Photoresist compositions containing selected 6-acetoxy cyclohexadienone photosensitizers and novolak resins

Information

  • Patent Grant
  • 4902603
  • Patent Number
    4,902,603
  • Date Filed
    Monday, October 5, 1987
    37 years ago
  • Date Issued
    Tuesday, February 20, 1990
    34 years ago
Abstract
A light-sensitive mixture useful as a negative-working photoresist composition comprising:(a) at least one novolak resin; and(b) at least one 6-acetoxy cyclohexadienone compound of the formula (I) below: ##STR1## wherein R.sub.1, R.sub.2, R.sub.3, R.sub.4 and R.sub.5 are individually selected from hydrogen and lower alkyl groups having from 1 to 4 carbon atoms with the proviso that at least three of the R.sub.1 to R.sub.5 groups are lower alkyl groups.
Description

BACKGROUND OF THE INVENTION
1. Field of the Invention
The present invention relates to light-sensitive mixtures useful as negative-working photoresist compositions containing at least one novolak resin and selected 6-acetoxy cyclohexadienone compounds as photosensitizers. Furthermore, the present invention also relates to substrates coated with these light-sensitive mixtures as well as the process of imaging and developing these light sensitive mixtures on these substrates.
2. Description of Related Art
Photoresist compositions are used in microlithography processes for making miniaturized electronic components such as in the fabrication of integrated circuits and printed wiring board circuitry. Generally, in these processes, a thin coating or film of a photoresist composition is first applied to a substrate material, such as silicon wafers used for making integrated circuits or aluminum or copper plates of printed wiring boards. The coated substrate is then baked to fix the coating onto the substrate. The baked coated surface of the substrate is next subjected to an image-wise exposure of radiation. This radiation exposure causes a chemical transformation in the exposed areas of the coated surface. Ultraviolet (UV) light, electron beam and X-ray radiant energy are radiation types commonly used today in microlithographic processes. After this image-wise exposure, the coated substrate is treated with a developer solution to dissolve and remove either the radiation-exposed or the unexposed areas of the coated surface of the substrate.
There are two types of photoresist compositions--negative-working and positive-working. When negative-working photoresist compositions are exposed image-wise to radiation, the areas of the resist composition exposed to the radiation become more insoluble to a developer solution (e.g. a cross-linking reaction occurs) while the unexposed areas of the photoresist coating remain relatively soluble to a developing solution. Thus, treatment of an exposed negative-working resist with a developer causes removal of the non-exposed areas of the resist coating and the creation of a negative image in the photoresist coating. On the other hand, when positive-working photoresist compositions are exposed image-wise to radiation, those areas of the resist composition exposed to the radiation become more soluble to the developer solution (e.g. a decomposition reaction occurs) while those areas not exposed remain relatively insoluble to the developer solution. Thus, treatment of an exposed positive-working resist with the developer causes removal of the exposed areas of the resist coating and the creation of a positive image in the photoresist coating.
After this development operation, the now partially unprotected substrate may be treated with a substrate-etchant solution or plasma gases and the like. This etchant solution or plasma gases etches the portion of the substrate where the photoresist coating was removed during development. The areas of the substrate where the photoresist coating still remains are protected and, thus, an etched pattern is created in the substrate material which corresponds to the photomask used for the image-wise exposure of the radiation. Later, the remaining areas of the photoresist coating may be removed during a stripping operation, leaving a clean etched substrate surface.
Positive-working photoresist compositions are currently favored over negative-working resists because the former generally have better resolution capabilities and pattern transfer characteristics.
Photoresist resolution is defined as the smallest feature which the resist composition can transfer from the photomask to the substrate with a high degree of image edge acuity after exposure and development. In many manufacturing applications today, resist resolution on the order of one micron or less are necessary.
In addition, it is generally desirable that the developed photoresist wall profiles be near vertical relative to the substrate. Such demarcations between developed and undeveloped areas of the resist coating translate into accurate pattern transfer of the mask image onto the substrate.
Still further, many current negative photoresist formulations also swell when subjected to development steps, thereby causing image distortion. And, negative photoresists generally require an organic developer solution. The employment of such organic materials creates special handling and disposal problems for the photoresist fabricator.
On the other hand, positive photoresist formulations are not favored for all commercial applications. For example, positive photoresists such as those based on novolak resins and orthonaphthoquinone diazide photosensitizers have certain processing limitations when their imaging is carried out in the deep ultraviolet region of the light spectrum. In this class of positive resists, both ingredients absorb light from the deep ultraviolet region and, thus, the photoresist requires increased input of radiation to compensate for the unwanted light absorptions.
