Embodiments of the present disclosure relate to a method for preparing a protective coating for semiconductor process chamber components using atomic layer deposition (ALD), a multi-component protective coating, and a semiconductor process chamber component coated with a multi-component protective coating.
Various manufacturing processes expose semiconductor process chamber components to high temperatures, high energy plasma, a mixture of corrosive gases, high stress, and combinations thereof. These extreme conditions may erode the chamber components, corrode the chamber components, and increase the chamber components' susceptibility to defects. It is desirable to reduce these defects and improve the components' erosion and/or corrosion resistance in such extreme environments. Coating semiconductor process chamber components with protective coatings is an effective way to reduce defects and extend their durability.
Protective coating films are typically deposited on chamber components by a variety of methods, such as thermal spray, sputtering, or evaporation techniques. In these techniques, the surfaces of the chamber components that are not directly exposed to the vapor source (e.g., are not in a line of sight of a material source) are coated with either a significantly thinner film than surfaces that are directly exposed to the vapor source, poor quality film, a low-density film, or not coated at all.
Some embodiments of the present invention cover a method for forming a multi-component coating composition on a semiconductor process chamber component. The method includes depositing a first film layer of a yttrium oxide or a yttrium fluoride onto a surface of a semiconductor process chamber component, wherein the first film layer is grown from at least two precursors using an atomic layer deposition process. The method further includes depositing a second film layer of an additional oxide or an additional fluoride onto the surface of the semiconductor process chamber component, wherein the second film layer is grown from at least two additional precursors using the atomic layer deposition process. The method further includes forming a multi-component composition comprising the first film layer and the second film layer. In some embodiments, the method may further include depositing at least one additional film layer, the at least one additional film layer comprising aluminum oxide or zirconium oxide, wherein the at least one additional film layer is grown from at least two additional precursor using the atomic layer deposition process.
In some embodiments, the present invention covers a coated semiconductor process chamber component. The coated semiconductor process chamber component may comprise a semiconductor process chamber component having a surface and a multi-component coating coated on the surface. In certain embodiments, the multi-component coating may comprise at least one first film layer of a yttrium oxide or a yttrium fluoride coated onto the surface using an atomic layer deposition process and at least one second film layer of an additional oxide or an additional fluoride coated onto the surface using an atomic layer deposition process. In some embodiments, the multi-component coating may further comprise at least one additional film layer comprising aluminum oxide or zirconium oxide coated onto the surface using an atomic layer deposition process.
In some embodiments, the present invention covers a multi-component coating composition for a surface of a semiconductor process chamber component. The multi-component coating composition may comprise at least one first film layer of a yttrium oxide or a yttrium fluoride coated onto the surface of the semiconductor process chamber component using an atomic layer deposition process and at least one second film layer of an additional oxide or an additional fluoride coated onto the surface of the semiconductor process chamber component using an atomic layer deposition process. The multi-component coating composition may be selected from the group consisting of YOxFy, YAlxOy, YZrxOy and YZrxAlyOz.
The present disclosure is illustrated by way of example, and not by way of limitation, in the figures of the accompanying drawings in which like references indicate similar elements. It should be noted that different references to “an” or “one” embodiment in this disclosure are not necessarily to the same embodiment, and such references mean at least one.
Embodiments are described herein with reference to a multi-component coating that includes multiple layers that have been deposited using atomic layer deposition (also referred to as atomic monolayer deposition or ALD). Each component may be a constituent material that is included in one or more layer of the coating. One example of a multi-component coating is a coating that includes a first component of yttrium and a second component of oxygen, such as yttria (Y2O3). In another example, a multi-component coating may include a first component of Y2O3 and a second component of YF3. The first and second components may be arranged in different layers of the multi-component coating. In some embodiments, after processing such as annealing the multiple layers of the multi-component coating may interdiffuse to form a homogenous or approximately homogenous coating that includes the constituent materials of the different layers. For example, the multiple components from the different layers may form a solid state phase of a first film layer and a second film layer. In a further example, an alternating stack of Y2O3 layers and YF3 layers may interdiffuse to form a solid state phase of a yttrium oxy-fluoride. The multi-component coating may be a coating having multiple different oxides, multiple different fluorides, or a combination of one or more oxides and one or more fluorides that have or have not interdiffused. Alternatively, or additionally, the multi-component coating may be a coating having a mixture of a metal and oxygen, a metal and fluorine, a metal and oxygen and fluorine, or multiple metals with one or more of oxygen and fluorine.
The multi-component coating may be grown or deposited using ALD with various ceramics including oxide based ceramics, nitride based ceramics and carbide based ceramics. Examples of oxide based ceramics include SiO2 (quartz), Al2O3, Y2O3, Y4Al2O9, Y2O3—ZrO2 and so on. Examples of carbide based ceramics include SiC, Si—SiC, and so on. Examples of nitride based ceramics include AlN, SiN, and so on.
