The present invention relates generally to the field of processes for making metal films and structures and articles of manufacture comprising such films. More particularly, the invention relates to methods for growing conformal metal sulfide films on nanostructures using atomic layer deposition and the resulting structures that may be used in various applications, including a photovoltaic device.
This section is intended to provide a background or context to the invention that is, inter alia, recited in the claims. Unless otherwise indicated herein, what is described in this section is not prior art to the description and claims in this application and is not admitted to be prior art by inclusion in this section.
There is a need to provide clean, safe, and sustainable energy to supply the growing global demand for energy. In contrast to other renewable resources whose globally extractable power is each less than 5 TW, the solar constant upon the earth's surface (120,000 TW) will exceed worldwide energy demand into the foreseeable future. This abundant supply of sunlight and the environmental friendliness of solar energy make the efficient conversion of solar radiation into electricity a compelling economic and scientific goal.
Photovoltaic (PV) devices that covert solar energy to electricity have been in use for several decades. However, widespread adoption of PV devices has been somewhat limited by their expense and inefficiency relative to other sources of energy. Advances in structures and materials are important to achieving widespread adoption of effective PV devices. The most desirable materials for use in PV, applications are both inexpensive and abundant. In general, however, these materials have high impurity and defect concentrations, both of which limit the diffusion length of charge carriers which is a critical performance parameter of PV devices. The reduced length over which charges may be extracted (LCE) effectively limits the useful thickness of the active layer, as thicker layers will not increase device efficiency. For example, the efficiency of silicon PV devices scale with semiconductor quality as the LCE approaches the active layer thickness required to collect 90% of incident photons (LOD). Decoupling these two important parameters has recently been recognized in several PV fields, including polymer and Si p-n junctions. The initial experimental results in this direction are modest, owing to the complexity of fabricating such sophisticated geometries.
Structural improvements in PV devices has opened the door to the use of new, less expensive materials that often possess highly desirable characteristics. To this end, there has been interest in using certain transition metal compounds, including copper compounds, among others. For example, various attempts using Cu2S in PV devices have been made. The first thin film. PV devices comprised CdS/Cu2S heterojunctions formed through the topotaxial exchange of Cd atoms on a CdS surface for Cu+ ions in solution. Interest in the technology waned in the late 1980s, however, in light of the instability of the heterojunction through which Cu+ ions are prone to diffuse. In its place, the more costly ternary chalcogenide chalcopyrites (CuMX2) [M=In, Ga; X═S, Se] have been developed, with power efficiencies now approaching 20%.
More recently, it has been shown that it is feasible to form stable p/n heterojuctions with CuxS paired with an alternative n-type semiconductor, TiO2. As cation exchange is not possible in these Cd-free PVs, alternative deposition methods for CuxS are required. More specifically, chalcocite (CuxS, x˜2) is favored for PV applications among a sizeable number of copper-poor polymorphs (CuxS, 2≧x≧1.75) as it offers the largest spectral coverage and most appropriate conductivity. In addition to traditional topotaxial growth, previous routes to phase-pure chalcocite include single-source evaporation and reactive sputtering. Techniques using nanoparticle syntheses and aerosol assisted chemical vapor deposition (AACVD, a liquid precursor delivery technique akin to spray pyrolysis) have also been attempted.
Atomic layer deposition (ALD) is one technique for producing thin, conformal layers. The ALD of Cu2S has also been attempted by alternating exposure to Cu(thd)2 (thd=thd-2,2,6,6-tetramethyl-3,5-heptanedione) and H2S. However, existing methods for formation of Cu2S ALD are not adequate. For example, over the range of temperatures in which the deposition is self-limiting, the growth rate is slow, not exceeding 0.4 Å/cycle. Notably, only the less desirable CuS (covellite) and/or Cu1.8S (digenite) phases are obtained using this approach. Additionally, thermal decomposition of the Cu(thd)z precursor limits the ability to coat nanoporous supports desirable in advanced PV devices. CuCl2 can also be used, but this requires excessively high temperatures, and the HCl byproduct can result in etching of the films and the deposition equipment. Thus, a substantially pure (and highly desirable) chalcocite phase has not been achieved with these precursors.
