 are each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, t-butyl, or phenyl. In a particularly useful refinement, R2 is t-butyl.


In a variation of the compound having formula (1), when R1 is C1-8 alkyl, M is Cr, Mn, Fe, Co, or Ni, and when R1 is N R5R6, M is Zn, Mg, Mn, Fe, Co, or Ni. In another variation, R1 is C1-8 alkyl and M is Zn, Mg, Cr, Mn, Fe, Co, or Ni. In still another variation, R1 is N R5R6 and M is Zn, Mg, Mn, Fe, Co, or Ni.


In another embodiment, an α-imino ketonate compound that is useful for the deposition of metal-containing films and, in particular, metal films is provided. The compound of this embodiment is described by formula II:




embedded image


wherein:


M is a metal selected from groups 2 to 12 of the Periodic Table. In particular, M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu;


R7, R8, R9 are each independently hydrogen, C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl; and


R10 is C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl.


In a refinement, R7, R8, R9, R10 are each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, t-butyl, or phenyl. In a particularly useful refinement, R10 is t-butyl. The α-imino enolate complexes of the present embodiment sublime in the range of 100-160° C. at 0.05 Torr and decompose in the temperature range of 190-295° C. making these compounds useful for atomic layer deposition (ALD).


In still another embodiment, an α-imino ketonate compound that is useful for forming a metal-containing film and, in particular, a metal film is provided. The α-imino ketonate compound is described generally by formula (III):




embedded image


M is a metal selected from groups 2 to 12 of the Periodic Table. In particular, M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu; R11 is C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl; and


R12, R13 are each independently hydrogen, C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl.


In a refinement, R11, R12, R13 are each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, t-butyl, or phenyl. In a particularly useful refinement, R11 is t-butyl. The α-imino ketonate complexes of the present embodiment sublime at 100-135° C. at 0.05 Torr and decompose between 180-250° C. making these compounds useful precursors for ALD.


In another embodiment, a method for forming a metal-containing compound includes a step of reacting a compound having bidentate ligands with an reactive compound to form a first product, the first compound selected from the group consisting of:




embedded image


wherein:


M is a metal selected from groups 2 to 12 of the Periodic Table. In particular, M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu;


R1 is C1-8 alkyl, C5-12 aryl, or N R5R6;


R2, R3, R4 are each independently C1-8 alkyl;


R5, R6 is C1-8 alkyl with the proviso that when M is Cr, R5 is C2-8 alkyl; and


R5, R6, R7, R8, R9, R10 are each independently C1-8 alkyl, C5-12 aryl, or C5-12 heteroaryl. In a refinement, the reactive compound is a reducing agent. In this variation, the resulting product is a metal (i.e, zero oxidation state). Examples of useful reducing agents include, but are not limited to, molecular hydrogen, atomic hydrogen, silane, disilane, organosilanes, compounds containing Si—H bonds, germane, organogermanes, compounds containing Ge—H bonds, stannane, compounds containing Sn—H bonds, other metal hydride compounds, formic acid, glyoxalic acid, oxalic acid, other carboxylic acids, diborane, compounds containing B—H bonds, hydrazine, carbon-substituted hydrazines, formalin, formaldehyde, organic alcohols, organoaluminum compounds, organozinc compounds, other organometallic compounds, plasma-activated versions of the above compounds. In another refinement, the reactive compound is an oxidizing agent with the resulting product being a metal oxide. Examples of useful oxidizing agents include, but are not limited to, water, ozone, molecular oxygen, atomic oxygen, organic alcohols, hydrogen peroxide, organic hydroperoxides, organic peroxides, nitrous oxide, plasma-activated versions of the above compounds. In still another variation, the activating compound is a nitriding agent (i.e., a nitrogen-containing agent) with the resulting product being a metal nitride. Examples of such nitriding agents include, but are not limited to, ammonia, hydrazine, alkyl-substituted hydrazines, and plasma activated versions thereof.


In another variation, a method for forming a metal-containing film using compounds 1, 2, or 3 is provided. FIG. 1 provides a schematic of an atomic layer deposition system that is useful for forming such films. Deposition system 10 includes reaction chamber 12, substrate holder 14, and vacuum pump 16. Typically, substrate 20 is heated via heater 18. The method has a deposition cycle comprising contacting substrate 20 with a vapor of a metal-containing compound described by formula 1, 2, or 3 as set forth above. In particular, the vapor is introduced from precursor source 22 into reaction chamber 12 for a predetermined pulse time. The pulse time is controlled via control valve 24. At least a portion of the vapor of the metal-containing compound having formula 1, 2, or 3 modifies (e.g, adsorbs or reacts with) substrate surface 26 to form a modified surface. The method further comprises contacting the modified surface with a vapor of a reactive compound from compound source 30 for a predetermined pulse time. The pulse time is controlled via control valve 32. The reactive compound causes the metal-containing compound to react and form at least a portion of the thin metal containing film on the surface of the substrate. The reduced pressure of chamber 12 is maintained by vacuum pump 16.


In a variation of the present embodiment, the method further comprises removing at least a portion of the vapor of the metal containing compound having formula 1, 2, or 3 that is lingering in the gas phase (i.e., has not adsorbed or reacted with the substrate) from the vicinity of the substrate before introducing the vapor of the reactive compound and removing at least a portion of the vapor of the reactive compound from the vicinity of the substrate. The metal-containing compound and reactive compound are removed in purging steps by introducing a purge gas from purge source 34 into reaction chamber 12 for a predetermined purge time. The purge time is controlled by control valve 36.


In another variation, the method further includes at least one additional deposition cycle comprising sequentially contacting the substrate with the vapor of a metal-containing compound having formula 1, 2, or 3 and then the vapor of the reactive compound. In some refinements, the substrate is contacted for a plurality of additional deposition cycles. For example, the substrate may be contacted with from 1 to several thousand deposition cycles depending on the thickness of the film desired.