In one embodiment, the processing chamber 100 includes a chamber body 102 and a showerhead 130 that enclose an interior volume 106. The showerhead 130 may include a showerhead base and a showerhead gas distribution plate. Alternatively, the showerhead 130 may be replaced by a lid and a nozzle in some embodiments. The chamber body 102 may be fabricated from aluminum, stainless steel or other suitable material. The chamber body 102 generally includes sidewalls 108 and a bottom 110. Any of the showerhead 130 (or lid and/or nozzle), sidewalls 108 and/or bottom 110 may include the multi-component coating.
An outer liner 116 may be disposed adjacent the sidewalls 108 to protect the chamber body 102. The outer liner 116 may be fabricated and/or coated with a multi-component coating. In one embodiment, the outer liner 116 is fabricated from aluminum oxide.
An exhaust port 126 may be defined in the chamber body 102, and may couple the interior volume 106 to a pump system 128. The pump system 128 may include one or more pumps and throttle valves utilized to evacuate and regulate the pressure of the interior volume 106 of the processing chamber 100.
The showerhead 130 may be supported on the sidewall 108 and/or top of the chamber body 102. The showerhead 130 (or lid) may be opened to allow access to the interior volume 106 of the processing chamber 100 in some embodiments, and may provide a seal for the processing chamber 100 while closed. A gas panel 158 may be coupled to the processing chamber 100 to provide process and/or cleaning gases to the interior volume 106 through the showerhead 130 or lid and nozzle. Showerhead 130 is used for processing chambers used for dielectric etch (etching of dielectric materials). The showerhead 130 may include a gas distribution plate (GDP) having multiple gas delivery holes 132 throughout the GDP. The showerhead 130 may include the GDP bonded to an aluminum showerhead base or an anodized aluminum showerhead base. The GDP 133 may be made from Si or SiC, or may be a ceramic such as Y2O3, Al2O3, YAG, and so forth. Showerhead 130 and delivery holes 132 may be coated with a multi-component coating as described in more detail below with respect to
For processing chambers used for conductor etch (etching of conductive materials), a lid may be used rather than a showerhead. The lid may include a center nozzle that fits into a center hole of the lid. The lid may be a ceramic such as Al2O3, Y2O3, YAG, or a ceramic compound comprising Y4Al2O9 and a solid-solution of Y2O3—ZrO2. The nozzle may also be a ceramic, such as Y2O3, YAG, or the ceramic compound comprising Y4Al2O9 and a solid-solution of Y2O3—ZrO2. The lid, showerhead 130 (e.g., including showerhead base, GDP and/or gas delivery conduits/holes) and/or nozzle may all be coated with a multi-component coating according to an embodiment.
Examples of processing gases that may be used to process substrates in the processing chamber 100 include halogen-containing gases, such as C2F6, SF6, SiCl4, HBr, NF3, CF4, CHF3, CH2F3, F, NF3, Cl2, CCl4, BCl3 and SiF4, among others, and other gases such as O2, or N2O. Examples of carrier gases include N2, He, Ar, and other gases inert to process gases (e.g., non-reactive gases). The substrate support assembly 148 is disposed in the interior volume 106 of the processing chamber 100 below the showerhead 130 or lid. The substrate support assembly 148 holds the substrate 144 during processing and may include an electrostatic chuck bonded to a cooling plate.
An inner liner may be coated on the periphery of the substrate support assembly 148. The inner liner may be a halogen-containing gas resist material such as those discussed with reference to the outer liner 116. In one embodiment, the inner liner 118 may be fabricated from the same materials of the outer liner 116. Additionally, the inner liner 118 may also be coated with a multi-component coating.
Each individual chemical reaction between a precursor and the surface is known as a “half-reaction.” During each half reaction, a precursor is pulsed onto the surface for a period of time sufficient to allow the precursor to fully react with the surface. The reaction is self-limiting as the precursor will only react with a finite number of available reactive sites on the surface, forming a uniform continuous adsorption layer on the surface. Any sites that have already reacted with a precursor will become unavailable for further reaction with the same precursor unless and/or until the reacted sites are subjected to a treatment that will form new reactive sites on the uniform continuous coating. Exemplary treatments may be plasma treatment, treatment by exposing the uniform continuous adsorption layer to radicals, or introduction of a different precursor able to react with the most recent uniform continuous film layer adsorbed to the surface.
In
Subsequently, article 210 having surface 205 and layer 215 may be introduced to a third precursor 270 that reacts with layer 215 to partially form a second layer 220 by forming a second adsorption layer 218. Subsequently, article 210 may be introduced to another precursor 275 (also referred to as a reactant) to cause a second half reaction to fully form the layer 220. The second film layer 220 may be uniform, continuous and conformal. The article 210 may alternately be exposed to the third precursor 270 and fourth precursor 275 up to y number of times to achieve a target thickness for the layer 220. Y may be an integer from 1 to 100, for example.