In a PV device, the reduced length over which charges may be extracted (LCE) effectively limits the useful thickness of the active layer. The efficiency of PVs scale with semiconductor quality as the LCE approaches the active layer thickness required to collected 90% of incident photons (LOD). Surmounting the incongruity between LOD and LCE in inexpensive materials may be accomplished by decoupling light absorption and carrier extraction into orthogonal spatial dimensions. For example, a PV device may be prepared where the planar junction is effectively folded to form a nanorod array. The interdigitation of not only the active layers, but also two transparent conducting oxide (TCO) electrodes allow for radial charge collection in the PV device. The result is a PV device where the total device thickness may be tuned for sufficient light absorption independent of the active layer thickness, which may be chosen to be equal to LCE. Thus, the device allows for efficient charge collection throughout the optically dense PV device, independent of the diffusion length (i.e. quality) or absorptivity of the material employed.
This invention comprises improved methods for preparing thin films of metal sulfide materials and resulting structures and articles of manufacture. The invention may be particularly applicable for producing thin films of metal sulfides (e.g., copper sulfide, Cu2S, InzSy) for use as the light absorbing layer in solar cells. The methods may also be used in forming mixed metal sulfides (e.g., CuInSy). These methods provide techniques for producing various metal sulfides in the form of thin, conformal layers on nanoporous supports as applicable to preparing solar cells, including interdigitated PV devices.
With regard to Cu2S, a true gas phase chemical vapor deposition route to high quality chalcocite films has been elusive. Importantly, a conformal (not line-of-sight) growth method compatible with nanoscale structuring is needed to diminish the discrepancy between the minority carrier diffusion length (20-240 nm) and the thickness necessary (>1 μm) for ample light harvesting in the near IR spectrum. Decoupling light absorption and carrier extraction into orthogonal spatial dimensions through use of high-aspect ratio architectures may diminish this incongruity. An ALD process may be used to prepare, for example, a copper sulfide (Cu2S) film, on a high-aspect ratio substrate. Thus, through ALD and/or additional further processes a relatively efficient and low cost interdigitated PV device may be prepared.
Various ALD precursors may be used to prepare metal and mixed metal sulfide films on a substrate, including an interdigitated PV device. For example, a Cu2S film may be prepared by ALD using a non-halogenated precursor that is sufficiently reactive at lower temperatures. In one embodiment, Bis(N,N′-di-sec-butylacetamidinato)dicopper(I), (Cu(DSB)2), along with hydrogen sulfide (H2S) precursors may be used to prepare a Cu2S film by ALD. Additionally, a cyclopentadienyl indium (InCp) precursor and a H2S precursor may be used to prepare a film of In2S3 by ALD. InCp shares many of the same advantages as the Cu(DSB)2, namely lower deposition temperatures and an absence of problems associated with halogenated byproducts. Multiple metal precursors may be used to form ALD mixed Metal sulfide films. For example, a copper indium sulfide (CuInS2) film may be prepared by applying the Cu2S and the In2S3 ALD precursors. These improved methods for depositing metal sulfide layers on a substrate will facilitate the manufacturing of interdigitated photovoltaic devices. Additionally, capitalizing on these advances in ALD and PV technology, new avenues in selective contacts, tandem PV and devices capable of water splitting all will become feasible.
In one embodiment, a method for preparing a portion of an interdigitated photovoltaic device is provided. The method comprises providing an atomic layer deposition (ALD) reactor, a high-aspect ratio substrate, a first precursor and a second precursor. The first precursor comprises at least one metal and the second precursor comprises a sulfur compound. The method further comprises exposing the high-aspect ratio substrate to the first precursor for a first period and exposing the high-aspect ratio substrate to the second precursor for a second period. The cycle of exposing the substrate to the first and the second precursors is repeated for a number of cycles until a metal sulfide film of a desired thickness is formed on the high-aspect ratio substrate.