In another variation, a method for forming a metal-containing film using compounds 1, 2, or 3 is provided. Referring again to FIG. 1, deposition system 10 includes reaction chamber 12, substrate holder 14, and vacuum pump 16. Typically, the substrate is heated via heater 18. The method has a deposition cycle comprising contacting substrate 20 with a vapor of a metal-containing compound described by formula 1, 2, or 3 as set forth above. In particular, the vapor is introduced from precursor source 22 into reaction chamber 12 for a predetermined pulse time. The pulse time is controlled via control valve 24. At least a portion of the vapor of the metal-containing compound having formula 1, 2, or 3 modifies (e.g, adsorbs or reacts with) substrate surface 26 to form a modified surface. In the next reaction step of the deposition cycle, an acid such as formic acid is then introduced from acid source 40 into reaction chamber 12 for a second predetermined pulse time. The second predetermined pulse time is controlled by valve 42. Examples of other suitable acids are provided in FIG. 2. In FIG. 2, R14 is H (i.e., hydride), C1-8 alkyl, C6-12 aryl, or C1-8 fluoroalkyl, X is N3−, NO3, halide (e.g., Cl, F, Br), and n is an integer from 1 to 6. In a refinement, R14 is hydride, C1-4 alkyl, C6-10 aryl, or C1-4 fluoroalkyl, X is N3−, NO3−, halide (e.g., Cl, F, Br), and n is an integer from 1 to 6. Examples of useful alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, t-butyl, isobutyl, sec-butyl, and the like. Examples of useful aryl groups include, but are not limited to, phenyl, tolyl, naphthyl, and the like. It should also be appreciated that R, R1, R2 may be optionally substituted with groups such as halide. The second predetermined pulse time should be sufficiently long that available binding sites on the first modified substrate surface are saturated and a second modified surface is formed. Typically, the second predetermined pulse time is from 0.1 second to 20 seconds. The second predetermined pulse time is controlled via control valve 32. Reaction chamber 12 is then purged with an inert gas for a second purge time (typically, 0.5 seconds to 2 minutes as set forth above).


In the final reaction step of the deposition cycle, a reducing agent is then introduced from reductant source 30 into reaction chamber 12 for a third predetermined time. Examples of suitable reducing agents include, but are not limited to, hydrazine, hydrazine hydrate, alkyl hydrazines, 1,1-dialkylhydrazines, 1,2-dialkylhydrazines, H2, H2 plasma, ammonia, ammonia plasma, silanes, disilanes, trisilanes, germanes, diborane, formalin, amine borane, dialkyl zinc, alkyl aluminum, alkyl gallium, alkyl indium complexes, and other plasma-based gases, and combinations thereof. The third predetermined pulse time should be sufficiently long that available binding sites on the second modified substrate surface are saturated with a metal layer being formed thereon. Typically, the third predetermined pulse time is from 0.1 second to 20 seconds. Reaction chamber 12 is then purged with an inert gas for a third purge time (typically, 0.5 seconds to 2 minutes as set forth above).


In a variation as set forth above, the method further comprises removing at least a portion of the vapor of the metal containing compound having formula 1, 2, or 3 that is lingering in the gas phase (i.e., has not adsorbed or reacted with the substrate) from the vicinity of the substrate before introducing the vapor of the reactive compound and removing at least a portion of the vapor of the reactive compound from the vicinity of the substrate. The metal-containing compound and reactive compound are removed in purging steps by introducing a purge gas from purge source 34 into reaction chamber 12 for a predetermined purge time. The purge time is controlled by control valve 36.


Pulse times and purge times also depend on the properties of the chemical precursors and the geometric shape of the substrates. Thin film growth on flat substrates uses short pulse and purge times, but pulse and purge times in ALD growth on 3-dimensional substrates can be very long. Therefore, in one refinement, pulse times and purge times are each independently from about 0.0001 to 200 seconds. In another refinement, pulse and purge times are each independently from about 0.1 to about 10 seconds.


In the film forming methods set forth above, the specific type of reactive compound that will be used depends on the particular metal compound to be made. If a metal film is to be made, the reactive compound will be a reducing agent as set forth above. If a metal oxide film is made, the reactive compound is an oxidizing agent as set forth above. If a nitride film is made, the reactive compound is a nitriding agent as set forth above.


During film formation by the methods, the substrate temperature will be at a temperature suitable to the properties of the chemical precursor(s) and film to be formed. In a refinement of the method, the substrate is set to a temperature from about 0 to 1000° C. In another refinement of the method, the substrate has a temperature from about 50 to 450° C. In another refinement of the method, the substrate has a temperature from about 100 to 250° C. In still another refinement of the method, the substrate has a temperature from about 150 to 400° C. In another refinement of the method, the substrate has a temperature from about 200 to 300° C.


The desired metal film thickness depends on the number of deposition cycles. Therefore, in a refinement, the deposition cycle is repeated a plurality of times to form a predetermined thickness of the metal film. In a further refinement, the deposition cycle is repeated a plurality of times to form a metal film having a thickness from about 5 nanometers to about 200 nanometers. In still another refinement, the deposition cycle is repeated a plurality of times to form a metal film having a thickness from about 5 nanometers to about 300 nanometers. In yet another refinement, the deposition cycle is repeated a plurality of times to form a metal film having a thickness from about 5 nanometers to about 100 nanometers.


During film formation by the method of the present embodiment, the substrate temperature will be at a temperature suitable to the properties of the chemical precursor(s) and film to be formed. In a refinement of the method, the substrate is set to a temperature from about 0 to 1000° C. In another refinement of the method, the substrate has a temperature from about 50 to 450° C. In another refinement of the method, the substrate has a temperature from about 100 to 250° C. In still another refinement of the method, the substrate has a temperature from about 150 to 400° C. In another refinement of the method, the substrate has a temperature from about 200 to 300° C.


Similarly, the pressure during film formation is set at a value suitable to the properties of the chemical precursors and film to be formed. In one refinement, the pressure is from about 10−6 Torr to about 760 Torr. In another refinement, the pressure is from about 0.1 millitorr to about 10 Torr. In still another refinement, the pressure is from about 1 to about 100 millitorr. In yet another refinement, the pressure is from about 1 to 20 millitorr.


The following examples illustrate the various embodiments of the present invention. Those skilled in the art will recognize many variations that are within the spirit of the present invention and scope of the claims.


EXPERIMENTAL SECTION 1

General Considerations.