Accordingly, there is a need for a better negative-working photoresist formulation which overcomes the deficiencies of current negative-working photoresists, especially in the area of the deep UV light region where positive-working resists have limitations as to commercialization. The present invention is believed to be an answer to that need.
SUMMARY OF THE INVENTION
Accordingly, the present invention is directed to a light-sensitive mixture useful as a negative-working photoresist composition comprising:
(a) at least one novolak-type resin; and
(b) at least one 6-acetoxy cyclohexadienone compound of the formula (I) below: ##STR2## wherein R.sub.1, R.sub.2, R.sub.3, R.sub.4 and R.sub.5 are individually selected from hydrogen and lower alkyl groups having from 1 to 4 carbon atoms with the proviso that at least three of the R.sub.1 to R.sub.5 groups are lower alkyl groups.
Moreover, the present invention also encompasses the process of coating substrates with these light-sensitive mixtures and then imaging and developing these coated substrates.
Still further, the present invention also encompasses said coated substrates (both before and after imaging) as novel articles of manufacture.
DETAILED DESCRIPTION
The 6-acetoxy cyclohexadienone compounds of formula (I) above may be preferably made by reacting about one mole of lead tetraacetate per one mole of the corresponding tri(lower alkyl) phenol in the presence of a solvent. These compounds of formula (I) are more preferably prepared by first dissolving or suspending each reactant in a suitable solvent, such as chloroform or the like. The reaction may be carried out at or below room temperature and is complete in a fairly short time (i.e. less than three and a half hours). The desired reaction product may be recovered by any conventional means. For example, the resulting reaction mixture may be washed with water several times, followed by recovery of the organic layer, which is then filtered and dried. This crude product may then be recrystallized to produce pure product.
One or more of these 6-acetoxy cyclohexadienone compounds are then combined with a novolak resin or resins to make light-sensitive mixtures useful as negative-working photoresist compositions. The term "novolak-type resin" is used herein to mean any novolak resin which is conventionally used in photoresist compositions. Suitable novolak resins include phenol-formaldehyde novolak resins and cresol-formaldehyde novolak resins, preferably having a molecular weight of about 500 to about 30,000, more preferably from about 1,000 to about 20,000. These novolak resins are preferably prepared by the condensation reaction of phenol or cresol with formaldehyde and are characterized by being light-stable, water-insoluble, alkali-soluble and film-forming. The preparation of examples of such suitable resins is disclosed in U.S. Pat. Nos. 4,377,631; 4,529,682; and 4,587,196, all of which issued to Medhat Toukhy and are incorporated herein by reference in their entireties.
The proportion of the above sensitizer compound of formula (I) in the light-sensitive mixture may preferably range from about 1 to about 30 percent, more preferably from about 5 to about 25 percent by weight of the non-volatile (e.g. non-solvent) content of the light-sensitive mixture. The proportion of novolak resin in the light-sensitive mixture may preferably range from about 70 to about 99 percent, more preferably, from about 75 to 95 percent of the non-volatile (e.g. excluding solvents) content of the light-sensitive mixture.
These light-sensitive mixtures may also contain conventional photoresist composition ingredients such as solvents, actinic and contrast dyes, anti-striation agents, plasticizers, speed enhancers, and the like. These additional ingredients may be added to the novolak resin and sensitizer solution before the solution is coated onto the substrate.
The resins and sensitizers may be dissolved in a solvent or solvents to facilitate their application to the substrate. Examples of suitable solvents include ethyl cellosolve acetate, n-butyl acetate, xylene, ethyl lactate, propylene glycol alkyl ether acetates, or mixtures thereof and the like. The preferred amount of solvent may be from about 50% to about 500% by weight, more preferably, from about 100% to about 400%, based on combined resin and sensitizer weight.
Actinic dyes help provide increased resolution by inhibiting back scattering of light off the substrate. This back scattering causes the undesirable effect of optical notching, especially where the substrate is highly reflective or has topography. Examples of actinic dyes include those that absorb light energy at approximately 400-460 nm [e.g. Fat Brown B (C.I. No. 12010); Fat Brown RR (C.I. No. 11285); 2-hydroxy-1,4-naphthoquinone (C.I. No. 75480) and Quinoline Yellow A (C.I. No. 47000)] and those that absorb light energy at approximately 300-340 nm [e.g. 2,5-diphenyloxazole (PPO-Chem. Abs. Reg. No. 92-71-7) and 2-(4-biphenyl)-6-phenyl-benzoxazole (PBBO-Chem. Abs. Reg. No. 17064-47-0)]. The amount of actinic dyes may be up to ten percent weight levels, based on the combined weight of resin and sensitizer.