Thereafter, the sequence of introducing the article 210 to precursors 260 and 265 x number of times and then to precursors 270 and 275 y number of times may be repeated and performed n number of times. N may be an integer from 1 to 100, for example. A result of the sequence may be to grow additional alternating layers 225, 230, 235, 240, 245, and 250. The number and thickness of the layers may be selected based on the targeted coating thickness and properties. The various layers may remain intact or in some embodiments may be interdiffused.
The surface reactions (e.g., half-reactions) are done sequentially. Prior to introduction of a new precursor, the chamber in which the ALD process takes place may be purged with an inert carrier gas (such as nitrogen or air) to remove any unreacted precursor and/or surface-precursor reaction byproducts. At least two precursors are used. In some embodiments, more than two precursors may be used to grow film layers having the same composition (e.g., to grow multiple layers of Y2O3 on top of each other). In other embodiments, different precursors may be used to grow different film layers having different compositions.
ALD processes may be conducted at various temperatures depending on the type of ALD process. The optimal temperature range for a particular ALD process is referred to as the “ALD temperature window.” Temperatures below the ALD temperature window may result in poor growth rates and non-ALD type deposition. Temperatures above the ALD temperature window may result in thermal decomposition of the article or rapid desorption of the precursor. The ALD temperature window may range from about 20° C. to about 400° C. In some embodiments, the ALD temperature window is between about 150-350° C.
The ALD process allows for conformal film layers having uniform film thickness on articles and surfaces having complex geometric shapes, holes with large aspect ratios, and three-dimensional structures. Sufficient exposure time of the precursor to the surface enables the precursor to disperse and fully react with the surface in its entirety, including all of its three-dimensional complex features. The exposure time utilized to obtain conformal ALD in high aspect ratio structures is proportionate to the square of the aspect ratio and can be predicted using modeling techniques. Additionally, the ALD technique is advantageous over other commonly used coating techniques because it allows in-situ on demand material synthesis of a particular composition or formulation without the need for a lengthy and difficult fabrication of source materials (such as powder feedstock and sintered targets).
With the ALD technique, multi-component films such as YOxFy, YAlxOy, YZrxOy, and YZrxAlyOz can be grown, for example, by proper sequencing of the precursors used to grow Y2O3, Al2O3, YF3, and ZrO2, as illustrated in more detail in the examples below.
In some embodiments, when the first film layer comprises yttrium oxide, the layer may be formed by the following process sequence:
1) Reaction of a precursor with the substrate surface. The precursor may include tris(N,N-bis(trimethylsilyl)amide)yttrium(III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III).
2) Purging of non-reacted precursor from the ALD process chamber.
3) Reaction of a second precursor with the surface. The second precursor may include H2O, O2, or O3.
4) Purging of the second non-reacted precursor from the ALD process chamber.
In some embodiments, when the first film layer comprises yttrium fluoride, the two precursors used may be tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III) and TiF4.
In some embodiments, when the second film layer comprises aluminum oxide, one precursor may include diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum. The second precursor may include H2O, O2, or O3. In some embodiments, when the second film layer comprises zirconium oxide, one precursor may include zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV). The second precursor may include H2O, O2, or O3.
The precursors listed above or any other suitable precursors may be used each time a yttrium oxide layer, a yttrium fluoride layer, an aluminum oxide layer, or a zirconium oxide layer is grown using ALD, regardless of whether it is the first, second, or Nth layer, where the Nth layer would represent the finite number of layers grown on the surface of the semiconductor process chamber component and selected based on targeted protective coating thickness and properties.
Pursuant to block 325, the method ultimately comprises forming a multi-component composition of the first film layer, the second film layer, and any additional film layers. In some embodiments, pursuant to block 320, forming the multi-component composition comprises annealing the semiconductor process chamber component comprising the first film layer, the second film layer, and any additional film layers deposited onto the semiconductor process chamber component. In some embodiments, the annealing may result in a multi-component composition comprising an interdiffused solid state phase of the at least one first film layer and the at least one second film layer and any of at least one additional film layers (if present). Annealing may be performed at a temperature ranging from about 800° C. to about 1800° C., from about 800° C. to about 1500° C., or from about 800° C. to about 1000° C. The annealing temperature may be selected based on the material of construction of the article, surface, and film layers so as to maintain their integrity and refrain from deforming, decomposing, or melting any or all of these components.
Pursuant to block 355, the method comprises depositing a film layer of a first oxide or a first fluoride onto a surface of an article via ALD. Pursuant to block 360, the method further comprises depositing a film layer of a second oxide or a second fluoride onto the surface of the article via ALD. Note that the film layer of the first oxide or first fluoride may be deposited before or after the film layer of the second oxide or the second fluoride is deposited. Accordingly, the film layer of the first oxide or first fluoride may be deposited over the film layer of the second oxide or the second fluoride in some embodiments. In other embodiments, the film layer of the second oxide or second fluoride may be deposited over the film layer of the first oxide or the first fluoride. In some embodiments, pursuant to block 365, the method may optionally further comprise depositing an additional film layer of a third oxide or a third fluoride onto the surface of the article via ALD.