All manipulations were carried out under argon using either Schlenk or glove box techniques, except that the ligands were prepared in ambient atmosphere. Tetrahydrofuran was distilled from sodium benzophenone ketyl, and hexane was distilled from P2O5. Anhydrous transition metal chlorides (CrCl2, MnCl2, FeCl2, CoCl2, and NiCl2) were obtained from Strem Chemicals Inc. and used as received. NiCl2.CH3CN was prepared according to a literature procedure.1 Potassium hydride (30 wt % dispersion in mineral oil; washed with hexane before use), tert-butyl amine, and 1,1-dimethylhydrazine were purchased from Sigma-Aldrich. tert-Butyl hydrazine hydrochloride was purchased from Acros Organics. Glyoxal was purchased from Alfa Aesar.



1H and 13C{1H} NMR spectra were obtained at 400 and 100 MHz in benzene-d6 or chloroform-d and were referenced to the residual proton and the 13C resonances of the solvents. Infrared spectra were obtained using Nujol as the medium. Melting points were obtained on a Thermo Scientific Mel-Temp 3.0 digital melting point apparatus and are uncorrected. Thermogravimetric analyses (TGA) were carried out with a SDT-2960 TGA/DTA instrument. Magnetic moments were determined in the solid state using a Johnson Mathey magnetic susceptibility apparatus, and by 1H NMR in benzene solution using the Evans method.


Preparation of 1,5-di-test-butyl-1,2,5-triazapentadiene

2-(2-(tert-butyl)hydrazono)acetaldehyde was prepared according to a published procedure.3 A 100 mL round bottom flask was charged with a magnetic stir bar, 2-(2-(tert-butyl)hydrazono)acetaldehyde (1.000 g, 7.80 mmol), and diethyl ether (15 mL). To this stirred solution at ambient temperature was slowly added tert-butyl amine (0.83 mL, 7.80 mmol) and the solution was stirred for 4 h. The resultant yellow solution was washed with water (20 mL) and the organic layer was separated. The organic layer was dried over anhydrous Na2SO4 and the volatile components were removed under reduced pressure. Light yellow crystals were obtained by sublimation of the crude solid at 80° C./0.05 Torr (0.786 g, 55%): mp 200° C.; IR (Nujol, cm−1) 3144 (m), 1620 (m), 1547 (m), 1365 (m), 1346 (m), 1304 (w), 1260 (w), 1222 (m) 1166 (m), 1096 (w), 1026 (w), 970 (w), 883 (w), 799 (w); 1H NMR (CDCl3, 23° C., δ) 7.84 (s, 1H, CHN), 7.30 (s, 1H, CHN), 5.28 (s, broad 1H, NH), 1.22 (s, 9H, C(CH3)3), 1.21 (s, 9H, C(CH3)3); 13C{1H} NMR (CDCl3, 23° C., ppm) 155.22 (s, CHN), 137.35 (s, CHN), 56.91 (s, C(CH3)3), 54.50 (s, C(CH3)3), 29.65 (s, C(CH3)3), 28.57 (s, C(CH3)3); ESI-HRMS: calcd for C10H22N3 ([M+H]+) 184.1814. found 184.1814.


Preparation of 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene

2-(2,2-Dimethylhydrazono)acetaldehyde was prepared according to a published procedure.4 A 100 mL round bottom flask was charged with a magnetic stir bar, 2-(2,2-dimethylhydrazono)acetaldehyde (1.000 g, 9.98 mmol), and water (20 mL). To this stirred solution at ambient temperature was slowly added a mixture of tert-butyl hydrazine hydrochloride (1.370 g, 11.00 mmol) and potassium hydroxide (0.726 g, 11.00 mmol) in water (30 mL). This solution was stirred for 15 min and was set aside for 18 hours. An oil formed initially, which converted to a yellow solid over this time. The solution was filtered and the solid was dried using a desiccator filled with P2O5. Light yellow crystals were obtained by sublimation at 60° C./0.05 Torr (1.120 g, 66%): mp 56° C.; IR (Nujol, cm−1) 3214 (m), 1559 (w), 1365 (m), 1300 (w), 1261 (w), 1229 (w) 1132 (w), 1038 (m), 1022 (m); 1H NMR (C6D6, 23° C., δ) 7.49 (d, 1H, (J=8.0 Hz), CH), 7.17 (d, 1H, (J=8.0 Hz), CH), 4.65 (s, broad 1H, NH), 2.47 (s, 6H, N(CH3)2), 1.14 (s, 9H, C(CH3)3); 13C{1H} NMR (100 MHz, benzene-d6, 23° C., ppm) 139.26 (s, CHN), 133.22 (s, CHN), 53.44 (s, C(CH3)3), 42.26 (s, N(CH3)2), 28.66 (s, C(CH3)3); ESI-HRMS: calcd for C8H19N4 ([M+H]+) 171.1610. found 171.1607.


Preparation of Bis(1,5-di-test-butyl-1,2,5-triazapentadienyl)nickel(II) (1)

A 100 mL Schlenk flask was charged with a magnetic stir bar, 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol), and tetrahydrofuran (30 mL). To this stirred solution at ambient temperature was slowly added potassium hydride (0.241 g, 6.00 mmol), and the solution was stirred for 4 h. This solution was then slowly added dropwise by cannula to a stirred suspension of anhydrous NiCl2.CH3CN (0.456 g, 2.70 mmol) in tetrahydrofuran (40 mL) at −78° C. The resultant dark brown solution was stirred for 15 h at ambient temperature. The volatile components were then removed under reduced pressure, and the resultant dark red powder was dissolved in hexane (60 mL). The solution was filtered through a 1 cm pad of Celite on a coarse glass frit, and the hexane was then removed under reduced pressure. Dark red crystals of 1 were obtained by sublimation at 155° C./0.05 Torr (0.397 g, 35%): mp 262° C.; IR (Nujol, cm−1) 1548 (m), 1365 (s), 1339 (m), 1253 (w), 1213 (m), 1174 (m), 1060 (w), 791 (w); 1H NMR (C6D6, 23° C., δ) 16.64 (s, broad 18H, C(CH3)3), 15.20 (s, broad 18H, C(CH3)3); μeff=2.84 and 2.86 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C20H40NiN6: C, 56.75; H, 9.53; N, 19.86. Found: C, 56.66; H, 9.49; N, 19.84.