Contrast dyes enhance the visibility of the developed images and facilitate pattern alignment during manufacturing. Examples of contrast dye additives that may be used together with the light-sensitive mixtures of the present invention include Solvent Red 24 (C.I. No. 26105), Basic Fuchsin (C.I. 42514), Oil Blue N (C.I. No. 61555) and Calco Red A (C.I. No. 26125) up to ten percent weight levels, based on the combined weight of resin and sensitizer.
Anti-striation agents level out the photoresist coating or film to a uniform thickness. This is important to ensure uniform radiation exposure over the film surface. Anti-striation agents may be used up to five percent weight levels, based on the combined weight of resin and sensitizer. One suitable class of anti-striation agents is non-ionic silicon-modified polymers. Non-ionic surfactants may also be used for this purpose, including, for example, nonylphenoxy poly(ethyleneoxy) ethanol; octylphenoxy (ethyleneoxy) ethanol; and dinonyl phenoxy poly(ethyleneoxy) ethanol.
Plasticizers improve the coating and adhesion properties of the photoresist composition and better allow for the application of a thin coating or film of photoresist which is smooth and of uniform thickness onto the substrate. Plasticizers which may be used include, for example, phosphoric acid tri-(.beta.-chloroethyl)-ester; stearic acid; dicamphor; polypropylene; acetal resins; phenoxy resins; and alkyl resins up to ten percent weight levels, based on the combined weight of resin and sensitizer.
Speed enhancers tend to increase the solubility of the photoresist coating in both the exposed and unexposed areas, and thus, they are used in applications where speed of development is the overriding consideration even though some degree of contrast may be sacrificed, i.e. in negative resists while the unexposed areas of the photoresist coating will be dissolved more quickly by the developer, the speed enhancers will also cause a larger loss of photoresist coating from the exposed areas. Speed enhancers that may be used include, for example, picric acid, nicotinic acid or nitrocinnamic acid at weight levels of up to 20 percent, based on the combined weight of resin and sensitizer.
The prepared light-sensitive resist mixture, can be applied to a substrate by any conventional method used in the photoresist art, including dipping, spraying, whirling and spin coating. When spin coating, for example, the resist mixture can be adjusted as to the percentage of solids content in order to provide a coating of the desired thickness given the type of spinning equipment and spin speed utilized and the amount of time allowed for the spinning process. Suitable substrates include silicon, aluminum or polymeric resins, silicon dioxide, doped silicon dioxide, silicon resins, gallium arsenide, silicon nitride, tantalum, copper, polysilicon, ceramics and aluminum/copper mixtures.
The photoresist coatings produced by the above described procedure are particularly suitable for application to thermally grown silicon/silicon dioxide-coated wafers such as are utilized in the production of microprocessors and other miniaturized integrated circuit components. An aluminum/aluminum oxide wafer can be used as well. The substrate may also comprise various polymeric resins especially transparent polymers such as polyesters and polyolefins.
After the resist solution is coated onto the substrate, the coated substrate is baked at approximately 70.degree. to 115.degree. C. until substantially all the solvent has evaporated and only a uniform light-sensitive coating remains on the substrate.
The coated substrate can then be exposed to radiation, especially ultraviolet radiation, in any desired exposure pattern, produced by use of suitable masks, negatives, stencils, templates, and the like. Conventional imaging process or apparatus currently used in processing photoresist-coated substrates may be employed with the present invention.
The exposed resist-coated substrates are next developed in alkaline inorganic or organic developing solution. This solution is preferably agitated, for example, by nitrogen gas agitation. Examples of alkaline inorganic developers include aqueous solutions of tetramethylammonium hydroxide, sodium hydroxide, potassium hydroxide, choline, sodium phosphates, sodium carbonate, sodium metasilicate, and the like. Examples of organic developers include isopropanol alone or mixed with methyl isobutylketone or mixtures of methyl ethyl ketone, ethanol and isopropanol and the like. The preferred developers for this invention are aqueous solutions of tetramethylammonium hydroxide.
Alternative development techniques such as spray development or puddle development, or combinations thereof, may also be used.
The substrates are allowed to remain in the developer until all of the resist coating has dissolved from the unexposed areas. Normally, development times from about 30 seconds to about 3 minutes are employed.