In another embodiment, a method for preparing a Cu2S film on a substrate is provided. The method comprises providing an ALD reactor, a substrate, a first precursor and a second precursor. The first precursor comprises copper and the second precursor comprises H2S. The method further comprises heating the substrate to a reaction temperature, exposing the substrate to the first precursor for a first predetermined duration and exposing the substrate to the second precursor for a second predetermined duration. The exposure of the substrate to first precursor and the second precursor is repeated for a predetermined number of cycles to form a Cu2S film on the substrate.
In still another embodiment, an interdigitated photovoltaic structure is provided. The structure comprises at least one transparent oxide conductor (TCO) electrode and an interfacial active layer coupled to the at least one TCO electrode. The interfacial active layer includes a first film coupled to a second film. The first film comprises a metal sulfide film. The at least one TCO electrode and the interfacial active layer are arranged to comprise a three dimensional nano-scale structure configured for substantially radial charge collection in response to incident light.
These and other advantages and features of the invention, together with the organization and manner of operation thereof, will become apparent from the following detailed description when taken in conjunction with the accompanying drawings, wherein like elements have like numerals throughout the several drawings described below.
The atomic layer deposition (ALD) process permits preparation of custom films with desired characteristics with nanoscale precision. Various interdigitated structures may be formed to optimize solar collection and charge production.
The interdigitated PV device 10 may further include a base substrate 110. In various embodiments the base substrate 100 may comprise metal, glass, fused silica or other appropriate material based on the application of the device. The interdigitated PV device 10 may also include a template 150 coupled to the second TCO electrode 140. In various embodiments, the template 150 may comprise anodic aluminum, a glass capillary membrane or other suitable material to increase light harvesting efficiency without loss of charge extraction efficiency.
Additional layers, above or below the metal sulfide film, may further be included. These layers may be prepared using ALD, other deposition techniques, or otherwise incorporated into a multilayer structure comprising the metal sulfide film. Additional metal sulfide films may also be deposited within the multilayer structure.
The architecture of the interdigitated PV as described above makes feasible the use of relatively inexpensive and abundant materials in the PV device. For example, CuInS2 in a PV device may be replaced with Cu2S, which is effective in view of the relaxed LCE requirements of the architecture. Through ALD, nanoscale fabrication of PV devices using these generally less expensive materials may be accomplished. In the ALD process, alternate exposures to reactive gas precursors may be separated by inert gas purging to deposit films of metal oxides, sulfides, nitrides or pure elements. The self-limiting nature of the layer-by-layer growth technique makes ALD uniquely suited to high-aspect ratio nanofabrication applications. Thus, ALD permits preparation of conformal coatings of substrates with aspect ratios greater than or about 1:100, which may have application as PV devices, components thereof, including transparent conducting oxides (TCOs), and other devices.
These techniques further open the door to the use of additional relatively inexpensive and abundant materials in PV devices. For example, iron oxide (α-Fe2O3, hematite/rust) is also now an attractive material for use in a PV device, given its abundance, stability, and environmental compatibility. Hematite's failure in previous photoelectrochemical systems has been attributed to its ultra-short hole diffusion length (2-4 nm) compared with its LOD>100 nm. Additional film materials including, for example, In2S3, CuInS2 and Cu2ZnSnS4, are also applicable to PV devices and other devices prepared using the ALD techniques described herein.
Copper compounds in particular are attractive compared to other common elements found in commercial PV devices (i.e. silicon, cadmium, tellurium, gallium, arsenic, indium) owing to its relative abundance, non-toxicity, and ease of purification. Chalcocite (Cu2S) is particularly appealing as an absorber layer, n-type layer, in thin film photovoltaic devices due to its low cost and nearly ideal bandgap (1.2 eV). To exploit these beneficial characteristics, a method of gas phase chemical vapor deposition of phase-pure Cu2S by ALD has been developed. The self-limiting surface reaction produced by alternating exposure to Bis(N,N′-di-sec-butylacetamidinato)dicopper(I) (Cu(DSB)2) and hydrogen sulfide (H2S) affords conformal deposition of thin films at temperatures as low as 130° C. Characterization of film morphology, crystallinity, and optical properties shows the as-deposited material to be well suited to applications in alternative approaches to PVs, such as the high-aspect ratio architectures described above.