Preparation of Bis(1,5-di-tert-butyl-1,2,5-triazapentadienyl)cobalt(II) (2)

In a fashion similar to the preparation of 1, treatment of anhydrous cobalt(II) chloride (0.350 g, 2.70 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1,5-di-tert-butyl-1,2,5-triazapentadienate (prepared from 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol) and potassium hydride (0.241 g, 6.00 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 2 (0.623 g, 57%) as dark green crystals upon sublimation at 160° C./0.05 Torr: mp 260° C.; IR (Nujol, cm−1) 1542 (s), 1364 (s), 1354 (s), 1340 (s), 1255 (m), 1214 (m), 1178 (s), 1054 (m), 996 (w), 790 (m); μeff=3.78 and 3.95 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C20H40CoN6: C, 56.72; H, 9.52; N, 19.84. Found: C, 56.59; H, 9.46; N, 19.79.


Preparation of Bis(1,5-di-test-butyl-1,2,5-triazapentadienyl)iron(II) (3)

In a fashion similar to the preparation of 1, treatment of anhydrous iron(II) chloride (0.342 g, 2.70 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1,5-di-tert-butyl-1,2,5-triazapentadienate (prepared from 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol) and potassium hydride (0.241 g, 6.00 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 3 (0.805 g, 73%) as dark red crystals upon sublimation at 175° C./0.05 Torr: mp 275° C.; IR (Nujol, cm−1) 1529 (s), 1362 (m), 1350 (m), 1336 (s), 1254 (m), 1242 (m), 1215 (m), 1176 (s), 1055 (m), 994 (m), 926 (m), 918 (m), 791 (m); μeff=5.00 and 4.92 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C20H40FeN6: C, 57.14; H, 9.59; N, 19.99. Found: C, 57.76; H, 9.29; N, 20.14.


Preparation of Bis(1,5-di-test-butyl-1,2,5-triazapentadienyl)manganese(II) (4)

In a fashion similar to the preparation of 1, treatment of anhydrous manganese(II) chloride (0.340 g, 2.70 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1,5-di-tert-butyl-1,2,5-triazapentadienate (prepared from 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol) and potassium hydride (0.241 g, 6.00 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 4 (0.597 g, 54%) as dark yellow crystals upon sublimation at 165° C./0.05 Torr: mp 284° C.; IR (Nujol, cm−1) 1552 (m), 1366 (m), 1346 (m), 1257 (m), 1176 (m), 1052 (w), 786 (w); μeff=5.89 and 5.85 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C20H40MnN6: C, 57.26; H, 9.61; N, 20.03. Found: C, 57.55; H, 9.50; N, 20.12.


Preparation of Bis(1,5-di-test-butyl-1,2,5-triazapentadienyl)chromium(II) (5)

In a fashion similar to the preparation of 1, treatment of anhydrous chromium(II) chloride (0.332 g, 2.70 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1,5-di-tert-butyl-1,2,5-triazapentadienate (prepared from 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol) and potassium hydride (0.241 g, 6.00 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 5 (0.602 g, 55%) as brown crystals upon sublimation at 165° C./0.05 Torn mp 257° C.; IR (Nujol, cm−1) 1500 (w), 1366 (m), 1351 (m), 1334 (m), 1313 (w), 1266 (s), 1231 (w), 1211 (w), 1179 (s), 1143 (m), 1135 (m), 1046 (m), 967 (s), 792 (m); μeff=4.85 and 4.96 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C20H40CrN6: C, 57.67; H, 9.68; N, 20.17. Found: C, 57.98; H, 9.48; N, 20.19.


Preparation of Bis(1,5-di-test-butyl-1,2,5-triazapentadienyl)magnesium(II) (6)

In a fashion similar to the preparation of 1, treatment of anhydrous magnesium(II) bromide (0.497 g, 2.70 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1,5-di-tert-butyl-1,2,5-triazapentadienate (prepared from 1,5-di-tert-butyl-1,2,5-triazapentadiene (1.000 g, 5.45 mmol) and potassium hydride (0.241 g, 6.00 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 6 (0.886 g, 81%) as yellow crystals upon sublimation at 165° C./0.05 Torr: mp 268° C.; IR (Nujol, cm−1) 1500 (w), 1366 (m), 1351 (m), 1334 (m), 1313 (w), 1266 (s), 1231 (w), 1211 (w), 1179 (s), 1143 (m), 1135 (m), 1046 (m), 967 (s), 792 (m); 1H NMR (C6D6, 23° C., δ) 6.87 (d, (J=4.4 Hz), 1H, CHN), 6.77 (d, (J=4.4 Hz), 1H, CHN), 1.45 (s, 18H, C(CH3)3), 1.06 (s, 18H, C(CH3)3); Anal. Calcd for C20H40MgN6: C, 61.77; H, 10.37; N, 21.61. Found: C, 61.92; H, 10.33; N, 21.76.


Preparation of Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)nickel(II) (7)

In a fashion similar to the preparation of 1, treatment of anhydrous NiCl2.CH3CN (0.490 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienate (prepared from 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene (1.000 g, 5.90 mmol) and potassium hydride (0.259 g, 6.50 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 7 (0.267 g, 23%) as dark red crystals upon sublimation at 105° C./0.05 Torr: mp 99° C.; IR (Nujol, cm−1) 1535 (w), 1366 (m), 1351 (m), 1317 (m), 1255 (m), 1195 (m), 1174 (m), 1055 (m), 1037 (m), 961 (m), 792 (m); 1H NMR (C6D6, 23° C., δ) 32.57 (s, broad 12H, N(CH3)2), 16.53 (s, broad 18H, C(CH3)3); μaff=2.86 and 2.85 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C16H34NiN8: C, 48.38; H, 8.63; N, 28.21. Found: C, 48.27; H, 8.53; N, 28.23.


Preparation of Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)cobalt(II) (8)

In a fashion similar to the preparation of 1, treatment of anhydrous cobalt(II) chloride (0.376 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienate (prepared from 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene (1.000 g, 5.90 mmol) and potassium hydride (0.259 g, 6.50 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 8 (0.301 g, 27%) as dark green crystals upon sublimation at 105° C./0.05 Torr: mp 105° C.; IR (Nujol, cm−1) 1529 (m), 1366 (m), 1352 (s), 1316 (m), 1256 (m), 1235 (m), 1216 (m), 1198 (m), 1178 (m), 1051 (m), 1029 (m), 963 (m), 789 (m), 779 (m); μeff=3.92 and 3.95 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C16H34CoN8: C, 48.35; H, 8.62; N, 28.19. Found: C, 48.24; H, 8.66; N, 28.14.