After selective dissolution of the coated wafers in the developing solution, they are preferably subjected to a deionized water rinse to fully remove the any remaining undesired portions of the coating and to stop further development. This rinsing operation (which is part of the development process) may be followed by blow drying with filtered air to remove excess water. A post-development heat treatment or bake may then be employed to increase the coating's adhesion and chemical resistance to etching solutions and other substances. The post-development heat treatment can comprise the oven baking of the coating and substrate below the coating's softening point.
In industrial applications, particularly in the manufacture of microcircuitry units on silicon/silicon dioxide-type substrates, the developed substrates may then be treated with a buffered, hydrofluoric acid etching solution or plasma gas etch. The resist compositions of the present invention are believed to be resistant to a wide variety of acid etching solutions or plasma gases and provide effective protection for the resist-coated areas of the substrate.
Later, the remaining ares of the photoresist coating may be removed from the etched substrate surface by conventional photoresist stripping operations.





The present invention is further described in detail by means of the following Examples. All parts and percentages are by weight unless explicitly stated otherwise.
EXAMPLE I
Preparation of 6-acetoxy-2,4,6-trimethylcyclohexa-2,4-dienone
2,4,6-Trimethylphenol (12.0 grams, 0.0881 moles) in chloroform (90 mls) was added to a suspension of lead tetraacetate (45 grams, 0.101 moles) in chloroform (70 mls). The temperature during addition was kept below 30.degree. C. The mixture was then stirred at room temperature for 2 hours. After the stirring was completed, the reaction mixture was then washed with water (3.times.200 mls) and the resulting organic layer was then filtered through Celatom FW-14 filter agent (61790-53-2) available from Aldrich Chemical Co., Inc. (Milwaukee, Wisc.). The filtered organic layer was dried with MgSO.sub.4 and evaporated to dryness. The oil thus obtained was recrystallized from petroleum ether (boiling range about 40.degree.-60.degree. C.) to give a light yellow solid (about 11 grams). The calculated yield was 64% based on the amount of phenol reactant.
The desired above-titled compound was confirmed by NMR, Infra-red and Elemental analysis.
EXAMPLE II
Preparation of Photoresist Formulation
Five grams of the sensitizer compound produced in Example I were mixed with a solution comprising 15.12 gms mixed 45% m- and 55% p-cresol-formaldehyde novolak resin (weight average M.W. of about 7000) and 51.84 gms of a solvent composed of 85% ethyl cellosolve acetate, 10% n-butyl acetate and 5% xylene and 18 mg of a non-ionic silicon-modified polymer anti-striation agent in a 8 oz. amber bottle. The bottle was then rolled for 12 hours at room temperature until all the solids were dissolved. The resulting resist solution was subsequently filtered through a 0.2 micron pore size filter using a Millipore microfiltration system (a 100 ml barrel and a 47 mm disk were used). The filtration was conducted in a nitrogen atmosphere under a gauge pressure of 10 pounds per square inch.
EXAMPLE III
Coating Of Photoresist Composition Onto Two Wafers
Approximately 3 ml of the filtered resist composition of Example II was spin-coated with a Model 5110-C single head spinner manufactured by Solitec, Inc. (Santa Clara, Calif.) onto two thermally grown silicon/silicon dioxide-coated wafer of four inches in diameter and having 5,400 angstroms of silicon oxide on their upper surface which was primed with 20% by volume hexamethyldisilazane (HMDS)/80% by volume xylene solution. The resist was applied to static wafers. Then, the wafers were each rotated to an initial spinning velocity of 500 revolutions per minute for 3 seconds, followed by acceleration at 2,000 revolutions per minute per second to a final spinning velocity of 4,800 revolutions per minute for 30 seconds. This spinning operation evenly spread the photoresist over the upper surface of the wafer to produce an even thin film. The coated wafers were each subsequently baked on a vacuum applied hot plate for 60 seconds. One was baked at 75.degree. C. and the other at 100.degree. C. The photoresist film thickness of each wafer was then measured to be approximately one micron with a Dektak IIa surface profilometer unit manufactured by Sloan Technology Corporation (Santa Barbara, Calif.).