Metal sulfide films were grown in a custom viscous flow ALD reactor similar in design to those that have been described previously in, for example, U.S. Patent Publication 2008/0286448, which contents are expressly incorporated herein. The ALD process comprises exposing a substrate to a sequence of various precursors for a sequence of predetermined periods of time. A cycle of alternating the various precursors, which may optionally be interspersed with a purge gas, is conducted forming a thin conformal film on the substrate. For example, the substrate may be exposed to a first precursor for a predetermined period of time. A purge gas exposure, which may be a substantially non-reactive gas, for example, N2, may follow the exposure of the first precursor. The substrate may then be exposed to a second precursor, and a purge gas sequence may again follow. The process may further include subsequent sequences of additional precursors, if any, optionally followed by a purge gas. The cycle of alternating precursors is repeated for n cycles until a desired film thickness is formed on the substrate.
The first ALD precursor may comprise a metal precursor such as a non-halogenated metal precursor containing, for example, Cu, Fe, In, Sn or Zn, The second ALD precursor may comprise a second metal precursor to form a bi-metallic film, or another precursor such as a sulfur containing compound. Subsequent ALD precursors may comprise additional metal precursors or other precursors. In various embodiments, the first ALD precursor may comprise a non-halogenated metal precursor. In a particular embodiment, the first ALD precursor may comprise a non-halogenated copper precursor. In a preferred embodiment the copper precursor comprises bis(N,N′-di-sec-butylacetamidinato)dicopper(I) (Cu(DSB)2). In various embodiments, the second ALD precursor comprises a sulfur containing compound. In a particular embodiment, the second ALD precursor comprises hydrogen sulfide (H2S). In embodiments where the first ALD precursor comprises Cu(DSB)2 and the second ALD precursor comprises H2S, a Cu2S film is formed on the substrate by repeating an alternating cycle of the first and the second precursors. More generally, the ALD process comprises a cycle of MP1-P2, where MP1 is the first metal precursor and P2 is the second precursor. The cycle may further comprise an interspersed purge gas, which may be designated MP1-purge-P2-purge.
In other embodiments, the second ALD precursor may comprise a second metal precursor. In a particular embodiment, the second metal precursor may comprise an indium metal precursor. In a preferred embodiment, the second metal precursor may comprise cyclopentadienyl indium (InCp) where indium is in the +1 oxidation state. In various embodiments, where the second ALD precursor comprises a metal precursor, the third ALD precursor may comprise a sulfur containing precursor, for example, H2S. In other embodiments, the second metal precursor may be the third ALD precursor and the second and the fourth ALD precursors may comprise H2S. Accordingly, in various embodiments the ALD cycle may comprise MP1-MP2-P3 and in another embodiment the cycle may comprise MP1-P2-MP3-P4. A purge gas may be interspersed in the above defined ALD cycles between any and all of the various precursors. In a particular embodiment, a CuInS2 film may be prepared where MP1 is selected as Cu(DSB)2, MP3 is selected as InCp, and P2 and P4 comprise H2S. It should be noted that the order of MP1 and MP3 in the cycle may be exchanged. In other words, the ALD cycle may alternatively comprise MP3-P2-MP1-P4.
In still further embodiments, the ALD cycle may comprise MP1-P2-MP3-P4-MP5-P6. Again, a purge gas may be interspersed in between any and all of the various precursors of the above cycle. In various embodiments, MP1 may comprise a non-halogenated copper precursor, and in a preferred embodiment the copper precursor comprises Cu(DSB)2. The MP3 precursor may comprise a second metal precursor, and in particular embodiments a Zn compound precursor. The MP5 precursor may comprise a third metal precursor, and in particular embodiments a Sn compound precursor. P2, P4 and P6 may comprise a sulfur compound such as H2S. In a particular embodiment, a Cu2ZnSnS4 film may be prepared where MP1 is selected as Cu(DSB)2, MP3 comprises a Zn compound, MP5 comprises a Sn compound, and P2, P4 and P6 comprise H2S. Again, the cycle order is not limited to MP1, MP3, MP5. One of skill in the art will also appreciate that a cycle may include additional metal precursors, MPn, and additional precursors, Pn, to obtain one or more films of desired characteristics.