In some embodiments, pursuant to block 370, the method may further comprise determining whether additional layers are to be added. Determining whether additional layers and/or how many layers are to be added can be either done in-situ, or prior to initiating the depositions (e.g., in the optional multi-component composition selection process). If additional layers are to be added, blocks 355, 360, and optionally 365 may be repeated. If no additional layers are to be added, the method proceeds to form a multi-component composition comprising all film layers deposited onto the surface of the article.
In some embodiments, when the first oxide, second oxide, or third oxide of any of the film layers comprises yttrium oxide, one precursor used to form yttrium oxide by ALD may be selected from tris(N,N-bis(trimethylsilyl)amide)yttrium(III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and the second precursor may be selected from H2O, O2, or O3. In some embodiments, when the first fluoride, second fluoride, or third fluoride of any of the film layers comprises yttrium fluoride, the two precursors used to form this film may be tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III) and TiF4.
In some embodiments, when the first oxide, second oxide, or third oxide of any of the film layers comprises aluminum oxide, one precursor used to form aluminum oxide by ALD may be selected from diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum, and the second precursor may be selected from H2O, O2, or O3. In some embodiments, when the first oxide, second oxide, or third oxide of any of the film layers comprises zirconium oxide, one zirconium oxide precursor may be selected from zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV), and the second precursor may be selected from H2O, O2, or O3.
The listed precursors or any other suitable precursors may be used each time a yttrium oxide layer, a yttrium fluoride layer, an aluminum oxide layer, or a zirconium oxide layer is grown using ALD, regardless of whether it is the first, second, or Nth film layer, where the Nth film layer would represent a finite number of film layers grown on the surface of the article and selected based on targeted protective coating thickness and properties.
In some embodiments, the method may proceed to optional block 375 where the multi-component composition of all film layers deposited onto the surface of the article may be annealed. In some embodiments, the annealing may result in a multi-component composition comprising an interdiffused solid state phase of all film layers deposited onto the surface of the article. Annealing may be performed at a temperature ranging from about 800° C. to about 1800° C., from about 800° C. to about 1500° C., or from about 800° C. to about 1000° C. The annealing temperature may be selected based on the material of construction of the article, surface, and film layers so as to maintain their integrity and refrain from deforming, decomposing, or melting any or all of these components.
In
In some embodiments, the at least one first film layer comprises a first continuous monolayer, and the at least one second film layer comprises a second continuous monolayer. In some embodiments, at least one additional layer may comprise at least one additional monolayer.
In other embodiments, the at least one first film layer comprises a first thick layer having a uniform thickness, the uniform thickness ranging from that of two monolayers to about 1 micrometer, and wherein the at least one second film layer comprises a second thick layer having the uniform thickness of the first film layer. In yet other embodiments, at least one additional film layer may comprise at least one additional thick layer having the uniform thickness of the other two thick layers.
In some embodiments, the multi-component coating composition may comprise at least one first film layer, at least one second film layer, and optionally one or more additional film layers, wherein the layers may vary in thickness. For example, some layers may be monolayers and some layers may be thick layers.
In some embodiments, the various film layers illustrated in
In some embodiments, the multi-component coating composition, whether comprising intact layers or an interdiffused solid state phase, is selected from the group consisting of YOxFy, YAlxOy, YZrxOy and YZrxAlyOz. The processes for creating these various multi-component coating compositions are illustrated in the examples below.
The complex geometry of lower surface 505 is configured to receive a multi-component coating. Lower surface 505 of showerhead 500 defines gas conduits 510 arranged in evenly distributed concentric rings. In other embodiments, gas conduits 510 may be configured in alternative geometric configurations and may have as many or as few gas conduits as needed depending on the type of reactor and/or process utilized. The multi-component coating is grown on surface 505 and in gas conduit holes 510 using the ALD technique which enables a conformal coating of relatively uniform thickness on the surface as well as in the gas conduit holes despite the complex geometry and the large aspect ratios of the holes.
Showerhead 500 may be exposed to corrosive chemistries such fluorine and may erode due to plasma interaction with the showerhead. The multi-component coating layer may reduce such plasma interactions and improve the showerhead's durability. The multi-component coating layer deposited with ALD maintains the relative shape and geometric configuration of the lower surface 505 and of the gas conduits 510 so as to not disturb the functionality of the showerhead. Similarly, when applied to other chamber components, the multi-component coating may maintain the shape and geometric configuration of the surface it is intended to coat so as to not disturb the component's functionality, provide plasma resistance, and improves erosion and/or corrosion resistance throughout the entire surface.