EXAMPLE IV
Mid-UV Image-Wise Exposure of the 75.degree. C. Coated Wafer
The coated wafer baked at 75.degree. C. in Example III was image-wise exposed to mid-UV light wavelengths , between 260-320 nm using a Canon Model PLA-501F aligner (Lake Success, N.Y.) in the hard contact mode, equipped with a Xenon-Mercury UV lamp and CM290 cold mirror. The mid-UV light wavelengths were passed through a quartz Series I multidensity resolution target from Detric Optics, Inc. (Hudson, Mass.) for ten seconds to provide various exposure energies on the coated surface of the wafer. Eight-tenths of a micron feature were confirmed on the target using scanning electron microscopy. The intensity at the wafer plane was measured with a Mimir Instruments Inc. (Santa Clara, Calif.) Model 100 Powermeter equipped with a detector for measurement at 254 nm. This measured intensity was 2.0 milliwatts per square centimeter.
EXAMPLE V
Development of Exposed Resist Coated Wafer
The resist-coated wafer exposed according to Example IV was then held with Teflon tweezers and immersed in a 500 milliliter polypropylene container containing 33% by volume WAYCOAT Positive MIF Developer solution (Olin Hunt Specialty Products, Inc., West Paterson, N.J.) in water. This WAYCOAT developer is an aqueous solution of tetramethylammonium hydroxide. The wafer was allowed to remain immersed in the diluted developer solution while the container was gently moved using a circular motion to provide swirl agitation for 90 seconds. Upon removal, the wafer was rinsed in deionized water for one minute and dried in a stream of filtered nitrogen. Unexpectedly, the unexposed areas of the photoresist film were developed rather than the exposed areas which are normally removed with positive resist. Thus, this photoresist surprisingly produced a negative image instead of the expected positive image.
This exposed and developed wafer was examined to determine the photospeed of the photoresist film and small feature sizes.
Photospeed of the resist was determined by looking at each of the developed areas of the resist coating corresponding to different percent transmittance windows of the SERIES I target. Photospeed of this resist was calculated by multiplying the exposure energy at the wafer plane (2.0 milliwatts per square centimeter), the lowest percent transmittance window of the target at which the resist fully coated, and the full transmittance time (10 seconds) and then dividing by 100.
Examination of fine features was done using a Nikon optical microscope with one thousand times magnification.
The first panel to be fully coated was the 31.6% transmittance window corresponding to a photospeed of 6.3 millijoule per square centimeter at 254 nm. The optical microscope revealed eights-tenths micron lines.
This measured photospeed and fine feature size indicates this photoresist formulation which was baked at 75.degree. C. and imaged in the mid-UV range would provide excellent resolution and, thus, appears suitable for commercial applications where these baking temperatures and imaging conditions are employed.
EXAMPLE VI
Deep-UV Imaqe-Wise Exposure of 100.degree. C. Baked Coated Wafer
The second wafer baked at 100.degree. C. in Example III was image-wise exposed to deep-UV light wavelengths between 220-250 nm using a Canon Model PLA-501F aligner (Lake Success, N.Y.) in the hard contact mode equipped with an Xenon-Mercury UV lamp and CM250 cold mirror for a 30 second exposure time. The deep-UV wavelengths were passed through the quartz Series I multidensity resolution target described in Example IV. The intensity was measured to be 5.08 milliwatts per square centimeter with a Mimir Instruments, Inc. (Santa Clara, Calif.) Model 100 Powermeter equipped with a detector for measurement at 254 nm.
EXAMPLE VII
Development of Exposed Resist Coated Wafer
The resist coated wafer exposed according to Example VI was then held with Teflon tweezers and immersed in a 500 milliliter polypropylene container containing 33% by volume WAYCOAT Positive MIF Developer solution (Olin Hunt Specialty Products, Inc., West Paterson, N.J.) in water. This WAYCOAT solution is an aqueous solution of tetramethylammonium hydroxide. The wafer was allowed to remain immersed in the developer solution while the container was moved in a circular motion for 90 seconds. Then the wafer was rinsed in deionized water for one minute and dried in a stream of filtered nitrogen. Unexpectedly, the unexposed areas of the photoresist film were developed rather than the exposed areas which are normally removed with positive resist. Thus, this photoresist surprisingly produced a negative image instead of the expected positive image.
The developed and exposed wafer was examined to determine photospeed and small feature sizes as in Example V.
The first panel to be fully coated was the 8.7% transmittance window corresponding to a photospeed of 13.2 millijoule per square centimeter at 254 nm. The optical microscope revealed eights-tenths micron lines.
This measured photospeed and fine feature size indicates this photoresist formulation which was baked at 100.degree. C. and imaged in the deep-UV range would provide excellent resolution and, thus, appears suitable for commercial applications where these baking temperatures and imaging conditions are employed.