Preparation of Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)iron(II) (9)

In a fashion similar to the preparation of 1, treatment of anhydrous iron(II) chloride (0.374 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienate (prepared from 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene (1.000 g, 5.90 mmol) and potassium hydride (0.259 g, 6.50 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 9 (0.190 g, 18%) as dark green crystals upon sublimation at 105° C./0.05 Torr: mp 106° C.; IR (Nujol, cm−1) 1515 (w), 1368 (m), 1351 (m), 1312 (w), 1258 (w), 1196 (w), 1176 (w), 1026 (w), 794 (w); μeff=4.78 and 4.82 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C16H34FeN8: C, 48.73; H, 8.69; N, 28.42. Found: C, 49.05; H, 8.72; N, 28.10.


Preparation of Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)manganese(II) (10)

In a fashion similar to the preparation of 1, treatment of anhydrous manganese(II) chloride (0.371 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienate (prepared from 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene (1.000 g, 5.90 mmol) and potassium hydride (0.259 g, 6.50 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 10 (0.350 g, 32%) as dark orange crystals upon sublimation at 105° C./0.05 Torr: mp 108° C.; IR (Nujol, cm−1) 1539 (m), 1357 (m), 1323 (m), 1256 (m), 1196 (m), 1186 (m), 1152 (w), 1048 (m), 957 (w), 1021 (m), 786 (w), 730 (w); μeff=5.80 and 5.82 μB in the solid state and in benzene solution, respectively. Anal. Calcd for C16H34MnN8: C, 48.84; H, 8.71; N, 28.48. Found: C, 48.86; H, 8.78; N, 28.32.


Preparation of Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)magnesium(II) (11)

In a fashion similar to the preparation of 1, treatment of anhydrous magnesium(II) bromide (0.543 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienate (prepared from 1-tert-butyl-5-dimethylamino-1,2,5-triazapentadiene (1.000 g, 5.90 mmol) and potassium hydride (0.259 g, 6.50 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 11 (0.689 g, 63%) as yellow crystals upon sublimation at 165° C./0.05 Torr: mp 113° C.; IR (Nujol, cm−1) 1529 (m), 1366 (m), 1352 (s), 1316 (m), 1256 (m), 1235 (m), 1216 (m), 1198 (m), 1178 (m), 1051 (m), 1029 (m), 963 (m), 789 (m), 779 (m); 1H NMR (C6D6, 23° C., δ) 6.73 (d, (J=4.4 Hz), 1H, CHN), 6.71 (d, (J=4.4 Hz), 1H, CHN), 2.31 (s, 18H, C(CH3)3), 1.45 (s, 18H, C(CH3)3); Anal. Calcd for C16H34MgN8: C, 52.97; H, 9.45; N, 30.89. Found: C, 52.82; H, 9.66; N, 30.83.


The following reaction scheme shows the synthesis of bis(1,2,5-triazapentadienyl) transition metal complexes.




embedded image









TABLE 1







Thermal properties of the complexes













Sublimation

Solid state





temperature
Melting
decomposition
%
% Non volatile


Complex
(° C./0.05 Torr)
point (° C.)
temperature (° C.)
Recovery
residue















1
175
255-257
280
97
3


2
165
282-284
310
97
2


3
175
273-275
310
98
<1


4
160
258-260
296
98
1


5
155
260-262
290
98
1


6
165
268-270
290
96
3


7
105
106-108
200
95
4


8
105
104-106
181
93
5


9
105
103-105
225
94
5


10
105
97-99
188
95
4


11
105
113-114
180
95
3










FIG. 3 provides TGA curves for compounds 1-5 and FIG. 3 provides TGA curves for compounds 7-10.


Solution phase reactivity.


To assess initial viability for use in ALD film growth, 10 (Bis(1-tert-butyl-5-dimethylamino-1,2,5-triazapentadienyl)nickel(II)) was treated with anhydrous hydrazine in tetrahydrofuran at 23° C. A metallic black precipitate was observed within 0.25 h. The precipitate stuck to the magnetic stir bar and a powder X-ray diffraction spectrum indicated the formation of nickel metal (FIG. 5).


Experimental Section 2

General Considerations.


All manipulations were carried out under argon using either Schlenk or glove box techniques, except the ligands were prepared in ambient atmosphere. Tetrahydrofuran was distilled from sodium benzophenone ketyl, hexane was distilled from P2O5. Anhydrous transition-metal chlorides (CuCl2, NiCl2, CoCl2, FeCl2, MnCl2 and CrCl2) were obtained from Strem Chemicals Inc. and used as received. NiCl2.CH3CN was prepared according to a literature procedure.1 Potassium hydride (30 wt % dispersion in mineral oil; washed with hexane before use), was purchased from Sigma-Aldrich. 3-Methylbutanal, and tert-butyl amine were purchased from across organics. SeO2 and pinacolone were purchased from Alfa Aesar.



1H and 13C{1H} NMR spectra were obtained at 400 and 100 MHz, respectively, in benzene-d6 or chloroform-d as indicated and were referenced to the residual proton and the 13C resonances of the solvents. Infrared spectra were obtained using Nujol as the medium. Magnetic moments were determined in the solid state using a Johnson Mathey magnetic susceptibility apparatus, and by, 1H NMR in benzene solution using Evans method.2 Melting points were determined on a Thermo Scientific Mel-Temp 3.0 digital melting point apparatus and are uncorrected. TGA and DTA were carried out with a SDT-2960 TGA/DTA instruments.


Preparation of 1-(tert-butylimino)-3-methylbutan-2-one

Isopropyl glyoxal[3-methyl-2-oxobutanal] was prepared using 3-methylbutanal and SeO2 according to a published procedure.5 A 100 mL round-bottomed flask was charged with a magnetic stir bar, 3-methyl-2-oxobutanal (1.000 g, 9.99 mmol) and diethyl ether (15 mL). To this stirred solution at ambient temperature was slowly added tert-butyl amine (1.059 g, 9.99 mmol). This solution was stirred for 6 h. The resultant yellow solution was washed with water (10 ml) and the organic layer was dried over anhydrous Na2SO4. The volatile components were removed by vacuum and resultant yellow oil was vacuum distilled. A light yellow oil was obtained at 60° C./0.05 Torr (1.147 g, 74%): IR (Nujol, cm−1) 1697 (s), 1638 (m), 1383 (s), 1365 (s), 1347 (s), 1213 (s), 1191 (s), 1149 (s), 1087 (s), 1027 (m), 949 (s), 902 (s), 644 (m); 1H NMR (CDCl3, 23° C., δ) 7.48 (s, 1H, CHN), 3.57 (sep, 1H, (J=7.2), CH(CH3)2), 1.19 (s, 9H, C(CH3)3), 1.04 (d, 6H, (J=7.2), CH(CH3)2); 13C{1H} NMR(CDCl3, 23° C., ppm) 206.33 (s, CO), 118.93 (s, CHN), 58.40 (s, C(CH3)3), 33.92 (s, CH(CH3)2), 28.96 (s, C(CH3)3), 18.25 (s, CH(CH3)2).