The resistance of the coating material to plasma is measured through “etch rate” (ER), which may have units of Angstrom/min (Å/min), throughout the duration of the coated components' operation and exposure to plasma. Plasma resistance may also be measured through an erosion rate having the units of nanometer/radio frequency hour (nm/RFHr), where one RFHr represents one hour of processing in plasma processing conditions. Measurements may be taken after different processing times. For example, measurements may be taken before processing, after 50 processing hours, after 150 processing hours, after 200 processing hours, and so on. An erosion rate lower than about 100 nm/RFHr is typical for a multi-component plasma resistant coating material. Variations in the composition of the multi-component coating grown on the showerhead or on any other semiconductor process chamber component may result in multiple different plasma resistances or erosion rate values. Additionally, a multi-component coating with a single composition exposed to various plasmas could have multiple different plasma resistances or erosion rate values. For example, a plasma resistant material may have a first plasma resistance or erosion rate associated with a first type of plasma and a second plasma resistance or erosion rate associated with a second type of plasma.
Gas conduit 510 may have an interior surface 555 which may be coated with a multi-component coating. The multi-component coating may comprise at least one first layer 560 and at least one second layer 565 and optionally at least one additional layer (not shown). The first film layer may comprise yttrium oxide or yttrium fluoride. The second film layer may comprise an additional oxide or an additional fluoride. The optional at least one additional layer may comprise aluminum oxide or zirconium oxide. All layers may be coated using an ALD process. The ALD process may grow conformal coating layers of uniform thickness throughout the interior surface of gas conduit 510 despite its large aspect ratio while ensuring that the final multi-component coating may also be thin enough so as to not plug the gas conduits in the showerhead.
In some embodiments, the multi-component coating may comprise intact layers of at least one first layer, at least one second layer, and optionally at least one additional layer. In an embodiment, the first, second, and any optional additional layers may alternate at a predetermined order. In another embodiment, the first, second, and any optional additional layers may be present in any order. In some embodiments, there may be an equal number of each one of the first, of the second, and of any optional additional layer. In other embodiments, some of the layers may be more prevalent than other layers so as to achieve certain properties for the multi-component coating. Certain properties may be plasma resistance and erosion/corrosion resistance that would improve the durability of the coated semiconductor process chamber component.
In some embodiments, the intact layers may comprise monolayers of uniform thickness. In other embodiments, the intact layers may comprise thicker layers of uniform thickness. Each thicker layer may have a thickness ranging from that of two monolayers to about 1 micrometer. In yet other embodiments, the intact layers may comprise a combination of monolayers and thick layers.
In other embodiments, the multi-component coating may comprise interdiffused solid state phase of at least one first layer, at least one second layer, and optionally at least one additional layer. In an embodiment, an interdiffused solid state phase of the various layers may be obtained through annealing. The composition of the layers, number of layers, frequency of each layer, and thickness of the layers will all contribute to the final properties of the multi-component coating layer.
The following examples are set forth to assist in understanding the embodiments described herein and should not be construed as specifically limiting the embodiments described and claimed herein. Such variations, including the substitution of all equivalents now known or later developed, which would be within the purview of those skilled in the art, and changes in formulation or minor changes in experimental design, are to be considered to fall within the scope of the embodiments incorporated herein. These examples may be achieved by performing method 300 or method 350 described above.
The first layer may be a yttrium oxide monolayer grown using ALD from a precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III) tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and a second precursor selected from H2O, O2 or O3. The second layer may be yttrium fluoride monolayer grown using ALD from a single combination of the precursors tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III) and TiF4. The resulting multi-component coating may comprise YOxFy where X and Y depend on the number of repetitions of the first and the second layer.
The first layer may be a yttrium oxide monolayer grown using ALD from a precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and a second precursor selected from H2O, O2, or O3. The second layer may be aluminum oxide monolayer grown using ALD from a precursor selected from diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum, and a second precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YAlxOy where X and Y depend on the number of repetitions of the first and the second layer.
In some experiments stacks of alternating layers of Y2O3 and Al2O3 were deposited via ALD, where each may layer had a thickness of 5 nm. Other thicknesses may also be used for the individual layers, such as anywhere from a few Angstroms to about 10 nm or thicker. A total coating thickness in the experiments was about 200 nm. Samples were annealed at temperatures of 500° C., 750° C., 800° C., 900° C. and or 1000° C. for 12 hrs. The annealed and as-coated samples were analyzed by grazing incidence x-ray diffraction to determine a microstructure of the coating for each of the samples. Testing showed that the coating transformed from an amorphous structure to a mostly crystalline structure consisting primarily of the cubic Y3Al5O12 or Y3Al5O13 (i.e., yttrium aluminum garnet) phase as a result of annealing at temperatures of 800° C. and above. At temperatures of 500° C. and 750° C., crystallization of Y2O3 occurred but the yttrium aluminum garnet phase did not form. For example, after annealing at 500° C. an amorphous phase and a crystalline Y2O3 phase were formed. The amorphous phase may contain some Y2O3 that has not crystallized. Table 1 below shows the phase identification of a stack of alternating layer films of Al2O3/Y2O3, as-deposited and annealed at various temperatures.