Claims
  • 1. A light-sensitive mixture useful as a negative-working photoresist composition comprising:
  • (a) at least one novolak resin; and
  • (b) at least one 6-acetoxy cyclohexadienone compound of the formula (I) below: ##STR3## wherein R.sub.1, R R.sub.3, R.sub.4 and R.sub.5 are individually selected from hydrogen and lower alkyl groups having from 1 to 4 carbon atoms with the proviso that at least three of the R.sub.1 to R.sub.5 groups are lower alkyl groups.
  • 2. The light-sensitive mixture of claim 1 wherein R.sub.1, R.sub.3 and R.sub.5 are lower alkyl groups and R.sub.2 and R.sub.4 are hydrogens.
  • 3. The light-sensitive mixture of claim 2 wherein R.sub.1, R.sub.3 and R.sub.5 are all methyl groups.
  • 4. The light-sensitive mixture of claim 1 wherein said novolak resin is selected from the group consisting of phenol-formaldehyde novolak resins and cresol-formaldehyde resins.
  • 5. The light-sensitive mixture of claim 1 wherein (a) is from about 70 to about 99 percent and (b) is from about 30 to about 1 percent of the non-volatile content of said mixture.
  • 6. The light-sensitive mixture of claim 1 further comprising one or more additives selected from the group consisting of solvents, actinic and contrast dyes, anti-striation agents, plasticizers and speed enhancers.
  • 7. A coated substrate comprising a substrate material coated with a film of a light-sensitive mixture comprising:
  • (a) at least one novolak resin; and
  • (b) at least one 6-acetoxy cyclohexadienone compound of the formula (I) below: ##STR4## wherein R.sub.1, R.sub.2, R.sub.3, R.sub.4 and R.sub.5 are individually selected from hydrogen and lower alkyl groups having from 1 to 4 carbon atoms with the proviso that at least three of the R.sub.1 to R.sub.5 groups are lower alkyl groups.
  • 8. The coated substrate of claim 7 wherein said substrate comprises one or more compounds selected from the group consisting of polyester, polyolefin, silicon, gallium arsenide, silicon/silicon dioxide, doped silicon dioxide, silicon nitride, aluminum/copper mixtures, tantalum, copper and polysilicon.
  • 9. The coated substrate of claim 7 wherein said substrate is a silicon wafer coated with silicon dioxide.
  • 10. The process of developing an image-wise exposed photoresist-coated substrate comprising:
  • (1) coating said substrate with a light-sensitive composition useful as a negative-working photoresist, said composition comprising:
  • (a) at least one novolak resin; and
  • (b) at least one 6-acetoxy cyclohexadienone compound of the formula (I) below: ##STR5## wherein R.sub.1, R.sub.2, R.sub.3, R.sub.4 and R.sub.5 are individually selected from hydrogen and lower alkyl groups having from 1 to 4 carbon atoms with the proviso that at least three of the R.sub.1 to R.sub.5 groups are lower alkyl groups;
  • (2) subjecting said coating on said substrate to an image-wise exposure of radiant light energy; and
  • (3) subjecting said image-wise exposed coated substrate to a developing solution wherein the unexposed areas of said light-exposed coating are dissolved and removed from the substrate, having a negative image-wise pattern in the coating.
  • 11. The process of claim 10 wherein said radiant light energy is ultraviolet light.
  • 12. The process of claim 10 wherein said developing solution is an aqueous solution of tetramethylammonium hydroxide.
US Referenced Citations (3)
Number Name Date Kind
3385700 Willems et al. May 1968
3385703 Poot May 1968
4496647 Kawabe et al. Jan 1985
Non-Patent Literature Citations (6)
Entry
Chemical Abstracts, vol. 67, 99505p.
Chemical Abstracts, vol. 64, 18782(h).
A. J. Waring et al., Stereoselective Photochemical Ring-opening of Cyclohexa-2,4-dienones, J. Chem. Soc., 1971, pp. 3274-3280.
G. Quinkert et al., "Thermally Reversible Photoisomerizations", Angew. Chem. International, vol. 11 (1972) No. 12, pp. 1072-1087.
G. Quinkert et al., "A Photochemical Entry to Macrocyclic Mono- and Dialctones", Angew. Chem. International, vol. 23 (1984), No. 6, pp. 440-442.
G. Quinkert et al., "Adducts of the Ketene (1E, 3Z)-1,2,3,4,5-Pentamethyl-6-oxo-1,3,5-hexatrienyl Acetate", Agnew. Chem. International, vol. 23 (1984), No. 6, pp. 442-444.