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)chromium(II) (12)

A 100 mL Schlenk flask was charged with a magnetic stir bar, 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and tetrahydrofuran (30 mL). To this stirred solution at ambient temperature was slowly added potassium hydride (0.284 g, 7.08 mmol), and solution was stirred for 4 hours. This solution was then slowly added dropwise by cannula to a stirred suspension of anhydrous chromium(II) chloride (0.393 g, 3.22 mmol) in tetrahydrofuran (40 mL) at −78° C. The resultant dark green solution was stirred for 15 hours at ambient temperature. The volatile components were then removed under reduced pressure, and the resultant dark green powder was dissolved in hexane (50 mL). The solution was filtered through a 1 cm pad of Celite on a coarse glass frit, and hexane was then removed under reduced pressure. Dark green crystals of 12 (0.115 g, 10%) were obtained by sublimation at 120° C./0.05 Torr: mp 150-152° C.; IR (Nujol, cm−1) 1601 (m), 1580 (w), 1360 (m), 1352 (m), 1305 (m), 1215 (m), 971 (w); μeff=4.80 and 4.98 μB in the solid state and in benzene solution, respectively Anal. Calcd for C18H32CrN2O2: C, 59.98; H, 8.95; N, 7.77. Found: C, 59.81; H, 8.86; N, 7.66.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)manganese(II) (13)

In a fashion similar to the preparation of 12, treatment of anhydrous manganese(II) chloride (0.403 g, 3.22 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-(tert-butylimino)-3-methylbutan-2-olate (prepared from 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and KH (0.284 g, 7.08 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 13 (0.429 g, 37%) as orange crystals upon sublimation at 165° C./0.05 Torr: mp 193-195° C.; IR (Nujol, cm−1) 1609 (m), 1594 (m), 1365 (m), 1349 (m), 1310 (m), 1291 (m), 1218 (m), 1202 (m), 1031 (w), 956 (m), 798 (w); μeff=8.45 and 7.89μB in the solid state and in benzene solution, respectively Anal. Calcd for C18H32MnN2O2: C, 59.49; H, 8.88; N, 7.71. Found: C, 59.39; H, 8.78; N, 7.64.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)iron(II) (14)

In a fashion similar to the preparation of 12, treatment of anhydrous iron(II) chloride (0.414 g, 3.22 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-(tert-butylimino)-3-methylbutan-2-olate (prepared from 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and KH (0.284 g, 7.08 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 14 (0.562 g, 49%) as dark red crystals upon sublimation at 155° C./0.05 Torr: mp 160-162° C.; IR (Nujol, cm−1) 1600 (w), 1595 (w), 1350 (w), 1358 (m), 1300 (m), 1260 (m), 1090 (m), 1020 (m), 799 (m); μeff=7.21 and 6.72μB in the solid state and in benzene solution, respectively Anal. Calcd for C18H32FeN2O2: C, 59.34; H, 8.85; N, 7.69. Found: C, 59.34; H, 8.76; N, 7.79.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)cobalt(II) (15)

In a fashion similar to the preparation of 12, treatment of anhydrous cobalt(II) chloride (0.418 g, 3.22 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-(tert-butylimino)-3-methylbutan-2-olate (prepared from 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and KH (0.284 g, 7.08 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 15 (0.933 g, 80%) as dark red crystals upon sublimation at 135° C./0.05 Torr: mp 166-168° C.; IR (Nujol, cm−1) 1605 (m), 1588 (m), 1365 (m), 1348 (m), 1307 (m), 1290 (m), 1203 (m), 964 (m), 799 (m); μeff=6.83 and 7.01 μB in the solid state and in benzene solution, respectively Anal. Calcd for C18H32CoN2O2: C, 58.85; H, 8.79; N, 7.62. Found: C, 59.02; H, 8.81; N, 7.67.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)nickel(II) (16)

In a fashion similar to the preparation of 12, treatment of anhydrous NiCl2.CH3CN (0.540 g, 3.22 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-(tert-butylimino)-3-methylbutan-2-olate (prepared from 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and KH (0.284 g, 7.08 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 16 (0.767 g, 66%) as pale green crystals upon sublimation at 120° C./0.05 Torr: mp 166-168° C.; IR (Nujol, cm−1) 1607 (w), 1574 (m), 1358 (m), 1351 (m), 1299 (m), 1213 (m), 978 (w), 799 (w); 1H NMR (C6D6, 23° C., δ) 7.94 (s, 1H, CHN), 2.48 (s, 6H, C(CH3)2), 2.31 (s, 6H, C(CH3)2), 1.35 (s, 18H, C(CH3)3); 13C{1H} NMR(C6D6, 23° C., ppm) 156.31 (s, CN), 150.64 (s, C(CH3)2), 126.95 (s, CO), 61.42 (s, C(CH3)3), 30.29 (s, C(CH3)2), 18.05 (s, C(CH3)3), 17.61 (s, C(CH3)2); Anal. Calcd for C18H32NiN2O2: C, 58.88; H, 8.78; N, 7.63. Found: C, 58.97; H, 8.89; N, 7.61.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)copper(II) (17)

In a fashion similar to the preparation of 12, treatment of anhydrous copper(II) chloride (0.430 g, 3.22 mmol) in tetrahydrofuran (40 mL) with a solution of potassium 1-(tert-butylimino)-3-methylbutan-2-olate (prepared from 1-(tert-butylimino)-3-methylbutan-2-one (1.000 g, 6.44 mmol) and potassium hydride (0.284 g, 7.08 mmol) in tetrahydrofuran (30 mL)) for 15 hours at ambient temperature afforded 17 (0.505 g, 43%) as brown crystals upon sublimation at 110° C./0.05 Torr: mp 135-138° C.; IR (Nujol, cm−1) 1607 (m), 1586 (s), 1365 (m), 1350 (m), 1300 (s), 1239 (m), 1214 (s), 1126 (m), 1035 (m), 971 (m), 675 (m); μeff=1.88 and 1.80μ13 in the solid state and in benzene solution, respectively Anal. Calcd for C18H32CuN2O2: C, 58.12; H, 8.67; N, 7.53. Found: C, 58.33; H, 8.76; N, 7.58.