Minor/trace phase:
Minor/Trace Phases:
Minor/Trace Phases:
The first layer may be a yttrium oxide monolayer grown using ALD from a precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and a second precursor selected from H2O, O2, or O3. The second layer may be zirconium oxide monolayer grown using ALD from a precursor selected from zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV), and a second precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YZrxOy where X and Y depend on the number of repetitions of the first and the second layer.
The first layer may be a yttrium oxide monolayer grown using ALD from a precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and a second precursor selected from H2O, O2, or O3. The second layer may be zirconium oxide monolayer grown using ALD from a precursor selected from zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV), and a second precursor selected from H2O, O2, or O3. The at least one additional layer may be aluminum oxide monolayer grown using ALD from a precursor selected from diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum, and a second precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YZrxAlyOz where X, Y, and Z depend on the number of repetitions of the first, second, and at least one additional layer.
The first layer may be a yttrium oxide thick layer grown using ALD from at least one precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and at least one precursor selected from H2O, O2, or O3. The second layer may be yttrium fluoride thick layer grown using ALD from the precursors tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III) and TiF4. The resulting multi component coating may comprise YOxFy where X and Y depend on the number of repetitions of the first and the second layer.
The first layer may be a yttrium oxide thick layer grown using ALD from at least one precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and at least one precursor selected from H2O, O2, or O3. The second layer may be aluminum oxide thick layer grown using ALD from at least one precursor selected from diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum, and at least one precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YAlxOy where X and Y depend on the number of repetitions of the first and the second layer.
The first layer may be a yttrium oxide thick layer grown using ALD from at least one precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and at least one precursor selected from H2O, O2, or O3. The second layer may be zirconium oxide thick layer grown using ALD from at least one precursor selected from zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV), and at least one precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YZrxOy where X and Y depend on the number of repetitions of the first and the second layer.
The first layer may be a yttrium oxide thick layer grown using ALD from at least one precursor selected from tris(N,N-bis(trimethylsilyl)amide)yttrium (III), tris(cyclopentadienyl)yttrium(III), tris(butylcyclopentadienyl)yttrium(III), or tris(2,2,6,6-tetramethyl-3,5-heptanedionato)yttrium(III), and at least one precursor selected from H2O, O2, or O3. The second layer may be zirconium oxide thick layer grown using ALD from at least one precursor selected from zirconium (IV) bromide, zirconium (IV) chloride, zirconium (IV) tert-butoxide, tetrakis(diethylamido)zirconium (IV), tetrakis(dimethylamido)zirconium (IV), or tetrakis(ethylmethylamido)zirconium (IV), and at least one precursor selected from H2O, O2, or O3. The at least one additional layer may be aluminum oxide thick layer grown using ALD from at least one precursor selected from diethylaluminum ethoxide, tris(ethylmethylamido)aluminum, aluminum sec-butoxide, aluminum tribromide, aluminum trichloride, triethylaluminum, triisobutylaluminum, trimethylaluminum, or tris(diethylamido)aluminum, and at least one precursor selected from H2O, O2, or O3. The resulting multi component coating may comprise YZrxAlyOz where X, Y, and Z depend on the number of repetitions of the first, second, and at least one additional layer.
The preceding description sets forth numerous specific details such as examples of specific systems, components, methods, and so forth, in order to provide a good understanding of several embodiments of the present invention. It will be apparent to one skilled in the art, however, that at least some embodiments of the present invention may be practiced without these specific details. In other instances, well-known components or methods are not described in detail or are presented in simple block diagram format in order to avoid unnecessarily obscuring the present invention. Thus, the specific details set forth are merely exemplary. Particular implementations may vary from these exemplary details and still be contemplated to be within the scope of the present invention.
Reference throughout this specification to “one embodiment” or “an embodiment” means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment. Thus, the appearances of the phrase “in one embodiment” or “in an embodiment” in various places throughout this specification are not necessarily all referring to the same embodiment. In addition, the term “or” is intended to mean an inclusive “or” rather than an exclusive “or.” When the term “about” or “approximately” is used herein, this is intended to mean that the nominal value presented is precise within ±10%.
Although the operations of the methods herein are shown and described in a particular order, the order of the operations of each method may be altered so that certain operations may be performed in an inverse order or so that certain operation may be performed, at least in part, concurrently with other operations. In another embodiment, instructions or sub-operations of distinct operations may be in an intermittent and/or alternating manner.
It is to be understood that the above description is intended to be illustrative, and not restrictive. Many other embodiments will be apparent to those of skill in the art upon reading and understanding the above description. The scope of the invention should, therefore, be determined with reference to the appended claims, along with the full scope of equivalents to which such claims are entitled.