Exposure of the substrate to the various precursors and the purge gas may be expressed as a timing sequence where each exposure comprises a predetermined exposure time. In the case of a cycle comprising MP1-purge-P2-purge, the ALD timing sequences can be expressed as t1-t2-t3-t4, where t1 is the exposure time for the first metal precursor, t2 is the purge time following the first exposure, t3 is the exposure time for the second precursor, and t4 is the purge time following the exposure to the second precursor, where the units for each exposure is in seconds. The properties of the resulting film may be configured by adjustably establishing the predetermined time for each sequence in the ALD cycle. The properties of the film may further be influenced by selectively adjusting, for example, the number of cycles, the ALD process temperature, and the substrate temperature.
The substrate exposed to the ALD process may comprise any of a number of substrates compatible with ALD and the various precursors used in the process. For example, the substrate may comprise silicon, fused silica, other materials, and combinations thereof. In various embodiments, the substrate may comprise a high-aspect ratio substrate (e.g., an aspect ratio of greater than or about 1:100). The high-aspect ratio substrates have particular application, in among other fields, PV devices. Selection of the precursors and ALD process parameters (as described in detail below) may be selected to produce a conformal thin film on the high-aspect ratio substrate. The resulting coated high-aspect ratio substrate conveniently decouples the active layer thickness and the diffusion length of the charge carrier in a PV device. Accordingly, a number of compositions hereto generally undesirable or less desirable for use in PV devices may now be effectively employed. These compositions may comprise relatively inexpensive and abundant materials and environmentally friendly materials.
The following non-limiting example is illustrative of various aspects of the invention.
In a particular embodiment, a Cu2S film was formed on a substrate by ALD using alternating exposures of a first precursor of [Cu(sBu-amd)]2 (Strem, 99%) and a second precursor H2S (Sigma-Alrich, ≧99.5%). The Cu2S films were deposited on 1×2 cm Si(100) and 2×2 cm fused silica substrates. Prior to loading, the substrates were ultrasonically cleaned in acetone and then isopropanol and blown dry using nitrogen. Prior to the Cu2S ALD, the substrates were first coated with 2 nm ALD Al2O3. The [Cu(sBu-amd)]2 first precursor vapor was delivered by 200 sccm nitrogen flow through a bubbler held at 110° C. while the H2S second precursor was stepped down to ˜10 Torr through a regulator. [Caution: H2S is a highly explosive and toxic gas.] A nitrogen purge gas was used after the first and the second precursor exposures. Ultrahigh purity nitrogen carrier gas continuously passes through the flow tube at a mass flow rate of 300 sccm and a pressure of 1 Torr. The process may be carried out a relative low temperature, for example, about 130° C. in a particular embodiment. The timing sequence was 15-15-1-10.
To enable in situ measurements, a QCM was installed in the ALD reactor in place of the substrates. The self-limiting growth of Cu2S employing [Cu(sBu-amd)]2 is demonstrated by in situ QCM at 130° C. With reference to
Film morphology was assessed with a Hitachi S4700 scanning electron microscope (SEM). X-ray diffraction (XRD) measurements were acquired on a Rigaku Miniflex Plus diffractometer using Cu Kα radiation. UV-vis-IR reflection-corrected absorption spectra were derived from measurements employing a Varian Cary 5000 with integrating sphere accessory (DRA-2500). The morphology of Cu2S via the ALD process was revealed by SEM analysis. Not to be limited by theory, the images of films prepared on silicon illustrated in
The phase purity and crystallographic orientation of the thin films were deduced from XRD.