Preparation of Bis(1-(test-butylimino)-3,3-dimethylbutan-2-oyl)chromium(II) (18)

In a fashion similar to the preparation of 12, treatment of anhydrous chromium(II) chloride (0.362 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of the lithium radical anion of 1-(tert-butylimino)-3,3-dimethylbutan-2-oyl (prepared from 1-(tert-butylimino)-3,3-dimethylbutan-2-one (1.000 g, 5.91 mmol) and lithium metal (0.045 g, 6.49 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 18 (0.056 g, 5%) as brown crystals upon sublimation at 135° C./0.05 Torr: mp 248-250° C.; IR (Nujol, cm−1) 1623 (w), 1489 (m), 1413 (w), 1367 (m), 1358 (m), 1341 (m), 1262 (w), 1200 (m), 1164 (m), 1062 (w), 984 (w).


Preparation of Bis(1-(tert-butylimino)-3,3-dimethylbutan-2-oyl)manganese(II) (19)

In a fashion similar to the preparation of 12, treatment of anhydrous manganese(II) chloride (0.365 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of the lithium radical anion of 1-(tert-butylimino)-3,3-dimethylbutan-2-oyl (prepared from 1-(tert-butylimino)-3,3-dimethylbutan-2-one (1.000 g, 5.91 mmol) and lithium metal (0.045 g, 6.49 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 19 (0.407 g, 37%) as dark orange crystals upon sublimation at 145° C./0.05 Torr: mp 175-177° C.; IR (Nujol, cm−1) 1650 (w), 1360 (m), 1344 (m), 1262 (w), 1211 (w), 1153 (w); μeff=5.96 and 5.86 μB in the solid state and in benzene solution, respectively Anal. Calcd for C40H78Mn2N4O4: C, 60.89; H, 9.97; N, 7.10. Found: C, 60.92; H, 10.04; N, 6.84.


Preparation of Bis(1-(tert-butylimino)-3,3-dimethylbutan-2-oyl)iron(II) (20)

In a fashion similar to the preparation of 12, treatment of anhydrous iron(II) chloride (0.381 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of the lithium radical anion of 1-(tert-butylimino)-3,3-dimethylbutan-2-oyl (prepared from 1-(tert-butylimino)-3,3-dimethylbutan-2-one (1.000 g, 5.91 mmol) and lithium metal (0.045 g, 6.49 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 20 (0.210 g, 18%) as dark green crystals upon sublimation at 140° C./0.05 Torr: mp 143-145° C.; IR (Nujol, cm−1) 1650 (m), 1365 (m), 1263 (w), 1214 (m), 1156 (w), 1125 (w), 1022 (w), 800 (w); μeff=4.82 and 4.74 μB in the solid state and in benzene solution, respectively Anal. Calcd for C40H77Fe2N4O4: C, 60.83; H, 9.83; N, 7.09. Found: C, 60.74; H, 9.60; N, 7.22.


Preparation of Bis(1-(tert-butylimino)-3,3-dimethylbutan-2-oyl)cobalt(II) (21)

In a fashion similar to the preparation of 12, treatment of anhydrous cobalt(II) chloride (0.383 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of the lithium radical anion of 1-(tert-butylimino)-3,3-dimethylbutan-2-oyl (prepared from 1-(tert-butylimino)-3,3-dimethylbutan-2-one (1.000 g, 5.91 mmol) and lithium metal (0.045 g, 6.49 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 21 (0.869 g, 79%) as dark red crystals upon sublimation at 135° C./0.05 Torr: mp 194-196° C.; IR (Nujol, cm−1) 1626 (w), 1482 (m), 1407 (m), 1332 (m), 1265 (w), 1216 (m), 1156 (m), 992 (w), 815 (w); μeff=1.79 and 1.73 μB in the solid state and in benzene solution, respectively Anal. Calcd for C20H38CoN2O2: C, 60.44; H, 9.64; N, 7.05. Found: C, 60.42; H, 9.48; N, 7.07.


Preparation of Bis(1-(tert-butylimino)-3-methylbut-2-en-2-olate)nickel (II) (22)

In a fashion similar to the preparation of 12, treatment of anhydrous NiCl2.CH3CN (0.498 g, 2.95 mmol) in tetrahydrofuran (40 mL) with a solution of the lithium radical anion of 1-(tert-butylimino)-3,3-dimethylbutan-2-oyl (prepared from 1-(tert-butylimino)-3,3-dimethylbutan-2-one (1.000 g, 5.91 mmol) and lithium metal (0.045 g, 6.49 mmol) in tetrahydrofuran (30 mL)) for 15 h at ambient temperature afforded 22 (0.340 g, 30%) as red crystals upon sublimation at 135° C./0.05 Torr: mp 181-183° C.; IR (Nujol, cm−1) 1633 (w), 1484 (m), 1407 (m), 1358 (s), 1264 (m), 1218 (m), 1158 (m), 991 (m), 887 (m), 818 (m), 761 (m), 621 (m); 1H NMR (C6D6, 23° C., δ) 9.93 (s, 1H, CHN), 2.27 (s, 9H, C(CH3)3), 0.70 (s, 9H, C(CH3)3); 13C{1H} NMR(C6D6, 23° C., ppm) 148.50 (s, CO), 132.07 (s, CN), 73.63 (s, C(CH3)3), 54.56 (s, C(CH3)3), 23.26 (s, C(CH3)2), 15.30 (s, C(CH3)3); Anal. Calcd for C20H38NiN2O2: C, 60.47; H, 9.64; N, 7.05. Found: C, 59.95; H, 9.38; N, 7.06.


The following reaction scheme shows the synthesis of bis(1-(tert-butylimino)-3-methylbutan-2-olate) transition metal complexes.




embedded image









TABLE 2







Thermal properties of 12-17.