This application claims priority to U.S. Provisional Patent Application 62/328,588, filed Apr. 27, 2016, which is herein incorporated by reference.
| Number | Name | Date | Kind |
|---|---|---|---|
| 5630314 | Kojima et al. | May 1997 | A |
| 5805973 | Coffinberry | Sep 1998 | A |
| 5840434 | Kojima et al. | Nov 1998 | A |
| 6139983 | Ohashi et al. | Oct 2000 | A |
| 6548424 | Putkonen | Apr 2003 | B2 |
| 6632549 | Ohashi et al. | Oct 2003 | B1 |
| 6641941 | Yamada et al. | Nov 2003 | B2 |
| 6685991 | Wataya et al. | Feb 2004 | B2 |
| 6777353 | Putkonen | Aug 2004 | B2 |
| 6858332 | Yamada | Feb 2005 | B2 |
| 6858546 | Niinisto et al. | Feb 2005 | B2 |
| 6916534 | Watava et al. | Jul 2005 | B2 |
| 7138192 | Yamada et al. | Nov 2006 | B2 |
| 7351658 | Putkonen | Apr 2008 | B2 |
| 7384696 | Hayasaki et al. | Jun 2008 | B2 |
| 7498272 | Niinisto et al. | Mar 2009 | B2 |
| 7560376 | Escher et al. | Jul 2009 | B2 |
| 7569280 | Havasaki et al. | Aug 2009 | B2 |
| 7696117 | Sun et al. | Apr 2010 | B2 |
| 7754621 | Putkonen | Jul 2010 | B2 |
| 7780786 | Mitsuhashi et al. | Aug 2010 | B2 |
| 7968205 | Nakano et al. | Jun 2011 | B2 |
| 7998883 | Putkonen | Aug 2011 | B2 |
| 8399862 | Ohmi et al. | Mar 2013 | B2 |
| 8619406 | Cho et al. | Dec 2013 | B2 |
| 8858745 | Sun et al. | Oct 2014 | B2 |
| 8916021 | Sun et al. | Dec 2014 | B2 |
| 9012030 | Han et al. | Apr 2015 | B2 |
| 9023427 | Matero et al. | May 2015 | B2 |
| 9090046 | Sun et al. | Jul 2015 | B2 |
| 9343289 | Sun et al. | May 2016 | B2 |
| 9394615 | Sun et al. | Jul 2016 | B2 |
| 9440886 | Sun et al. | Sep 2016 | B2 |
| 9551070 | Chang et al. | Jan 2017 | B2 |
| 9617188 | Sun et al. | Apr 2017 | B2 |
| 9617633 | He et al. | Apr 2017 | B2 |
| 9633884 | He et al. | Apr 2017 | B2 |
| 9850573 | Sun | Dec 2017 | B1 |
| 10186400 | Wu et al. | Jan 2019 | B2 |
| 10573497 | Wu et al. | Feb 2020 | B2 |
| 20020115252 | Haukka et al. | Aug 2002 | A1 |
| 20020177001 | Harada et al. | Nov 2002 | A1 |
| 20030029563 | Kaushal | Feb 2003 | A1 |
| 20030051811 | Uchimaru et al. | Mar 2003 | A1 |
| 20030127049 | Han et al. | Jul 2003 | A1 |
| 20040023811 | Iijima | Feb 2004 | A1 |
| 20040033385 | Kaushal et al. | Feb 2004 | A1 |
| 20050037536 | Lai | Feb 2005 | A1 |
| 20050151184 | Lee et al. | Jul 2005 | A1 |
| 20050227118 | Uchimaru et al. | Oct 2005 | A1 |
| 20060037536 | Kobayashi et al. | Feb 2006 | A1 |
| 20060040508 | Ji et al. | Feb 2006 | A1 |
| 20060073354 | Watanabe et al. | Apr 2006 | A1 |
| 20060202621 | Yoo | Sep 2006 | A1 |
| 20080066647 | Harada et al. | Mar 2008 | A1 |
| 20080213496 | Sun et al. | Sep 2008 | A1 |
| 20080254231 | Lin et al. | Oct 2008 | A1 |
| 20080264565 | Sun et al. | Oct 2008 | A1 |
| 20090194233 | Tamura | Aug 2009 | A1 |
| 20100119843 | Sun | May 2010 | A1 |
| 20100119844 | Sun et al. | May 2010 | A1 |
| 20100129670 | Sun et al. | May 2010 | A1 |
| 20100323124 | Vartabedian et al. | Dec 2010 | A1 |
| 20110008955 | Horii et al. | Jan 2011 | A1 |
| 20110091700 | Simpson | Apr 2011 | A1 |
| 20120135155 | Han et al. | May 2012 | A1 |
| 20120138472 | Han | Jun 2012 | A1 |
| 20130154059 | Ohmi et al. | Jun 2013 | A1 |
| 20140116338 | He et al. | May 2014 | A1 |
| 20140120312 | He et al. | May 2014 | A1 |
| 20140159325 | Parkhe et al. | Jun 2014 | A1 |
| 20150004418 | Sun et al. | Jan 2015 | A1 |
| 20150021324 | Sun et al. | Jan 2015 | A1 |
| 20150024155 | Sun et al. | Jan 2015 | A1 |
| 20150061237 | Sun et al. | Mar 2015 | A1 |
| 20150064450 | Sun et al. | Mar 2015 | A1 |