The suitability of ALD formed α-Cu2S thin films for application in PV is further established by UV-vis-NIR spectroscopy. In contrast to XRD and electrical characterization, the extent of copper deficiency in CuxS may be probed for very thin films, even prior to crystallite formation or island coalescence. The optical assignment of CuxS single crystal polymorphs (2≧x≧1.75) is enabled by previous detailed spectroscopic studies. As depicted in
The chemical vapor deposition of chalcocite was realized by ALD. A maximum growth rate of ˜0.9 Å/cycle at 130° C. was measured from both in situ QCM and cross-sectional SEM analysis. XRD and optical spectroscopy confirm the phase purity of the preferentially orientation thin films. The growth of high quality and conformal Cu2S films make this process a promising route to nanostruetured photovoltaics.
The foregoing description of embodiments of the present invention have been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the present invention to the precise form disclosed, and modifications and variations are possible in light of the above teachings or may be acquired from practice of the present invention. The embodiments were chosen and described to explain the principles of the present invention and its practical application to enable one skilled in the art to utilize the present invention in various embodiments and with various modifications as are suited to the particular use contemplated. The features of the embodiments described herein may be combined in all possible combinations of methods, apparatus, modules and systems.
This application is related to and claims priority from U.S. Provisional Patent Application 61/181,181, filed May 26, 2009 and is hereby incorporated by reference in its entirety.
The United States Government claims certain rights in this invention pursuant to Contract No. W-31-109-ENG-38 between the United States Government and the University of Chicago and/or pursuant to DE-AC02-06CH11357 between the United States Government and UChicago Argonne, LLC representing Argonne National Laboratory.
Number | Name | Date | Kind |
---|---|---|---|
4948623 | Beach et al. | Aug 1990 | A |
7041596 | Dalton et al. | May 2006 | B1 |
7148144 | Avanzino | Dec 2006 | B1 |
20050098204 | Roscheisen et al. | May 2005 | A1 |
20050186342 | Sager et al. | Aug 2005 | A1 |
20080142972 | Redeker et al. | Jun 2008 | A1 |
Entry |
---|
Martinson et al., “Atomic layer deposition of Cu2S for future application in photovoltaics”, Applied Physics Letters 94, 123107 (2009). |
Johansson et al., “Growth of Conductive Copper Sulfide Thin Films by Atomic Layer Deposition”, J. Mater. Chem., (2002), vol. 12, pp. 1022-1026. |
Li et al., “Atomic Layer Deposition of Ultrathin Copper Metal Films from a Liquid Copper(I) Amidinate Precursor”, Journal of the Electrochemical Society, (2006), vol. 153, No. 11, pp. C787-C794, The Electrochemical Society. |
Meester et al., “Low Pressure Chemical Vapor Deposition of CuxS”, J. Phys, IV France, (2001), pp. Pr3-239-Pr3-246, EDP Sciences, Les Ulis. |
Nanu et al., “CuInS2-TiO2 Heterojunctions Solar Cells Obtained by Atomic Layer Deposition”, Thin Solid Films, (2003), pp. 492-496, vol. 431-432, Elsevier, The Netherlands. |
Reijnen et al., “Comparison of CuxS Films Grown by Atomic Layer Deposition and Chemical Vapor Deposition”, Chem. Mater., (2005), pp. 2724-2728, American Chemical Society, USA. |
Schneider et al., “Copper(I) tert-Butylthiolato Clusters as Single-Source Precursors for High-Quality Chalcocite Thin Films: Film Growth and Microstructure Control”, Chem. Mater., (2007), pp. 2780-2785, vol. 19, American Chemical Society, USA. |
Zhengwen Li, et al., “Synthesis and Characterization of Copper(I) Amidinates as Precursors for Atomic Layer Deposition (ALD) of Copper Metal”, Inorganic Chemistry., vol. 44, No. 6, 2005 pp. 1728-1735, American Chemical Society, USA, Published on the Web Feb. 3, 2005. |
Number | Date | Country | |
---|---|---|---|
20100300524 A1 | Dec 2010 | US |
Number | Date | Country | |
---|---|---|---|
61181181 | May 2009 | US |