Isolated


Solid state





yield by
Sublimation

decomposition

% Non



sublimation
temperature
Melting
temperature
%
volatile


Compound
(%)
(° C./0.05 Torr)
point (° C.)
(° C.)
Recovery
residue
















12
10
120
150-152
220
96
3


13
37
165
193-195
295
97
2


14
49
155
160-162
262
97
2


15
80
135
166-168
276
98
<1


16
66
120
166-168
260
97
2


17
43
110
135-138
190
97
2









The following reaction scheme shows the synthesis of bis(1-(tert-butylimino)-3,3-dimethylbutan-2-oyl) transition metal complexes.




embedded image









TABLE 3







Thermal properties of 18-22.














Isolated yield








by
Sublimation
Melting
Solid state

% Non-



sublimation
temperature
point
decomposition
%
volatile


Compound
(%)
(° C./0.05 Torr)
(° C.)
temperature (° C.)
Recovery
residues
















18
5
135
248-250
250
90
7


19
37
145
175-177
245
91
6


20
18
140
143-145
241
90
8


21
79
135
194-196
235
93
6


22
30
135
181-183
180
90
5










FIG. 6 provides TGA traces of compounds 18-20, and 22.


Solution Phase Reactivity.


In order to get some insight into reactivity of these precursors, 15-17 were treated with reducing co-reagents. In these reactions, a solution of 15-17 in tetrahydrofuran was treated with 5-times molar excess of NH2NH2 and BH3(NHMe2) in separate flasks. Reactions that did not afford a black powder or black solution at ambient temperature within one hour were then refluxed for one hour. Results are summarized in Table 4. Treatment of 17 with NH2NH2 and BH3(NHMe2) afforded a copper colored powder which gave reflections for copper metal in X-ray powder diffraction (FIG. 7). Additionally, 16 reacted with both reducing agents at ambient temperature to afford nickel metal which was confirmed by X-ray powder diffraction (FIG. 8). Moreover, 15 reacted with BH3(NHMe2) at ambient temperature and gave a black precipitate which stuck to stir bar, suggesting the formation of cobalt metal. However, X-ray powder diffraction did not show reflections. Treatment of 15 with NH2NH2 did not afford a black solution or black precipitate either at ambient temperature or reflux condition.









TABLE 4







Reactivity of 15-17 toward reducing agents in tetrahydrofuran.










Reducing agent
(CoL2)2 (15)
NiL2 (16)
CuL2 (17)





NH2NH2
No change
metallic mirror on
copper colored




the flask wall
powder


BH3(NHMe2)
Black powder;
black powder; sticks
copper colored



sticks to
to stir bar
powder



stir bar









While embodiments of the invention have been illustrated and described, it is not intended that these embodiments illustrate and describe all possible forms of the invention. Rather, the words used in the specification are words of description rather than limitation, and it is understood that various changes may be made without departing from the spirit and scope of the invention.


REFERENCES



  • Reedijk, J.; Groeneveld, W. L. Rect. Tray. Chim. Pays-Bas 1968, 87, 552.

  • Evans, D. F. J. Chem. Soc. 1959, 2003.

  • McNab, H. J. Chem. Soc., Perkin Trans. 2 1981, 1283.

  • Severin, T.; Poehlmann, H. Chem. Ber. 1977, 110, 491.

  • Kwiatowski, P.; Chaladaj, W.; Jurczak, J. Tetrahedron 2006, 62, 5116-5125.


Claims
  • 1. A compound having formula (I):
  • 2. The compound of claim 1 wherein M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu.
  • 3. The compound of claim 1 wherein R2 is t-butyl.
  • 4. The compound of claim 1 wherein when R1 is C1-8 alkyl, M is Zn, Mg, Cr, Mn, Fe, Co, or Ni, and when R1 is NR5R6, M is Zn, Mg, Mn, Fe, Co, or Ni.
  • 5. The compound of claim 1 wherein R1 is C1-8 alkyl and M is Zn, Mg, Cr, Mn, Fe, Co, or Ni.
  • 6. The compound of claim 1 wherein R1 is NR5R6 and M is Zn, Mg, Mn, Fe, Co, or Ni.
  • 7. The compound of claim 1 wherein R1 is C1-8 alkyl.
  • 8. The compound of claim 1 wherein R1 is methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, t-butyl, or phenyl.
  • 9. The compound of claim 1 wherein R1 is t-butyl or N(CH3)2.
  • 10. A compound having formula 2:
  • 11. The compound of claim 10 wherein M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu.
  • 12. The compound of claim 10 wherein R7, R8, R9, R10 are each independently C1-8 alkyl.
  • 13. The compound of claim 10 wherein R10 is t-butyl.
  • 14. A compound having formula (3):
  • 15. The compound of claim 14 wherein M is Zn, Mg, Cr, Mn, Fe, Co, Ni, or Cu.
  • 16. A method comprising: a) reacting a compound having bidentate ligands with an reactive compound to form a first product, the first compound selected from the group consisting of:
  • 17. The method of claim 16 wherein M is Zn, Mg, Cr, Mn, Fe, Co, or Ni.
  • 18. The method of claim 16 wherein the activating compound is an oxidizing agent and the first product includes a metal oxide.
  • 19. The method of claim 16 wherein the activating compound is a reducing agent and the first product includes a metal in the zero oxidation state.
  • 20. The method of claim 16 wherein the activating compound is a nitriding agent and the first product includes a metal nitride.
  • 21. The method of claim 16 comprising a deposition cycle including: a) contacting a substrate with a vapor of the first compound form a first modified surface; andc) contacting the substrate with the reactive compound.
  • 22. The method of claim 21 wherein a metal-containing layer is deposited on the substrate.
  • 23. The method of claim 21 further comprising contacting the first modified surface with an acid.
  • 24. The method of claim 16 wherein the metal-containing layer includes a component selected from the group consisting of metals in the zero oxidation state, metal nitrides, metal oxides, and combinations thereof.
CROSS-REFERENCE TO RELATED APPLICATION

This application claims the benefit of U.S. provisional application Ser. No. 61/658,064 filed Jun. 11, 2012, the disclosure of which is incorporated in its entirety by reference herein.

PCT Information
Filing Document Filing Date Country Kind
PCT/US2013/045144 6/11/2013 WO 00
Provisional Applications (1)
Number Date Country
61658064 Jun 2012 US