| 20150152540 | Sato et al. | Jun 2015 | A1 |
| 20150158775 | Sun et al. | Jun 2015 | A1 |
| 20150201461 | Duan et al. | Jul 2015 | A1 |
| 20150270108 | Sun et al. | Sep 2015 | A1 |
| 20150299050 | Sun et al. | Oct 2015 | A1 |
| 20150307982 | Firouzdor et al. | Oct 2015 | A1 |
| 20150311043 | Sun et al. | Oct 2015 | A1 |
| 20150311044 | Sun et al. | Oct 2015 | A1 |
| 20150321964 | Sun et al. | Nov 2015 | A1 |
| 20150329955 | Sun et al. | Nov 2015 | A1 |
| 20160076129 | Nagayama et al. | Mar 2016 | A1 |
| 20160079040 | Park et al. | Mar 2016 | A1 |
| 20160181627 | Roeder et al. | Jun 2016 | A1 |
| 20160211121 | Sun et al. | Jul 2016 | A1 |
| 20160254125 | Huang et al. | Sep 2016 | A1 |
| 20160273095 | Lin et al. | Sep 2016 | A1 |
| 20160281230 | Varadarajan et al. | Sep 2016 | A1 |
| 20160312351 | Liu et al. | Oct 2016 | A1 |
| 20160326625 | Sun et al. | Nov 2016 | A1 |
| 20160326626 | Sun et al. | Nov 2016 | A1 |
| 20160336210 | Cooke | Nov 2016 | A1 |
| 20160358749 | Sant | Dec 2016 | A1 |
| 20160375515 | Xu et al. | Dec 2016 | A1 |
| 20160379806 | Xu et al. | Dec 2016 | A1 |
| 20170010969 | Chiu et al. | Jan 2017 | A1 |
| 20170022595 | Sato et al. | Jan 2017 | A1 |
| 20170110293 | Sun et al. | Apr 2017 | A1 |
| 20170140969 | Kuo | May 2017 | A1 |
| 20170314125 | Fenwick et al. | Nov 2017 | A1 |
| 20180044800 | Hendrix et al. | Feb 2018 | A1 |
| Number | Date | Country |
|---|---|---|
| 1655362 | Aug 2005 | CN |
| 1906026 | Jan 2007 | CN |
| 101218376 | Jul 2008 | CN |
| 101418435 | Apr 2009 | CN |
| 102575345 | Jul 2012 | CN |
| 103215535 | Jul 2013 | CN |
| 104715993 | Jun 2015 | CN |
| 105074889 | Nov 2015 | CN |
| 105088141 | Nov 2015 | CN |
| 105225997 | Jan 2016 | CN |
| 207193391 | Apr 2018 | CN |
| H03115535 | May 1991 | JP |
| 2006082474 | Mar 2006 | JP |
| 2007131951 | May 2007 | JP |
| 2007217782 | Aug 2007 | JP |
| 2012159133 | Aug 2012 | JP |
| 20110037282 | Apr 2011 | KR |
| 20170044396 | Apr 2017 | KR |
| 03089682 | Oct 2003 | WO |
| 2007115029 | Oct 2007 | WO |
| 2013032260 | Mar 2013 | WO |
| 2013032809 | Mar 2013 | WO |
| 2014205212 | Dec 2014 | WO |
| 2015120265 | Aug 2015 | WO |
| Entry |
|---|
| Putkonen (Chemical Vapor Deposition 2001, 7, 44-50). |
| Pilvi (Chemical Vapor Deposition 2009, 15, 27-32). |
| Ginestra (Electrochemical and Solid-State Letters, 10 (10) B161-B165 (2007)) (Year: 2007). |
| Johansson, P. et al., “Atomic Layer Deposition Process for Barrier Applications of Flexible Packaging,” 2010 Place Conference, Apr. 18-21, 2010, 33 pages, Albequerque, New Mexico. |
| Rowland, J.C. “Atomic Layer Depositions of the Al2O3-Y2O3 Pseudo-Binary System”, Doctoral Disertation, University of Florida, ProQuest LLC, 2010, pp. 1-106. |
| Japanese Office Action and English Translation thereof for Japanese patent application No. 2017-250741, dated Feb. 16, 2021, 7 pages. |
| Japanese Office Action and English Translation thereof for Japanese patent application No. 2017-086912, dated Feb. 16, 2021, 11 pages. |
| Chinese Office Action and English Translation thereof for Chinese patent application No. 201910516222, dated Jan. 13, 2021, 13 pages. |
| Sanghoon Ji et al., “Fabrication of low-temperature solid oxide fuel cells with a nanothin protective layer by atomic layer deposition”; Nanoscale Research Letters, Jan. 23, 2013, vol. 8, No. 48, 7 pages. |
| Number | Date | Country | |
|---|---|---|---|
| 20170314125 A1 | Nov 2017 | US |
| Number | Date | Country | |
|---|---|---|---|
| 62328588 | Apr 2016 | US |